A kind of water-based temporary protective ink capable of being washed and faded and preparation method thereof
By using a water-based temporary protection ink composed of acrylic acid and (meth)acrylate copolymer emulsion and hydrogenated rosin solution, safety hazards and environmental protection problems in the film removal process in the prior art are solved, and rapid and environmentally friendly water rinsing is achieved. Film and high temperature protection effect.
Patent Information
- Application Number
- CN202411230881.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-09-04
AI Technical Summary
The existing temporary protection inks have safety hazards and environmental protection problems during the film removal process, and the production efficiency is low, making it difficult to meet the needs of environmental protection and high temperature protection.
The aqueous temporary protective ink consisting of 75%~80% acrylic acid and (meth)acrylate copolymer emulsion and 20%~25% hydrogenated rosin solution are removed by non-ionic surfactants and peroxide initiators. The ionic water is copolymerized to form a protective film that is easy to elute the film.
It realizes rapid film removal in room temperature water, environmentally friendly and safe, and maintains the integrity of the film at high temperature of 200℃. It is suitable for glass high-temperature processing operation protection, and complete fall off under 50℃ warm water or ethanol.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials and relates to a water-based ink, in particular to a water-based temporary protective ink capable of being washed and faded and a preparation method thereof. Background Art
[0002] Products containing glass are everywhere in modern life, such as smartphones, tablets, car glass, etc., but glass is very susceptible to damage and contamination, which in turn affects the appearance and performance of the product. Covering the glass surface with a temporary protective film is an important means of protection, which can protect the glass from physical damage or other contamination during production, transportation or storage, but the traditional peelable protective glue / protective film needs to be manually peeled off, which is time-consuming and labor-intensive. Printing ink, as the current preferred way to protect glass, often has the disadvantage of difficult film cleaning. Although some products can be de-filmed with alkali solution or hot water (water with a temperature above 90°C) or other solvents, for example, patent CN201711128800.1 proposes a method for preparing alkali-degraded LED curing protective ink. The temporary protective ink in this patent can be de-inked with alkali solution, but the alkali solution is corrosive to glass and can easily cause the glass to become foggy. In addition, high-temperature water also has problems such as easy burns, and the safety factor is low. Patent CN202210050307.7 proposes a temporary protective ink for optical glass and its preparation method. The temporary protective ink in this patent can be de-inked with propylene glycol methyl ether acetate or alcohol, but a stripping solution is required during the film fading process, which increases costs. Patent CN201510500145.2 A water-washable touch screen temporary protective ink and its preparation method and application. The ink in this patent can protect the touch screen cover glass or ITO glass surface film from damage during the construction process at a high temperature of 200°C, and can be quickly washed off in 50°C water after the construction is completed. However, the ink film-forming time of this patent is relatively long, and the surface drying requires 30 to 60 minutes, and the production efficiency is low. In addition, with the increase in global environmental protection awareness, people have also put forward environmental protection requirements for this type of temporary protective ink. Therefore, it is urgent to develop a temporary protective ink that is easy to de-film and harmless to the environment. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a water-based temporary protective ink that can be washed and faded and a preparation method thereof.
[0004] To achieve the above object, the present invention provides a water-based temporary protective ink that can be washed and faded. The raw materials include 75% to 80% of acrylic acid and (meth) acrylate copolymer emulsion and 20% to 25% of hydrogenated rosin solution in mass percentage.
[0005] Furthermore, the acrylic acid and (meth)acrylate copolymer emulsion is obtained by copolymerizing acrylic acid, long-chain alkyl methacrylate and short-chain alkyl acrylate in deionized water with a peroxide initiator in the presence of a non-ionic surfactant.
[0006] Furthermore, the mass ratio of the acrylic acid, the nonionic surfactant, the initiator, the deionized water, the long-chain alkyl methacrylate and the short-chain alkyl acrylate is (20-40): (2.5-10): (0.25-0.75): 100: (2-10): (2-10).
[0007] Furthermore, the molecular formula of the long-chain alkyl methacrylate is CH2=C(CH3)COO(CH2)nCH3, wherein n=11~17.
[0008] Furthermore, the long-chain alkyl methacrylate is selected from one or more of dodecyl methacrylate, tetradecyl methacrylate, hexadecyl methacrylate or octadecyl methacrylate.
[0009] Furthermore, the molecular formula of the short-chain alkyl acrylate is CH2=CCOO(CH2)nCH3 or CH2=C(CH3)COO(CH2)nCH3, wherein n=1~3, specifically one or more of ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, preferably butyl acrylate.
[0010] Furthermore, the initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate, preferably potassium persulfate.
[0011] Furthermore, the nonionic surfactant is selected from alkylphenol polyoxyethylene ether OP-10 or polyoxyethylene sorbitan monooleate TWEEN 80; preferably alkylphenol polyoxyethylene ether OP-10.
[0012] Furthermore, the hydrogenated rosin solution is obtained by dissolving hydrogenated rosin in anhydrous ethanol.
[0013] Furthermore, the mass ratio of the hydrogenated rosin to anhydrous ethanol is (4-8):35.
[0014] The present invention also proposes a method for preparing the water-based temporary protective ink that can be washed and removed, comprising the following steps:
[0015] The acrylic acid and (meth)acrylate copolymer emulsion is added into the hydrogenated rosin solution, and the mixture is mixed and stirred to obtain the water-based temporary protective ink capable of being washed and faded.
[0016] Furthermore, the mixing and stirring is carried out at a temperature of 10-30° C., for a time of 1-3 hours, and at a stirring speed of 300-800 rpm.
[0017] Compared with the prior art, the present invention has the following advantages and technical effects:
[0018] 1. The water-based temporary protective ink prepared by the present invention mainly uses water and ethanol as solvents, has no other harmful volatiles, and is environmentally friendly and safe.
[0019] 2. The water-based temporary protective ink of the present invention has a fast film-forming speed on the glass surface, good film adhesion and high hardness. After the protective effect is completed, the film can be quickly and completely removed by rinsing with water at room temperature for 1 minute. The protective film falls off in pieces and is easy to collect and separate from the cleaning water. The post-processing process is more convenient and environmentally friendly.
[0020] 3. The protective film formed on the glass surface by the water-based temporary protective ink of the present invention will not crack or re-stick at a high temperature of 200°C, and can be used for protecting glass during high-temperature (below 200°C) processing operations. Moreover, after being subjected to a high temperature of 200°C, the protective film can be completely removed from the surface of the glass substrate by soaking in warm water at 50°C for 5 minutes or rinsing in anhydrous ethanol at room temperature for 1 to 2 minutes. DETAILED DESCRIPTION
[0021] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0022] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0023] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0024] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0025] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0026] The embodiment of the present invention provides a water-based temporary protective ink that can be washed and faded. The raw materials include 75% to 80% of acrylic acid and (meth) acrylate copolymer emulsion and 20% to 25% of hydrogenated rosin solution in terms of mass percentage.
[0027] In a preferred embodiment of the present invention, the acrylic acid and (meth)acrylate copolymer emulsion is obtained by copolymerizing acrylic acid, long-chain alkyl methacrylate and short-chain alkyl acrylate in deionized water with a peroxide initiator in the presence of a non-ionic surfactant.
[0028] In some embodiments of the present invention, the mass ratio of acrylic acid, nonionic surfactant, initiator, deionized water, long-chain alkyl methacrylate and short-chain alkyl acrylate is (20-40): (2.5-10): (0.25-0.75): 100: (2-10): (2-10).
[0029] In a more preferred embodiment of the present invention, the mass ratio of acrylic acid, nonionic surfactant, initiator, deionized water, long-chain alkyl methacrylate and short-chain alkyl acrylate is (20-25): (3.75-5): (0.4-0.6): 100: (3.75-4): (4.5-8).
[0030] In a preferred embodiment of the present invention, the molecular formula of the long-chain alkyl methacrylate is CH2=C(CH3)COO(CH2)nCH3, wherein n=11 to 17. More preferably, the long-chain alkyl methacrylate is selected from one or more of dodecyl methacrylate, tetradecyl methacrylate, hexadecyl methacrylate or octadecyl methacrylate, and most preferably is dodecyl methacrylate.
[0031] In a preferred embodiment of the present invention, the molecular formula of the short-chain alkyl acrylate is CH2=CCOO(CH2)nCH3 or CH2=C(CH3)COO(CH2)nCH3, wherein n=1 to 3. More preferably, the short-chain alkyl acrylate is one or more of ethyl acrylate, ethyl methacrylate, butyl acrylate, and butyl methacrylate, and most preferably butyl acrylate.
[0032] In a preferred embodiment of the present invention, the initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate, preferably potassium persulfate.
[0033] In a preferred embodiment of the present invention, the nonionic surfactant is selected from alkylphenol polyoxyethylene ether OP-10 or polyoxyethylene sorbitan monooleate TWEEN 80; preferably alkylphenol polyoxyethylene ether OP-10.
[0034] In a preferred embodiment of the present invention, the method for preparing the acrylic acid and (meth)acrylate copolymer emulsion comprises the following steps:
[0035] S1: Weigh the raw materials according to the above-mentioned dosage ratio, add the non-ionic surfactant into deionized water, stir magnetically for 0.5-2h at 10-30°C, then add the long-chain alkyl methacrylate and the short-chain alkyl acrylate, continue to stir magnetically for 2-4h at 10-30°C, then add acrylic acid, continue to stir magnetically for 0.5-2h until all dissolved, to obtain a mixed solution;
[0036] S2: Weigh 30wt% (mass percentage) of the mixed solution, add 30wt% (mass percentage) of the initiator, stir magnetically under nitrogen protection, and heat to 60°C, and continue magnetic stirring for 0.5-2h to obtain a prepolymer solution;
[0037] S3: Add the remaining 70wt% (mass percentage) of the mixed solution and the remaining 70wt% (mass percentage) of the initiator to the prepolymer solution, continue magnetic stirring at 60°C for 0.5-2h under nitrogen protection, and cool down to obtain an acrylic acid and (meth)acrylate copolymer emulsion.
[0038] In a preferred embodiment of the present invention, the hydrogenated rosin solution is obtained by dissolving hydrogenated rosin in anhydrous ethanol.
[0039] In a preferred embodiment of the present invention, the mass ratio of hydrogenated rosin to anhydrous ethanol is (4-8):35. More preferably, the mass ratio of hydrogenated rosin to anhydrous ethanol is (5-8):35.
[0040] The embodiment of the present invention also provides a method for preparing the water-based temporary protective ink that can be washed and removed, comprising the following steps:
[0041] The acrylic acid and (meth)acrylate copolymer emulsion is added into the hydrogenated rosin solution, and the mixture is mixed and stirred to obtain the water-based temporary protective ink capable of being washed and faded.
[0042] In a preferred embodiment of the present invention, the temperature of the mixing and stirring is 10-30°C, the time is 1-3 hours, and the stirring speed is 300-800 rpm. More preferably, the temperature of the mixing and stirring is 20-30°C, the time is 2 hours, and the stirring speed is 500-700 rpm.
[0043] The raw materials used in the embodiments of the present invention are all commercially available, specifically: acrylic acid, analytical grade, Zhiyuan Chemical Reagent Co., Ltd.; dodecyl methacrylate, analytical grade, Shanghai MacLean Biochemical Technology Co., Ltd.; butyl acrylate, analytical grade, Shandong Keyuan Biochemical Co., Ltd.; non-ionic surfactant OP-10, analytical grade, Shanghai Aladdin Biotechnology Co., Ltd.; potassium persulfate, analytical grade, Tianjin Damao Chemical Reagent Factory; hydrogenated rosin, West Asia Reagent; anhydrous ethanol, analytical grade, Zhiyuan Chemical Reagent Co., Ltd.
[0044] In the embodiments of the present invention, normal temperature refers to "25±3°C".
[0045] The technical solution of the present invention is further illustrated by the following embodiments.
[0046] Example 1
[0047] A method for preparing a water-based temporary protective ink that can be washed and removed by water comprises the following steps:
[0048] S1: Weigh 3.75g of surfactant OP-10 and add it to 100g of deionized water, stir it magnetically at 20°C for 1h, then add 4g of dodecyl methacrylate and 4.5g of butyl acrylate, continue to stir it magnetically at 20°C for 2h, then add 25g of acrylic acid, continue to stir it magnetically for 1h until it is completely dissolved, to obtain a mixed solution;
[0049] S2: Weigh 41g of the mixed solution (30wt% of the total mass of the mixed solution), add 0.15g of initiator potassium persulfate (30wt% of the total mass of the initiator), stir magnetically under nitrogen protection, heat to 60°C, and continue magnetic stirring for 0.5h to obtain a prepolymer solution;
[0050] S3: adding the remaining mixed solution (70 wt% of the total mass of the mixed solution) and 0.35 g of initiator potassium persulfate (70 wt% of the total mass of the initiator added) to the prepolymer solution, stirring the mixture under nitrogen protection at 60° C. for 1.5 h, and cooling the mixture to obtain an acrylic acid and (meth)acrylate copolymer emulsion;
[0051] S4: Weigh 5 g of hydrogenated rosin into a glass beaker, add 35 g of anhydrous ethanol, seal the beaker and stir magnetically at 20°C until the hydrogenated rosin is completely dissolved to obtain a light yellow transparent hydrogenated rosin solution;
[0052] S5: Add hydrogenated rosin solution to the acrylic acid and (meth) acrylate copolymer emulsion, stir magnetically for 2 hours at 20°C until the mixture is evenly mixed, and finally obtain a water-based temporary protective ink with a solid content of about 30%.
[0053] The speed of magnetic stirring during the preparation process was 500 rpm.
[0054] Deionized water and anhydrous ethanol are solvents in the water-based temporary protective ink, and the copolymer of acrylic acid and (meth) acrylate and hydrogenated rosin are solutes. The specific test method for the solid content of the protective ink is as follows (the same below): First, dry the clean weighing bottle in an electric constant temperature blast drying oven at 100°C, wait for it to be completely dry and then put it in a dryer, wait for the weighing bottle to cool down at room temperature, accurately weigh its mass, and record it as W0. Then take 2g of water-based temporary protective ink and add it to the weighing bottle, so that it is evenly distributed on the bottom of the bottle, and accurately weigh the total mass of the protective ink and the weighing bottle, and record it as W1. Finally, put the weighing bottle containing the protective ink into an oven at 100°C, take it out after drying for 1 hour, put it in the dryer to room temperature and measure the weight again, then put the weighing bottle containing the protective ink back into the oven to continue drying, repeat the above operation until the difference between two consecutive weighings is less than 0.01g, and record the mass of the weighing bottle at this time as W2. The solid content calculation of the protective ink is as follows:
[0055]
[0056] Wherein: X is the solid content of the protective ink (%), W0 is the mass of the weighing bottle / g, W1 is the total mass of the weighing bottle and the protective ink / g, and W2 is the total mass of the weighing bottle and the protective ink after the solvent is completely removed / g.
[0057] According to GB / T2794, the viscosity of the water-based temporary protective ink prepared in Example 1 was tested using a BGD152 / 2S smart touch viscometer at a test temperature of 25° C. A suitable rotor model was selected and a suitable speed was set as required so that the pointer was between 20% and 80% of the dial. The test results showed that the viscosity of the water-based temporary protective ink prepared in Example 1 was 3000 mPa×s.
[0058] The water-based temporary protective ink prepared in Example 1 was applied to the surface of the glass sheet, and the coating thickness was about 30 μm. The film was cured at 100°C for 15 minutes. The film was colorless, transparent and crack-free. The film hardness was H according to GB / T6739, and the film adhesion was grade 2 according to GB / T9286. The protective film was washed with 25°C water (the angle between the water flow and the edge of the glass plate protective film was 45°) for 1 minute, and it could be removed in one piece. After the film was removed, the glass did not fog. In addition, the protective film was heated at 200°C for 30 minutes without cracking or re-adhesion. The film hardness was 2H according to GB / T6739, and the film adhesion was grade 1 according to GB / T9286. It can be used for high-temperature (below 200°C) glass processing protection, and the protective film can be removed from the glass surface in one piece after being soaked in 50°C warm water for 5 minutes after being exposed to a high temperature of 200°C.
[0059] Example 2
[0060] A method for preparing a water-based temporary protective ink that can be washed and removed by water comprises the following steps:
[0061] S1: Weigh 3.75g of surfactant OP-10 and add it to 100g of deionized water, stir it magnetically at 30°C for 0.5h, then add 4g of dodecyl methacrylate and 6.5g of butyl acrylate, continue to stir it magnetically at 30°C for 3h, then add 25g of acrylic acid, continue to stir it magnetically for 1h until it is completely dissolved, to obtain a mixed solution;
[0062] S2: Weigh 42g of the mixed solution (30wt% of the total mass of the mixed solution), add 0.18g of initiator potassium persulfate (30wt% of the total mass of the initiator), stir magnetically under nitrogen protection, heat to 60°C, and continue magnetic stirring for 0.5h to obtain a prepolymer solution;
[0063] S3: adding the remaining mixed solution (70 wt% of the total mass of the mixed solution) and 0.42 g of initiator potassium persulfate (70 wt% of the total mass of the initiator added) to the prepolymer solution B, stirring the mixture under nitrogen protection at 60° C. for 1 h, and cooling the mixture to obtain an acrylic acid and (meth)acrylate copolymer emulsion;
[0064] S4: Weigh 5 g of hydrogenated rosin into a glass beaker, add 35 g of anhydrous ethanol, seal the beaker and stir magnetically at 30°C until the hydrogenated rosin is completely dissolved to obtain a light yellow transparent hydrogenated rosin solution;
[0065] S5: Add hydrogenated rosin solution to the acrylic acid and (meth) acrylate copolymer emulsion, stir magnetically for 2 hours at 30°C until the mixture is uniformly mixed, and finally obtain a water-based temporary protective ink with a solid content of 30%.
[0066] The speed of magnetic stirring during the preparation process was 600 rpm.
[0067] According to GB / T2794, the viscosity of the water-based temporary protective ink prepared in Example 2 was tested using a BGD152 / 2S intelligent touch viscometer at a test temperature of 25° C. A suitable rotor model was selected and a suitable speed was set as required so that the pointer was between 20% and 80% of the dial. The test results showed that the viscosity of the water-based temporary protective ink prepared in Example 2 was 10000 mPa×s.
[0068] The water-based temporary protective ink prepared in Example 2 was applied to the surface of the glass sheet, and the coating thickness was about 30 μm. It was cured by baking at 100°C for 15 minutes. The appearance of the adhesive film was colorless, transparent and crack-free. The hardness of the film tested according to GB / T6739 was HB, and the adhesion of the film tested according to GB / T9286 was level 2. The protective film was rinsed with 25°C water (the angle between the water flow and the edge of the glass plate protective film was 45°) for 1 minute, and it could be removed in one piece. After the film was removed, the glass did not fog. In addition, the glass protective film was heated at 200°C for 30 minutes without cracking or re-adhesion. The hardness of the film tested according to GB / T6739 was H, and the adhesion of the film tested according to GB / T9286 was level 1. It can be used for high-temperature (below 200°C) processing protection of glass, and the protective film can be removed from the glass surface in one piece after being rinsed with anhydrous ethanol at room temperature for 1 to 2 minutes after being subjected to a high temperature of 200°C.
[0069] Example 3
[0070] A method for preparing a water-based temporary protective ink that can be washed and removed by water comprises the following steps:
[0071] S1: Weigh 5 g of surfactant OP-10 and add it to 100 g of deionized water, stir it magnetically at 25°C for 1 h, then add 3.75 g of dodecyl methacrylate and 8 g of butyl acrylate, continue to stir it magnetically at 25°C for 3.5 h, then add 25 g of acrylic acid, continue to stir it magnetically for 1 h until it is completely dissolved, to obtain a mixed solution;
[0072] S2: Weigh 42g of the mixed solution (30wt% of the total mass of the mixed solution), add 0.15g of initiator potassium persulfate (30wt% of the total mass of the initiator), stir magnetically under nitrogen protection, heat to 60°C, and continue magnetic stirring for 0.5h to obtain a prepolymer solution;
[0073] S3: adding the remaining mixed solution (70 wt% of the total mass of the mixed solution) and 0.35 g of initiator potassium persulfate (70 wt% of the total mass of the initiator added) to the prepolymer solution B, stirring the mixture under nitrogen protection at 60° C. for 1 h, and cooling the mixture to obtain an acrylic acid and (meth)acrylate copolymer emulsion;
[0074] S4: Weigh 6 g of hydrogenated rosin into a glass beaker, add 35 g of anhydrous ethanol, seal the beaker, and stir magnetically at 25°C until the hydrogenated rosin is completely dissolved to obtain a light yellow transparent hydrogenated rosin solution;
[0075] S5: Add hydrogenated rosin solution to the acrylic acid and (meth) acrylate copolymer emulsion, stir magnetically for 2 hours at 25°C until the mixture is uniformly mixed, and finally obtain a water-based temporary protective ink with a solid content of 30%.
[0076] The speed of magnetic stirring during the preparation process was 700 rpm.
[0077] According to GB / T2794, the viscosity of the water-based temporary protective ink prepared in Example 3 was tested using a BGD152 / 2S intelligent touch viscometer at a test temperature of 25° C. A suitable rotor model was selected and a suitable speed was set as required so that the pointer was between 20% and 80% of the dial. The test results showed that the viscosity of the water-based temporary protective ink prepared in Example 3 was 13000 mPa×s.
[0078] The water-based temporary protective ink prepared in Example 3 was applied to the surface of the glass sheet, and the coating thickness was about 30 μm. It was cured by baking at 100°C for 15 minutes. The appearance of the adhesive film was colorless, transparent and crack-free. The hardness of the film tested according to GB / T6739 was HB, and the adhesion of the film tested according to GB / T9286 was level 2. The protective film was rinsed with 25°C water (the angle between the water flow and the edge of the glass plate protective film was 45°) for 1 minute, and it could be removed in one piece. After the film was removed, the glass did not fog. In addition, the protective film was heated at 200°C for 30 minutes without cracking or re-adhesion. The hardness of the film tested according to GB / T6739 was H, and the adhesion of the film tested according to GB / T9286 was level 1, which can be used for high-temperature (below 200°C) glass processing protection, and the protective film can be removed from the glass surface in one piece after being soaked in 50°C warm water for 5 minutes after being exposed to a high temperature of 200°C.
[0079] Example 4
[0080] A method for preparing a water-based temporary protective ink that can be washed and removed by water comprises the following steps:
[0081] S1: Weigh 3.75 g of surfactant OP-10 and add it to 100 g of deionized water, stir it magnetically at 25°C for 1 h, then add 3.75 g of dodecyl methacrylate and 6 g of butyl acrylate, continue to stir it magnetically at 25°C for 4 h, then add 20 g of acrylic acid, continue to stir it magnetically for 0.5 h until it is completely dissolved, to obtain a mixed solution;
[0082] S2: Weigh 40g of the mixed solution (30wt% of the total mass of the mixed solution), add 0.12g of initiator potassium persulfate (30wt% of the total mass of the initiator), stir magnetically under nitrogen protection, heat to 60°C, and continue magnetic stirring for 0.5h to obtain a prepolymer solution;
[0083] S3: adding the remaining mixed solution (70 wt% of the total mass of the mixed solution) and 0.28 g of initiator potassium persulfate (70 wt% of the total mass of the initiator added) to the prepolymer solution, stirring the mixture under nitrogen protection at 60° C. for 2 h, and cooling the mixture to obtain an acrylic acid and (meth)acrylate copolymer emulsion;
[0084] S4: Weigh 8 g of hydrogenated rosin into a glass beaker, add 35 g of anhydrous ethanol, seal the beaker, and stir magnetically at 25°C until the hydrogenated rosin is completely dissolved to obtain a light yellow transparent hydrogenated rosin solution;
[0085] S5: Add hydrogenated rosin solution to the acrylic acid and (meth) acrylate copolymer emulsion, stir magnetically for 2 hours at 25°C until the mixture is uniformly mixed, and finally obtain a water-based temporary protective ink with a solid content of 30%.
[0086] The speed of magnetic stirring during the preparation process was 600 rpm.
[0087] According to GB / T2794, the viscosity of the water-based temporary protective ink prepared in Example 4 was tested using a BGD152 / 2S intelligent touch viscometer at a test temperature of 25° C. A suitable rotor model was selected and a suitable speed was set as required so that the pointer was between 20% and 80% of the dial. The test results showed that the viscosity of the water-based temporary protective ink prepared in Example 4 was 4000 mPa×s.
[0088] The water-based temporary protective ink prepared in Example 4 was applied to the surface of the glass sheet, and the coating thickness was about 30 μm. It was cured by baking at 100°C for 15 minutes. The appearance of the adhesive film was colorless, transparent and crack-free. The hardness of the film tested according to GB / T6739 was HB, and the adhesion of the film tested according to GB / T9286 was level 2. The protective film was rinsed with 25°C water (the angle between the water flow and the edge of the glass plate protective film was 45°) for 1 minute, and it could be removed in one piece. After the film was removed, the glass did not fog. In addition, the protective film was heated at 200°C for 30 minutes without cracking or re-adhesion. The hardness of the film tested according to GB / T6739 was H, and the adhesion of the film tested according to GB / T9286 was level 1. It can be used for high-temperature (below 200°C) processing protection of glass, and the protective film can be removed from the glass surface in one piece after being rinsed with anhydrous ethanol at room temperature for 1 to 2 minutes after being subjected to a high temperature of 200°C.
[0089] Comparative Example 1
[0090] The same as Example 1, except that in step S5, the mass percentage of the acrylic acid and (meth)acrylate copolymer emulsion is 70%, and the mass percentage of the hydrogenated rosin solution is 30%.
[0091] The temporary protective ink prepared in this comparative example is applied to the surface of the glass sheet, and the coating thickness is about 30μm. It is cured by baking at 100℃ for 15min. The appearance of the film is light yellow, translucent and crack-free. The hardness of the film is H according to GB / T6739, and the adhesion of the film is level 2 according to GB / T9286. The protective film is rinsed with 25℃ water (the angle between the water flow and the edge of the glass plate protective film is 45°) for 1 minute, and the film cannot be peeled off. After continuous rinsing for 30 minutes, the film still cannot be completely peeled off. The protective film is heated at 200℃ for 30min without cracking and re-adhesion. The hardness of the film is H according to GB / T6739, and the adhesion of the film is level 1 according to GB / T9286. It can be used for high-temperature (below 200℃) glass processing protection, but the protective film cannot be peeled off from the glass surface after being soaked in 50℃ warm water for 30min after being exposed to 200℃.
[0092] Comparative Example 2
[0093] The same as Example 1, except that in step S5, the mass percentage of the acrylic acid and (meth)acrylate copolymer emulsion is 95%, and the mass percentage of the hydrogenated rosin solution is 5%.
[0094] The temporary protective ink prepared in this comparative example was applied to the surface of the glass sheet, and the coating thickness was about 30μm. It was cured by baking at 100℃ for 15min. The appearance of the film was colorless, transparent and without cracks, but the hardness and adhesion of the film decreased. According to the provisions of GB / T6739, the hardness of the film was tested to be 2B, and according to the method of GB / T9286, the adhesion of the film was tested to be level 3, and the protective ability of the glass was poor. The protective film was rinsed with 25℃ water (the angle between the water flow and the edge of the glass plate protective film was 45°) for 1 minute, and the film swelled and ruptured locally, and could not be completely peeled off. There was residual glue on the surface of the glass after rinsing. In addition, the protective film will become soft and sticky when heated at 160~200℃ for 30min, and cannot withstand the high temperature (below 200℃) processing and protection of glass.
[0095] Comparative Example 3
[0096] A method for preparing a temporary protective ink (without adding hydrogenated rosin solution) comprises the following steps:
[0097] S1: Weigh 3.75g of surfactant OP-10 and add it to 100g of deionized water, stir it magnetically at 20°C for 1h, then add 4g of dodecyl methacrylate and 4.5g of butyl acrylate, continue to stir it magnetically at 20°C for 2h, then add 25g of acrylic acid, continue to stir it magnetically for 1h until it is completely dissolved, to obtain a mixed solution;
[0098] S2: Weigh 41g of the mixed solution (30wt% of the total mass of the mixed solution), add 0.15g of initiator potassium persulfate (30wt% of the total mass of the initiator), stir magnetically under nitrogen protection, heat to 60°C, and continue magnetic stirring for 0.5h to obtain a prepolymer solution;
[0099] S3: Add the remaining mixed solution (70wt% of the total mass of the mixed solution) and 0.35g of initiator potassium persulfate (70wt% of the total mass of the initiator added) into the prepolymer solution, continue magnetic stirring at 60°C for 1.5h under nitrogen protection, cool down, and obtain an acrylic acid and (meth) acrylate copolymer emulsion, which is a temporary protective ink.
[0100] The speed of magnetic stirring during the preparation process was 500 rpm.
[0101] The temporary protective ink prepared in this comparative example was applied to the surface of the glass sheet, and the coating thickness was about 30μm. It was cured by baking at 100℃ for 15min. The appearance of the film was colorless, transparent and without cracks, but the hardness and adhesion of the film decreased. According to the provisions of GB / T6739, the hardness of the film was 3B, and according to the method of GB / T9286, the adhesion of the film was 3, and the protective ability of the glass was poor. The protective film was rinsed with 25℃ water (the angle between the water flow and the edge of the glass plate protective film was 45°) for 1 minute. The film absorbed water and swelled, becoming soft and sticky, and could not be completely peeled off. There was residual glue on the surface of the glass after rinsing. In addition, the protective film will become soft and sticky when heated at 160~200℃ for 30min, and cannot withstand the high temperature (below 200℃) processing and protection of glass.
[0102] Comparative Example 4
[0103] The same as Example 1, except that the surfactant OP-10 in Example 1 is replaced by the cationic surfactant cetyltrimethylammonium bromide (CTAB). The specific preparation method is as follows:
[0104] S1: 3.75 g of surfactant CTAB was weighed and added to 100 g of deionized water, and magnetically stirred at 20°C for 1 h. Then, 4 g of dodecyl methacrylate and 4.5 g of butyl acrylate were added, and magnetic stirring was continued at 20°C for 2 h. Then, 25 g of acrylic acid was added, and magnetic stirring was continued for 1 h until all the water was dissolved to obtain a mixed solution.
[0105] S2: Weigh 41g of the mixed solution (30wt% of the total mass of the mixed solution), add 0.15g of initiator potassium persulfate (30wt% of the total mass of the initiator), stir magnetically under nitrogen protection, heat to 60°C, and continue magnetic stirring for 0.5h to obtain a prepolymer solution;
[0106] S3: adding the remaining mixed solution (70 wt% of the total mass of the mixed solution) and 0.35 g of initiator potassium persulfate (70 wt% of the total mass of the initiator added) to the prepolymer solution, stirring the mixture under nitrogen protection at 60° C. for 1.5 h, and cooling the mixture to obtain an acrylic acid and (meth)acrylate copolymer emulsion;
[0107] S4: Weigh 5 g of hydrogenated rosin into a glass beaker, add 35 g of anhydrous ethanol, seal the beaker and stir magnetically at 20°C until the hydrogenated rosin is completely dissolved to obtain a light yellow transparent hydrogenated rosin solution;
[0108] S5: Add hydrogenated rosin solution to the acrylic acid and (meth) acrylate copolymer emulsion, stir magnetically for 2 hours at 20°C until the mixture is uniformly mixed, and finally obtain a water-based temporary protective ink with a solid content of 30%.
[0109] The speed of magnetic stirring during the preparation process was 500 rpm.
[0110] The temporary protective ink prepared in this comparative example was applied to the surface of the glass sheet, and the coating thickness was about 30 μm. It was cured by baking at 100°C for 15 minutes. The film was colorless, transparent and crack-free. The film hardness was H according to GB / T6739, and the film adhesion was level 2 according to GB / T9286. However, the protective film was continuously washed with 25°C water (the angle between the water flow and the edge of the glass plate protective film was 45°) for 2 hours, and the film did not peel off at all.
[0111] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A water-based temporary protective ink that can be washed and faded, characterized in that: In terms of mass percentage, the raw materials include 75% to 80% of acrylic acid and (meth) acrylate copolymer emulsion and 20% to 25% of hydrogenated rosin solution; The acrylic acid and (meth) acrylic acid ester copolymer emulsion is obtained by copolymerizing acrylic acid, long-chain alkyl methacrylate and short-chain alkyl acrylate in deionized water with a peroxide initiator in the presence of a non-ionic surfactant.
2. The water-based temporary protective ink capable of being washed and removed by water according to claim 1, characterized in that: The mass ratio of the acrylic acid, the nonionic surfactant, the initiator, the deionized water, the long-chain alkyl methacrylate and the short-chain alkyl acrylate is (20-40): (2.5-10): (0.25-0.75): 100: (2-10): (2-10).
3. The water-based temporary protective ink capable of being washed and removed by water according to claim 1, characterized in that: The molecular formula of the long-chain alkyl methacrylate is CH2=C(CH3)COO(CH2)nCH3, wherein n=11-17.
4. The water-based temporary protective ink capable of being washed and removed by water according to claim 1, characterized in that: The molecular formula of the short-chain alkyl acrylate is CH2=CCOO(CH2)nCH3 or CH2=C(CH3)COO(CH2)nCH3, wherein n=1-3.
5. The water-based temporary protective ink capable of being washed and removed by water according to claim 1, characterized in that: The initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate.
6. The water-based temporary protective ink capable of being washed and removed by water according to claim 1, characterized in that: The hydrogenated rosin solution is obtained by dissolving hydrogenated rosin in anhydrous ethanol.
7. The water-based temporary protective ink capable of being washed and removed according to claim 6, characterized in that: The mass ratio of the hydrogenated rosin to anhydrous ethanol is (4-8):
35.
8. A method for preparing the water-based temporary protective ink capable of being washed and removed by water according to any one of claims 1 to 7, characterized in that: The following steps are involved: The acrylic acid and (meth)acrylate copolymer emulsion is added into the hydrogenated rosin solution, and the mixture is mixed and stirred to obtain the water-based temporary protective ink capable of being washed and faded.
9. The method for preparing the water-based temporary protective ink capable of being washed and removed by water according to claim 8, characterized in that: The mixing and stirring is performed at a temperature of 10-30° C., a time of 1-3 hours, and a stirring speed of 300-800 rpm.