Nano tungsten oxide and preparation method thereof
By adding sodium tartrate and polyethylene glycol to the sodium tungstate solution and processing it in an acidic environment, the problem of uneven purity and particle size distribution of nano-tungsten oxide was solved, and nano-tungsten oxide with high purity and uniform particle size was prepared. , expanding its application scope.
Patent Information
- Application Number
- CN202410929674.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-08
AI Technical Summary
The traditional preparation method of nanometer tungsten oxide has problems such as low purity, uneven particle size distribution and unsatisfactory morphology, which limits its application in high-demand fields.
Add sodium tartrate and polyethylene glycol to sodium tungstate solution, slowly add acid dropwise to adjust the pH, filter the precipitate, transfer to dilute hydrochloric acid, stir, wash, dry, and roast to obtain high-purity nanotubular tungsten oxide.
The high purity (≥99.9wt%) and uniform particle size distribution (50nm~300nm) of nano-tungsten oxide are achieved, expanding its application potential in fields such as catalysis and energy storage.
Smart Images

Figure CN118745004A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tungsten oxides, and in particular relates to nano tungsten oxide and a preparation method thereof. Background Art
[0002] As an important functional material, nano-tungsten oxide has shown broad application prospects in energy storage, photocatalysis, gas sensing and other fields. Its unique physical and chemical properties, such as high melting point, high hardness, excellent wear resistance and conductivity, make it have important application value in many fields. However, the traditional preparation method of nano-tungsten oxide often has some problems, such as low purity and uneven particle size distribution, which limit its application in some high-demand fields.
[0003] At present, the preparation methods of nano tungsten oxide mainly include solid phase method and liquid phase method. The solid phase method is to prepare nano tungsten oxide by directly subjecting tungsten compounds to oxidation reaction at high temperature. This method is simple, but the reaction conditions and parameters are difficult to control, which can easily lead to uneven particle size distribution or unsatisfactory morphology of the obtained nano tungsten oxide particles. In addition, impurities may be introduced or amorphous structures may be produced during the preparation process, thus affecting the performance and application of nano tungsten oxide. Therefore, the solid phase method has certain limitations in the preparation of high-quality nano tungsten oxide.
[0004] The liquid phase method is to dissolve tungsten compounds in a solvent and then prepare nano tungsten oxide through chemical reactions or physical methods. Compared with the solid phase method, the liquid phase method has better controllability and can obtain more uniform particle size and morphology. However, the liquid phase method has challenges in equipment requirements, reaction conditions, and post-processing, all of which may affect the performance and application of nano tungsten oxide. Therefore, although the liquid phase method can prepare high-quality nano tungsten oxide, there are still some limitations in practical applications. Summary of the invention
[0005] The purpose of the present invention is to solve the above-mentioned shortcomings and provide a nano tungsten oxide and a preparation method thereof.
[0006] In the first aspect, a method for preparing nano tungsten oxide adopts the following technical solution:
[0007] A method for preparing nano tungsten oxide comprises the following steps:
[0008] Sodium tartrate and polyethylene glycol are added to the sodium tungstate solution, acid is slowly added dropwise to adjust the pH, and the precipitate is obtained by filtration;
[0009] The precipitate is transferred to dilute hydrochloric acid for stirring, washed with pure water, and then dried, roasted, and cooled to obtain the nano tungsten oxide.
[0010] Sodium tartrate acts as both a cosolvent and an auxiliary agent, selectively controlling the morphology of the tungsten oxide precursor to obtain nano-tubular tungsten oxide; polyethylene glycol acts as a porogen or emulsifier to fully improve the dispersibility of the system; in an acidic environment, a tungstic acid sol is obtained, and stirring in dilute acid can further improve the particle morphology; after calcination, nano-tubular tungsten oxide is obtained.
[0011] Furthermore, the concentration of sodium tungstate is 10 g / L to 40 g / L.
[0012] Furthermore, the concentration of sodium tartrate is 4 g / L to 8 g / L; the concentration of polyethylene glycol is 1 g / L to 3 g / L.
[0013] The concentration range of sodium tartrate and polyethylene glycol is crucial to controlling the reaction process and the performance of the final product. These additives, as cosolvents and emulsifiers, can affect the morphology and dispersibility of nano-tungsten oxide, thereby affecting its application performance.
[0014] Furthermore, nitric acid was slowly added dropwise to adjust the pH to 2.0-3.0, and stirring was continued for 1 h-3 h.
[0015] The step of slowly adding nitric acid to adjust the pH to 2.0-3.0 and continuing stirring for 1-3 hours helps to precisely control the reaction conditions, thereby optimizing the performance of the product. The control of pH value and stirring time can form uniform nano-tungsten oxide with desired properties.
[0016] Furthermore, the concentration of the dilute hydrochloric acid is 6 mol / L to 12 mol / L.
[0017] The concentration range of dilute hydrochloric acid has an important influence on the effect of the washing step. The appropriate concentration can ensure the effective removal of impurities without damaging the structure and performance of nano-tungsten oxide.
[0018] Further, the precipitate is transferred into dilute hydrochloric acid and stirred for 8 to 12 minutes.
[0019] Furthermore, the drying temperature is 80° C. to 150° C., and the drying time is 4 h to 8 h.
[0020] Furthermore, the calcination temperature is 300° C. to 500° C., and the calcination time is 2 h to 3 h.
[0021] In the second aspect, a nano tungsten oxide adopts the following technical solution:
[0022] A nano tungsten oxide is prepared by any of the above-mentioned methods for preparing the nano tungsten oxide.
[0023] Furthermore, the purity of the nano-tungsten oxide is ≥99.9wt%, the particle size is 50nm-300nm, and the bulk ratio is 1.4-1.6g / cm3 .
[0024] The high purity (≥99.9wt%), particle size range (50nm~300nm) and uniform particle size distribution of nano tungsten oxide provide a larger specific surface area and better catalytic performance, giving it a wider application potential in catalysis, energy storage and other fields.
[0025] Beneficial effects of the present invention:
[0026] The invention provides a method for preparing nano tungsten oxide. Sodium tartrate acts as both a cosolvent and an auxiliary agent to selectively control the morphology of a tungsten oxide precursor to obtain nano tubular tungsten oxide. Polyethylene glycol is used as a porogen or emulsifier to fully improve the dispersibility of the system. In an acidic environment, a tungstic acid sol is obtained, and stirring in dilute acid can further improve the particle morphology. After calcination, nano tubular tungsten oxide is obtained.
[0027] The invention provides a nano tungsten oxide with a purity of ≥99.9wt%, a uniform particle size distribution, and 50nm-300nm to provide a higher specific surface area for the tungsten oxide, excellent physical and chemical activity, and broadened the application field of the nano tungsten oxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a morphology photograph of the nano tungsten oxide provided in Example 2. DETAILED DESCRIPTION
[0029] The following is a further specific description of a nano tungsten oxide and a preparation method thereof described in the present invention in conjunction with an embodiment. For the sake of simplicity of description, this document cannot list all the alternative technical features and implementation schemes contained in the present invention. Therefore, those skilled in the art should know that any technical features and implementation schemes in this embodiment do not limit the scope of protection of the present invention, which includes any alternative technical features and implementation schemes adopted by all those skilled in the art without creative labor. Specifically, the implementation schemes obtained by replacing any technical feature in the present invention or combining any two or more technical features provided by the present invention should be within the scope of protection of the present invention.
[0030] If no specific techniques and conditions are specified in the examples, the procedures are carried out according to the techniques and conditions described in the literature in the art or according to the product instructions. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0031] Example
[0032] Example 1
[0033] Embodiment 1 provides a method for preparing nano tungsten oxide, comprising the following steps:
[0034] Add 4 g / L sodium tartrate and 1 g / L polyethylene glycol to a 10 g / L sodium tungstate solution, slowly add nitric acid to adjust the pH to 2.0, continue stirring for 1 hour, and filter to obtain the precipitate;
[0035] The precipitate was transferred to 6 mol / L dilute hydrochloric acid and stirred for 8 min, washed by centrifugation with pure water for 5 times, and then dried at 80° C. for 4 h, calcined at 300° C. for 3 h, and cooled to obtain nano tungsten oxide.
[0036] Example 2
[0037] Embodiment 2 provides a method for preparing nano tungsten oxide, comprising the following steps:
[0038] Add 6 g / L sodium tartrate and 2 g / L polyethylene glycol to 25 g / L sodium tungstate solution, slowly add nitric acid to adjust the pH to 2.5, continue stirring for 2 h, and filter to obtain the precipitate;
[0039] The precipitate was transferred to 9 mol / L dilute hydrochloric acid and stirred for 10 min, washed by centrifugation with pure water for 5 times, and then dried at 120° C. for 6 h, calcined at 400° C. for 2.5 h, and cooled to obtain nano tungsten oxide.
[0040] Example 2 provides a morphology photo of nano tungsten oxide. Figure 1 .
[0041] Example 3
[0042] Embodiment 3 provides a method for preparing nano tungsten oxide, comprising the following steps:
[0043] Add 8 g / L sodium tartrate and 3 g / L polyethylene glycol to 40 g / L sodium tungstate solution, slowly add nitric acid to adjust the pH to 3.0, continue stirring for 3 hours, and filter to obtain the precipitate;
[0044] The precipitate was transferred to 12 mol / L dilute hydrochloric acid and stirred for 12 min, washed by centrifugation with pure water for 5 times, and then dried at 150° C. for 4 h, calcined at 500° C. for 2 h, and cooled to obtain nano tungsten oxide.
[0045] Comparative Example
[0046] Comparative Example 1
[0047] Comparative Example 1 provides a method for preparing nano tungsten oxide, which is different from Example 2 in that sodium tartrate is replaced by polyethylene glycol in equal amounts, that is, sodium tartrate is not added, and the concentration of polyethylene glycol is 8 g / L.
[0048] Comparative Example 2
[0049] Comparative Example 2 provides a method for preparing nano tungsten oxide, which differs from Example 2 in that polyethylene glycol is replaced by sodium tartrate in equal amounts, that is, polyethylene glycol is not added, and the concentration of sodium tartrate is 8 g / L.
[0050] Comparative Example 3
[0051] Comparative Example 3 provides a method for preparing nano tungsten oxide, which differs from Example 2 in that sodium tartrate is not added.
[0052] Comparative Example 4 provides a method for preparing nano tungsten oxide, which differs from Example 2 in that nitric acid is added dropwise to adjust the pH to 3.5.
[0053] Comparative Example 5
[0054] Comparative Example 5 provides a method for preparing nano tungsten oxide, which is different from Example 2 in that the precipitate is not stirred in hydrochloric acid, as follows:
[0055] Add 6 g / L sodium tartrate and 2 g / L polyethylene glycol to 25 g / L sodium tungstate solution, slowly add nitric acid to adjust the pH to 2.5, continue stirring for 2 h, and filter to obtain the precipitate;
[0056] The precipitate was washed by centrifugation with pure water for 5 times, and then dried at 120° C. for 6 hours, calcined at 400° C. for 2.5 hours, and cooled to obtain nano tungsten oxide.
[0057] Comparative Example 6
[0058] Comparative Example 6 provides a method for preparing nano tungsten oxide, which differs from Example 2 in that the concentration of dilute hydrochloric acid is 5 mol / L.
[0059] Comparative Example 7
[0060] Comparative Example 7 provides a method for preparing nano tungsten oxide, which is different from Example 2 in that the concentration of dilute hydrochloric acid is 13 mol / L.
[0061] Comparative Example 8
[0062] Comparative Example 8 provides a method for preparing nano tungsten oxide, which is different from Example 2 in that the calcination temperature is 550°C.
[0063] Indicator testing
[0064] The particle size and bulk ratio data of the nano-tungsten oxide prepared by the nano-tungsten oxide preparation methods provided in Examples 1-3 and Comparative Examples 1-8 are shown in Table 1 below.
[0065] Table 1
[0066]
[0067] It can be seen from Table 1 that within the theoretical range, the particle size of tungsten oxide increases with the increase of reagent content. Tartaric acid affects the particle size, while polyethylene glycol does not affect the particle size. It mainly improves the morphology and particle dispersion. Too low hydrochloric acid concentration will increase the particle size of tungsten oxide. The pH value has the greatest influence on the particle size. Too high or too low pH value will lead to uneven particle size distribution and obvious thickening. As long as the time and temperature do not deviate too high, the roasting temperature has little effect on the particle size.
[0068] For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived from them are still within the scope of protection of the claims of the invention.
Claims
1. A method for preparing nano tungsten oxide, characterized in that: The following steps are involved: Sodium tartrate and polyethylene glycol are added to the sodium tungstate solution, acid is slowly added dropwise to adjust the pH, and the precipitate is obtained by filtration; The precipitate is transferred to dilute hydrochloric acid and stirred, and then washed with pure water. The precipitate is then dried, roasted, and cooled to obtain the nano tungsten oxide.
2. The method for preparing nano tungsten oxide according to claim 1, characterized in that: The concentration of sodium tungstate is 10g / L to 40g / L.
3. The method for preparing nano tungsten oxide according to claim 1, characterized in that: The concentration of sodium tartrate is 4 g / L to 8 g / L; the concentration of polyethylene glycol is 1 g / L to 3 g / L.
4. The method for preparing nano tungsten oxide according to claim 1, characterized in that: Slowly add nitric acid to adjust the pH to 2.0-3.0 and continue stirring for 1h-3h.
5. The method for preparing nano tungsten oxide according to claim 1, characterized in that: The concentration of dilute hydrochloric acid is 6 mol / L to 12 mol / L.
6. The method for preparing nano tungsten oxide according to claim 1, characterized in that: The precipitate is transferred into dilute hydrochloric acid and stirred for 8 to 12 minutes.
7. The method for preparing nano tungsten oxide according to claim 1, characterized in that: The drying temperature is 80℃~150℃, and the drying time is 4h~8h.
8. The method for preparing nano tungsten oxide according to claim 1, characterized in that: The calcination temperature is 300°C to 500°C, and the calcination time is 2h to 3h.
9. A nano tungsten oxide, characterized in that: The nano tungsten oxide is prepared by the preparation method of any one of claims 1 to 8.
10. A nano tungsten oxide according to claim 9, characterized in that: The purity of the nano tungsten oxide is ≥99.9wt%, the particle size is 50nm-300nm, and the bulk ratio is 1.4-1.6g / cm 3 .