High-strength hydrogen storage container steel plate with excellent high heat input resistance and manufacturing method of high-strength hydrogen storage container steel plate
Through composition design and quenching and tempering heat treatment, a hydrogen storage container steel plate with excellent high-energy welding performance and low-temperature impact toughness is prepared, which solves the problems of insufficient welding performance and low-temperature toughness of steel plates under high pressure in the existing technology, and achieves high Manufactured from steel plates with high strength and toughness.
Patent Information
- Application Number
- CN202410861849.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing container steel plates for hydrogen storage cannot meet the requirements of large linear energy welding under high pressure, and their low-temperature impact toughness and welding heat-affected zone performance are insufficient, making it difficult to meet the needs of widely used hydrogen energy storage.
Through composition design and two-stage controlled rolling process, combined with quenching and tempering heat treatment, the chemical composition prepared is C: 0.08%-0.10%, Si: 0.20%-0.35%, Mn: 1.60%-1.80%, Cr: 0.40%- 0.50%, Mo:0.05%-0.15%, Ni:0.20%-0.40%, V: 0.20%-0.40%, Nb: 0.02%-0.03%, Ti: 0.02%-0.04%, Al: 0.003%-0.005%, Ca: 0.003%-0.005% steel plate, using large linear energy 100-150kJ/ cm welding to ensure the mechanical properties and low-temperature impact toughness of the welding heat-affected zone.
The yield strength, tensile strength and elongation of the steel plate are significantly improved at high and low temperatures. The performance of the welding heat-affected zone is excellent, meeting the manufacturing and application requirements of pressure vessels, and the hydrogen-induced cracking resistance is significantly improved.
Smart Images

Figure BDA0004919314870000091 
Figure BDA0004919314870000092 
Figure BDA0004919314870000093
Abstract
Description
Technical Field
[0001] The present invention relates to the field of preparation of hydrogen storage container steel plates, and in particular to a quenched and tempered high-strength hydrogen storage container steel plate with excellent resistance to large linear energy and a manufacturing method thereof, which is particularly suitable for gas hydrogen storage tanks. Background Art
[0002] In recent years, with the increase in global energy demand, the demand for renewable energy has continued to increase. In order to build a cleaner, low-carbon, safe and efficient energy system, limit fossil energy and implement renewable energy substitution, hydrogen energy has become an important energy carrier for the effective recycling of renewable energy and is widely used in urban transportation, industrial production and urban construction. Therefore, the research and development of steel plates for gas hydrogen storage under different high pressures is extremely important and has become the primary task of hydrogen energy storage.
[0003] Energy input is a very important process parameter in welding construction. It refers to the energy input from the welding power source to the weld per unit length, also known as heat input, and is generally expressed in kilojoules / cm (kJ / cm). Conventional welding heat input is below 50kJ / cm, and generally above 50kJ / cm is called high energy input welding. Increasing the energy input can improve welding efficiency and shorten the engineering manufacturing cycle. Therefore, in the welding method of medium and thick steel plates, high energy input welding is often used. The high energy input welding method can be formed in one pass, and the production efficiency is increased several times, which significantly reduces the production cost. However, high energy input welding will have an adverse effect on the toughness of the heat affected zone (HAZ) of traditional low alloy steel. The heat affected zone (HAZ) of the weld is continuously affected by the high temperature deposited metal in the weld, and is in a high temperature state for a long time, and the cooling rate is slow, resulting in severe coarsening of the original austenite grains, which ultimately reduces the low temperature impact toughness of the steel plate and even produces welding cracks.
[0004] CN117070855A "Corrosion-resistant ultra-large line energy welding steel plate and its production method", its chemical composition is: Ce: 0.05-0.5%, Sn: 0.05-0.5%, Cu: 0.1-0.5%, Si: 0.1-0.4%, C: ≤0.12%, Mn: ≤2.0%, and other elements. The Ce and Sn content in its designed composition is relatively high, which is prone to segregation and generates large-sized inclusions, and the steel plate is prone to cracks during welding; CN116574981A "A high-quality low-temperature storage In "Steel Plate for Oil Tanks and Its Production Method", the chemical composition is designed as follows: C: 0.05-0.07%, Si: 0.10-0.30%, Mn: 1.45-1.55%, Cr: 0.20-0.25%, V: 0.035-0.040%, Ni: 0.15-0.20%, Ti: 0.025-0.030%, and the balance is Fe and other elements. Through controlled rolling and controlled cooling process + tempering heat treatment, the low-temperature impact toughness of the steel plate is only guaranteed to be -20°C. Its applicable environment is limited and it is difficult to overcome the use environment.
[0005] Steel plates for containers are mainly quenched and tempered steel plates. By improving the manufacturing method and adjusting the content of alloy elements in the steel grade, the hydrogen resistance and the ability to resist high-wire energy welding can be improved. It is urgent to develop quenched and tempered high-strength hydrogen storage container steel plates with excellent resistance to high-wire energy and their manufacturing methods. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention aims to provide a high-strength steel plate for hydrogen storage containers with excellent resistance to large line energy and a manufacturing method thereof. The present invention adopts a composition design combined with a two-stage controlled rolling production process, as well as a quenching and tempering heat treatment, so that the mechanical properties of the steel plate obtained and the mechanical properties of the simulated post-weld heat treatment meet the following requirements: yield strength R eL ≥600MPa, tensile strength R m :720~850MPa, elongation A≥21%, -50℃ low temperature impact toughness KV2≥100J, -50℃ low temperature tensile yield strength R eL ≥620MPa, tensile strength R m :735~880MPa, elongation ≥21%; use high wire energy 100~150kJ / cm to weld steel plates, the yield strength of the welding heat affected zone (HAZ) R eL ≥650MPa, tensile strength R m : 780~900MPa, elongation ≥19%, -50℃ HAZ zone impact toughness KV2 ≥80J. (36-60)mm thickness steel plate has excellent strength and low temperature impact toughness, and has uniform and fine structure, which can meet the manufacturing and application requirements of steel plates for pressure vessels.
[0007] The object of the invention is achieved in this way:
[0008] A quenched and tempered container steel plate with excellent resistance to large line energy. The chemical composition of the steel used is as follows, calculated by mass percentage: C: 0.08%-0.10%, Si: 0.20%-0.35%, Mn: 1.60%-1.80%, P: ≤0.015%, S: ≤0.005%, Cr: 0.40%-0.50%, Mo: 0.05%-0.15%, Ni: 0.20%-0.40%, V: 0.20%-0.40%, Nb: 0.02%-0.03%, Ti: 0.02%-0.04%, Al: 0.003%-0.005%, Ca: 0.003%-0.005%, and the balance is Fe and unavoidable impurities.
[0009] Furthermore, the component V / C≥2.5.
[0010] Furthermore, the steel plate yield strength R eL ≥600MPa, tensile strength R m : 720~850MPa, elongation ≥21%, -50℃ impact toughness KV2 ≥100J, -50℃ low temperature tensile yield strength R eL ≥620MPa, tensile strength R m :735~880MPa, elongation ≥21%; use high wire energy 100~150kJ / cm to weld steel plates, the yield strength of the welding heat affected zone (HAZ) R eL ≥650MPa, tensile strength R m : 780~900MPa, elongation ≥19%, -50℃ welding heat affected zone (HAZ) impact toughness KV2≥80J.
[0011] Furthermore, the steel plate microstructure is bainite tempered structure + acicular ferrite, the bainite tempered structure accounts for 85-95% of the volume, the acicular ferrite accounts for 5-15% of the volume, the grain size is 8-10, the average size of the composite inclusions is 1-3μm, and the steel plate thickness is 36-60mm.
[0012] The reasons for the composition design of the present invention are as follows:
[0013] C: 0.08%~0.10%
[0014] Cr, Mo and Ti are the main elements of the present invention, and the effects of the above chemical elements are analyzed as follows:
[0015] C forms various carbides with alloy elements in steel to strengthen it. It is an element that directly improves the strength of steel plates. Too high C content will lead to poor toughness, plasticity and welding performance of steel. In order to ensure that the steel plate has good low-temperature impact toughness, strength and welding performance matching during use, the increase of C content will easily lead to the increase of bainite and cementite, affecting toughness. Therefore, in order to ensure that the carbon equivalent is low enough and meet the excellent conditions of welding performance, the C content is limited to 0.08% to 0.10%.
[0016] Si: 0.20%~0.35%
[0017] Si is an element that increases carbon activity in steel. In the high silicon concentration area, it can reduce the diffusion flow of carbon to carbides, inhibit the coarsening of carbides, and a certain amount of Si can increase the strength of steel plates, improve the hardenability of steel, and reduce the ductile-brittle transition temperature within a certain range, thereby improving the plasticity of steel. Therefore, the Si content is limited to 0.20% to 0.35%.
[0018] Mn: 1.60%~1.80%
[0019] Mn plays a role of solid solution strengthening in steel. It can be dissolved in Fe matrix in large quantities to improve the strength and hardness of steel plate, improve hot working performance, prevent hot cracks, and improve the distribution of sulfides. By increasing the Mn content, the strength loss caused by the reduction of C content can be compensated, and the Mn content within a certain range can improve the toughness of weld metal and the solubility of Nb and V in steel. However, if the Mn content is too high, it is easy to form segregation in the steel plate, which is not good for plasticity and toughness. Therefore, Mn is limited to 1.60% to 1.80%.
[0020] P:≤0.015%
[0021] P is a harmful element in steel, which has a great impact on low temperature impact toughness and is also an element that is very easy to segregate, so its content should be controlled to be low during the steelmaking process. The present invention controls P within a range that does not affect the performance, so the P content is controlled to be below 0.015%.
[0022] S:≤0.005%
[0023] S is also a harmful element in steel. It is easy to form MnS in steel, which can easily become the source of crack formation in subsequent processing and has a great influence on the toughness of steel. However, considering the operability and cost of steelmaking, S is controlled below 0.005%.
[0024] Cr: 0.40%~0.50%
[0025] Cr, as the main element of this patent, is an element that stabilizes carbides. The addition of chromium reduces the dissolution rate of carbides, improves the toughness and hardenability of steel, and reduces local decarburization caused by the penetration and diffusion of H atoms in the metal lattice. During the quenching and tempering process, the Cr-containing carbides generated are dissolved in the matrix and refine the grains, so the Cr content is controlled between 0.40% and 0.50%.
[0026] Mo: 0.05%~0.15%
[0027] As the main element of this patent, Mo has a strong carbon fixation ability in steel, which can improve the corrosion resistance and reduce the defects such as decarburization and hydrogen bulging caused by H on the steel plate; it can also promote bainite transformation, inhibit the formation of grain boundary ferrite, provide nucleation sites for acicular ferrite during welding, improve welding performance, dissolve in austenite and ferrite through solid solution strengthening to improve the strength and toughness of steel, and also inhibit the occurrence of temper brittleness. However, a high content of Mo will increase the hardness and affect the subsequent processing performance, so the content is controlled between 0.05% and 0.15%.
[0028] Ni: 0.20%~0.40%
[0029] Ni is the main element for stabilizing austenite in steel. Ni can exist in austenite and ferrite in the form of solid solution with Fe, so it can improve the strength of steel, refine the grains, and improve the low-temperature impact toughness of steel. However, due to the high cost of nickel, it will also make it difficult to remove the iron oxide scale of the steel plate, thereby increasing the cost, so the Ni content is limited to between 0.20% and 0.40%.
[0030] V: 0.20%~0.40%
[0031] V can be dissolved into austenite at high temperature, and can increase the hardenability of steel after solid solution. V exists in steel mainly in the form of precipitates, and the strength and hardness of steel are guaranteed by precipitation strengthening. Microalloying can promote the increase of V-containing carbonitride compounds formed in steel. The precipitation of carbonitrides is conducive to providing intracrystalline ferrite nucleation coherent interface pinning at the grain boundary, inhibiting grain boundary movement and grain growth, and improving the toughness and tempering stability of steel; V elements can be compositely precipitated with inclusions, which is conducive to deformation-induced ferrite phase transformation; adjusting the ratio of V to C, the carbides formed by vanadium and carbon in steel increase, which can improve the hydrogen corrosion resistance of steel plates in low temperature and high pressure service environments. Therefore, V is limited to 0.20% to 0.40%.
[0032] Nb: 0.02%~0.03%
[0033] Nb in steel can inhibit austenite recrystallization during rolling, promote grain refinement, improve strength and toughness, reduce overheat sensitivity and temper brittleness, improve welding performance, and can also produce solid solution strengthening, precipitate a large amount of Nb (C, N) with dislocations on the grain boundaries, and low Nb content can improve the toughness of the heat-affected zone of steel plate welding. The heat-affected zone of steel plates with high Nb content cools slowly during high-line energy welding. Nb segregated at the grain boundaries is easy to precipitate under high Nb content, resulting in a carbon-poor zone, which promotes the nucleation and growth of ferrite on the austenite grain boundaries at high temperatures. Therefore, Nb is limited to 0.02% to 0.03%.
[0034] Ti: 0.02%~0.04%
[0035] Ti is the main element of this patent. As one of the most effective microalloying elements that promotes the formation of beneficial inclusions and acicular ferrite, it can form a large number of dispersed fine TiN or TiO particles. After Ti treatment during the steelmaking process, its content can change the composition, size and distribution of weld inclusions when it is within a reasonable range. And they can serve as the heterogeneous nucleation core of acicular ferrite during the solidification of the structure, and promote the formation of acicular ferrite in the grains during solidification and cooling, thereby playing a role in refining the grains. When w(Ti)≥0.09%, it will not only reduce the content of acicular ferrite, but also cause a large amount of bainite and hard-brittle phase MA components to form, which will deteriorate the low-temperature toughness of the steel plate. Therefore, the Ti content is limited to 0.02%~0.04%.
[0036] Al: 0.003%~0.005%
[0037] As the main deoxidizer in steel, Al can fix N elements, refine grains, and improve the toughness of steel. When welding steel plates, the nitrides precipitated at high temperatures can refine the structure of the heat-affected zone of welding. In order to make deoxidation and nitrogen fixation more complete, the Al content is limited to 0.003% to 0.005%.
[0038] Ca: 0.003%~0.005%
[0039] Ca acts as a deoxidizing and desulfurizing agent in steel and can modify inclusions. After oxide metallurgical treatment in the steelmaking process, beneficial composite inclusions can be obtained. After heat treatment, the inclusions can become spheroidized and small, providing nucleation sites for acicular ferrite. Therefore, the Ca content is limited to 0.003% to 0.005%.
[0040] The second technical solution of the present invention is to provide a method for manufacturing high-strength hydrogen storage container steel plate with excellent resistance to large linear energy, including the following process flow: smelting, continuous casting, slab heating, controlled rolling, cooling, and heat treatment.
[0041] 1. Smelting:
[0042] Specifically, it includes molten iron pretreatment - converter smelting - argon blowing and stirring - LF furnace refining - RH vacuum treatment.
[0043] The molten iron is first pre-treated in an argon station and controlled at 1350-1450°C. It is then blown at the top and bottom of a converter, and Ti iron is first added for deoxidation, and then Al wire, Ca wire, and Mg alloy wire are added, with an interval time of no more than 6 minutes, to deform the non-metallic inclusions in the molten steel and give play to the role of oxide metallurgy; the LF furnace is then used for refining and adjusting the composition, ensuring that the argon soft blowing time is 12-18 minutes, the refining time is 30-60 minutes, to ensure that the chemical composition of the molten steel is uniform and impurities are removed, and deep dephosphorization and desulfurization treatment are performed to reduce the P content in the molten steel to below 0.015%, and the S content to below 0.005%; RH vacuum treatment is then used for further refining and adjustment of the composition, ensuring that the molten steel temperature is 1600-1620°C, the vacuum degree is maintained at ≤5.0mbar, and the vacuum treatment time is 40-80 minutes, so that the inclusions in the molten steel can fully float, and the purity of the molten steel and the micro-alloying treatment time of the molten steel are ensured to be sufficient. By first adding Ti iron and then adding Al wire, Ca wire and Mg alloy wire, the non-metallic inclusions in the molten steel are deformed, the role of oxide metallurgy is brought into play, the quality of the continuous casting billet is improved, beneficial composite inclusion particles are obtained, and a heterogeneous nucleation core is provided for subsequent organization formation.
[0044] 2. Casting
[0045] The casting process is argon protected during the entire casting process. The light pressure reduction technology is used, the pressure reduction is controlled at 2-5mm, and the billet drawing speed is controlled at 0.9-1.3m / min to eliminate the internal defects of the casting and improve the surface quality of the casting. The beneficial composite inclusion particles can provide nucleation points for the grains of the casting to refine the grains of the casting. The secondary cooling water is controlled at 5000-6000L / min to improve the central segregation and central looseness of the casting and improve the internal quality of the casting. The casting superheat is 20-40℃ to improve the internal quality of the casting. The casting straightening temperature is controlled at 960±30℃ to reduce the generation of cracks in the casting, and a continuous casting billet with a thickness of 300-360mm is obtained. Finally, the slab is cleaned, slowly cooled, and the continuous casting billet quality is inspected.
[0046] 3. Heating
[0047] The continuous casting billet heating is divided into preheating section, heating section and soaking section: the preheating section is controlled at 700-800℃, the heating section is controlled at 1250-1300℃, the soaking section is controlled at 1180-1220℃, and the total time of the slab in the furnace is 210-270min to ensure the uniform temperature of the billet. By heating the billet in three stages, the temperature of the core of the billet reaches 1180-1220℃, ensuring that the billet structure is completely austenite; but when the heating temperature is higher than 1300℃, it is easy to cause excessive growth of the grains inside the billet, affecting the distribution of beneficial inclusions inside the structure.
[0048] 4. Rolling
[0049] After the billet is out of the furnace, a two-stage controlled rolling and controlled cooling technology is adopted. First, rough rolling is carried out, the starting rolling temperature is controlled at 1130-1180℃, the rolling speed is controlled at 1.1-1.5m / s, and the single-pass reduction rate of rough rolling is controlled at 12%-18%, ensuring that the total reduction rate of rough rolling is ≥55% to fully refine the austenite grains; the starting rolling temperature of finishing rolling is 900±50℃, the rolling temperature of the final rolling pass is controlled at 820-840℃, the rolling speed is controlled at 1.0-1.3m / s, the single-pass reduction rate of finishing rolling is ≥13%, and the total reduction rate of finishing rolling is ≥35%. The grains are further flattened and elongated, and the increase in the grain boundary area provides more nucleation sites for the subsequent phase transformation process. By controlling the total reduction rate of rough rolling and finishing rolling, the grains of the steel plate are sufficiently refined and the internal defects of the steel plate are eliminated. After rolling, controlled cooling is carried out, with the start cooling temperature of 750-800℃, the red return temperature of 580-650℃, and the cooling rate of 11-24℃ / s to ensure fine grains, promote the formation of fine precipitates, and improve the mechanical properties of the steel plate. Then the steel plate is stacked and slowly cooled, with the slow cooling temperature of 400-550℃, the number of steel plates stacked is 10-16, and the stacking time is guaranteed to be 16-24h, so that H and O in the steel plate have enough time to be eliminated. The thickness of the obtained steel plate is 36-60mm.
[0050] 5. Heat treatment
[0051] After stacking and slow cooling, the steel plate is subjected to quenching and tempering heat treatment. In order to ensure the various mechanical properties of the steel plate, the steel plate is first subjected to quenching and tempering heat treatment process, with a quenching temperature of 950±10℃, a quenching heating rate of 1.5±0.2min / mm, a tempering temperature of 620±10℃, a tempering heating rate of 1.4±0.3min / mm, and air cooling after the quenching and tempering heat treatment. Through quenching and tempering heat treatment, the beneficial composite inclusion particles are spheroidized and fine, and the fine precipitates in the organization are evenly distributed, ensuring that the steel plate has high strength and good low-temperature performance, and the steel plate organization is uniform, and the organization is bainite tempering organization (85-95% by volume) + acicular ferrite (5-15% by volume).
[0052] The beneficial effects of the present invention are:
[0053] The invention, based on the strengthening elements of C, Si and Mn, firstly reduces the C content in the steel to ensure that the carbon equivalent is sufficiently low and meets the excellent conditions of the welding performance of the steel plate. In order to ensure sufficient strength and toughness of the steel plate, the Mn content is increased to compensate for the strength loss caused by the reduction of the C content, and the Mn content within a certain range can improve the toughness of the weld metal and the solubility of Nb and V in the steel; by adding the carbon-fixing element Mo, it is dissolved in the matrix, the grains are refined, the local decarburization caused by the penetration and diffusion of hydrogen atoms in the metal lattice is reduced, the generation of steel plate defects caused by hydrogen atoms is reduced, and the hydrogen resistance of the steel plate is improved; a small amount of Ti content is added to form a large number of dispersed fine TiN or TiO particles, and after Ti treatment in the steelmaking process, the composition, size and distribution form of the weld inclusions can be changed, and they can be used as the heterogeneous nucleation core of the acicular ferrite during the solidification of the structure.
[0054] During oxygen converter smelting, Ti iron is first added, and then Al wire, Ca wire, and Mg alloy wire are added to deform the non-metallic inclusions in the molten steel, giving full play to the role of oxide metallurgy. After vacuum treatment, full-process protection casting is adopted during continuous casting to improve the quality of continuous casting billets, and beneficial composite inclusion particles can be obtained, which can be used as the heterogeneous nucleation core of acicular ferrite during organizational solidification. After heat treatment, the composite inclusion particles can become spheroidized, providing nucleation sites for acicular ferrite.
[0055] 1. The microstructure of the steel plate of the present invention is bainite tempered structure + acicular ferrite, the structure ratio is bainite tempered structure volume accounts for 85-95%, acicular ferrite volume accounts for 5-15%, the grain size is 8-10, and the average size of the composite inclusions is 1-3μm.
[0056] 2. The thickness of the steel plate of the present invention is 36-60 mm. After the steel plate for container is subjected to the quenching and tempering heat treatment process, the steel plate has higher strength performance, good low temperature performance and excellent mechanical properties after simulated post-weld heat treatment. Its mechanical properties are: yield strength R eL ≥600MPa, tensile strength R m :720~850MPa, elongation A≥21%, -50℃ low temperature impact toughness KV2≥100J, -50℃ low temperature tensile yield strength R eL ≥620MPa, tensile strength R m :735~880MPa, elongation A≥21%;
[0057] 3. The present invention adopts a large line energy of 100-150 kJ / cm to weld the steel plate, and the yield strength R of the welding heat affected zone (HAZ) eL ≥650MPa, tensile strength R m:800~920MPa, elongation ≥18%, -50℃ HAZ zone impact toughness KV2≥80J.
[0058] 4. The steel plate of the present invention has good resistance to hydrogen-induced cracking after heat treatment. The sample is immersed in solution A (5% by mass NaCl + 0.5% by mass acetic acid solution), filled with nitrogen for 60 to 80 minutes, immersed for 96 to 98 minutes, and the immersion solution temperature is 25±3°C. The crack length percentage CLR≤5%, the crack thickness percentage CTR≤5%, and the crack sensitivity percentage CSR≤5%.
[0059] 5. The present invention simulates the post-weld heat treatment process to test the mechanical properties of the steel plate. The simulated post-weld heat treatment temperature is 580-650°C and the insulation time is 120-360 minutes. The mechanical property requirements are: yield strength R eL ≥600MPa, tensile strength R m :720~850MPa, elongation A≥21%, -50℃ low temperature impact toughness KV2≥100J. DETAILED DESCRIPTION
[0060] The present invention will be further described below by way of examples.
[0061] The embodiment of the present invention performs smelting, continuous casting, slab heating, controlled rolling, cooling, and heat treatment according to the component ratio of the technical solution.
[0062] Slab heating
[0063] The preheating section is controlled at 700-800℃, the heating section is controlled at 1250-1300℃, the soaking section is controlled at 1180-1220℃, and the total slab in the furnace time is 210-270min;
[0064] Rolling
[0065] After the billet is out of the furnace, a two-stage controlled rolling and controlled cooling technology is adopted. The starting temperature of the rough rolling is 1130-1180℃, the rolling speed is controlled at 1.1-1.5m / s, the single-pass reduction rate is controlled at 12%-18%, and the total reduction rate is guaranteed to be ≥58%; the starting temperature of the finishing rolling is 900±50℃, the rolling temperature of the final rolling pass is 820-840℃, the rolling speed is controlled at 1.0-1.3m / s, the single-pass reduction rate of the finishing rolling is ≥13%, and the total reduction rate of the finishing rolling pass is guaranteed to be ≥35%;
[0066] cool down
[0067] After rolling, the steel plate is cooled under controlled conditions, with the cooling temperature at 750-800℃, the red-returning temperature at 580-650℃, and the cooling rate at 11-24℃ / s; then the plate is stacked and slowly cooled, with the slow cooling temperature at 400-550℃, the number of steel plates stacked is 10-16, and the stacking time is guaranteed to be 16-24h;
[0068] Heat Treatment
[0069] The steel plate is first subjected to a quenching and tempering heat treatment process, with a quenching temperature of 950±10°C, a quenching heating rate of 1.5±0.2min / mm, a tempering temperature of 620±10°C, a tempering heating rate of 1.4±0.3min / mm, and air cooling after the quenching and tempering heat treatment.
[0070] Furthermore, the smelting process includes top and bottom blowing in a converter, first adding Ti iron for deoxidation, then adding Al wire, Ca wire, and Mg alloy wire to deform the non-metallic inclusions in the molten steel; using LF furnace refining to adjust the composition, ensuring that the argon soft blowing time is 12-18 minutes and the refining time is 30-60 minutes; then using RH vacuum treatment to further refine and adjust the composition, ensuring that the molten steel temperature is 1600-1620°C, and the vacuum treatment time is 40-80 minutes.
[0071] Furthermore, the pouring process is argon-protected pouring throughout the process, and the billet is cast using light reduction technology. The reduction amount is controlled at 2-5 mm, the billet drawing speed is controlled at 0.9-1.3 m / min, the secondary cooling water is controlled at 5000-6000 L / min, the casting superheat is controlled at 20-40°C, and the billet straightening temperature is controlled at 960±30°C.
[0072] The embodiments specifically illustrate the content of the present invention. These embodiments are only general descriptions of the content of the present invention and do not limit the content of the present invention. Table 1 is the chemical composition of the embodiment, Table 2 is the smelting and casting method of the embodiment, Table 3 is the rolling process parameters of the embodiment, Table 4 is the cooling and heat treatment process parameters of the embodiment, Table 5 is the mechanical properties of the embodiment, Table 6 is the mechanical properties of the welding heat affected zone of the embodiment, Table 7 is the test results of the organizational volume, grain size and hydrogen cracking resistance of the embodiment, and Table 8 is the mechanical properties of the steel after heat treatment of the embodiment of the present invention.
[0073] Table 1 Chemical composition of the examples (wt%)
[0074]
[0075] Table 2 Example smelting and casting method
[0076]
[0077] Table 3 Example rolling process parameters
[0078]
[0079]
[0080] Table 4 Cooling and heat treatment process parameters of the embodiment
[0081]
[0082] Table 5 Mechanical properties of the examples
[0083]
[0084] Table 6 Mechanical properties of heat affected zone of welding of example
[0085]
[0086] Table 7 Example tissue volume, grain size and hydrogen-induced cracking resistance test results
[0087]
[0088]
[0089] Note: The sample is immersed in solution A, filled with nitrogen for 60-80 minutes, immersed for 96-98 hours, and the solution temperature is 25±3°C. Solution A is (5% by mass NaCl + 0.5% by mass acetic acid solution).
[0090] Table 8 Mechanical properties of steel after heat treatment in the present invention
[0091]
[0092] Note: The heat treatment temperature of mold welding is 580-650℃, and the holding time is 120-360min.
[0093] According to GB / T229-2020 "Metallic Materials Charpy Pendulum Impact Test Method", the weld heat affected zone was sampled and tested, and its -50℃ low-temperature impact toughness was above 100J, indicating that the weld heat affected zone of the steel plate has good low-temperature impact toughness. Tensile specimens were taken from the steel plate for tensile testing. The test was carried out in accordance with GB / T228.3-2019 "Metallic Materials Tensile Test Part 3: Low-temperature Test Method". The yield strength and tensile strength were both above 8, indicating that the steel plate has high strength and can be used in the low-temperature service environment of hydrogen storage; the grain size was measured according to GB / T6394-2017 "Method for Determination of Average Grain Size of Metals", and the grain size of the steel plate was above 8 levels, which indicates that the crack sensitivity of the steel plate is low; the anti-HIC performance of the steel plate was measured according to GB / T 8650-2015 "Evaluation Method for Hydrogen-Induced Cracking of Pipeline Steel and Pressure Vessel Steel", and the results showed that the designed steel grade has good anti-HIC performance. These fully demonstrate that the steel plate has excellent resistance to high line energy welding and hydrogen resistance.
[0094] As can be seen from the above, the steel plate of the present invention has high strength performance, good -50℃ low temperature impact toughness and excellent mechanical properties after simulated post-weld heat treatment. The mechanical properties of the steel plate and the mechanical properties of simulated post-weld heat treatment are: yield strength R eL ≥600MPa, tensile strength R m : 720~850MPa, elongation ≥21%, -50℃ low temperature impact toughness KV2 ≥100J, -50℃ low temperature tensile yield strength R eL ≥620MPa, tensile strength R m :735~880MPa, elongation ≥21%; use high wire energy 100~150kJ / cm to weld steel plates, the yield strength of the welding heat affected zone (HAZ) R eL ≥650MPa, tensile strength R m : 780~900MPa, elongation ≥18%, -50℃ HAZ zone impact toughness KV2≥80J, steel plate thickness specification 36~60mm; and has good resistance to hydrogen-induced cracking.
[0095] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. A high-strength hydrogen storage container steel plate having excellent resistance to large linear energy, characterized in that: Measured by weight percentage, it includes the following components: C: 0.08%-0.10%, Si: 0.20%-0.35%, Mn: 1.60%-1.80%, P: ≤0.015%, S: ≤0.005%, Cr: 0.40%-0.50%, Mo: 0.05%-0.15%, Ni: 0.20%-0.40%, V: 0.20%-0.25%, Nb: 0.02%-0.03%, Ti: 0.02%-0.04%, Al: 0.003%-0.005%, Ca: 0.003%-0.005%, and the balance is Fe and unavoidable impurities.
2. The high-strength steel plate for hydrogen storage container with excellent resistance to large linear energy according to claim 1, characterized in that: The component V / C≥2.
3. The high-strength steel plate for hydrogen storage container with excellent resistance to large linear energy according to claim 1, characterized in that: The steel plate has a yield strength ReL≥600MPa, a tensile strength Rm: 720-850MPa, an elongation ≥21%, an impact toughness KV2≥100J at -50°C, a low-temperature tensile yield strength ReL≥620MPa, a tensile strength Rm: 735-880MPa, and an elongation ≥21%.
4. The high-strength steel plate for hydrogen storage container with excellent resistance to large linear energy according to claim 1, characterized in that: The steel plates are welded with a large line energy of 100-150 kJ / cm, the yield strength of the welding heat affected zone (HAZ) ReL≥650 MPa, the tensile strength Rm: 780-900 MPa, the elongation ≥18%, and the impact toughness of the -50°C welding heat affected zone (HAZ) KV2≥80J.
5. The high-strength hydrogen storage container steel plate having excellent resistance to large linear energy according to claim 1, characterized in that: The steel plate microstructure is bainite tempered structure + acicular ferrite, the bainite tempered structure accounts for 85-95% of the volume, the acicular ferrite accounts for 5-15% of the volume, the grain size is 8-10, and the average size of the composite inclusions is 1-3 μm.
6. The high-strength hydrogen storage container steel plate having excellent resistance to large linear energy according to claim 1, characterized in that: The steel plate has a thickness of 36 to 60 mm.
7. A method for manufacturing a high-strength hydrogen storage container steel plate having excellent resistance to large linear energy according to any one of claims 1 to 6, comprising smelting, continuous casting, slab heating, controlled rolling, cooling, and heat treatment, characterized in that: Slab heating The preheating section is controlled at 700-800℃, the heating section is controlled at 1250-1300℃, the soaking section is controlled at 1180-1220℃, and the total slab in the furnace time is 210-270min; Rolling After the billet is out of the furnace, a two-stage controlled rolling and controlled cooling technology is adopted. The starting temperature of the rough rolling is 1130-1180℃, the rolling speed is controlled at 1.1-1.5m / s, the single-pass reduction rate is controlled at 12%-18%, and the total reduction rate is guaranteed to be ≥58%; the starting temperature of the finishing rolling is 900±50℃, the rolling temperature of the final rolling pass is 820-840℃, the rolling speed is controlled at 1.0-1.3m / s, the single-pass reduction rate of the finishing rolling is ≥13%, and the total reduction rate of the finishing rolling pass is guaranteed to be ≥35%; cool down After rolling, the steel plate is subjected to weak cooling, with the start cooling temperature of 750-800℃, the return temperature of 580-650℃, and the cooling rate of 11-24℃ / s; then it is stacked and slowly cooled, with the slow cooling temperature of 400-550℃, the number of steel plates stacked is 10-16, and the stacking time is guaranteed to be 16-24h; Heat Treatment The steel plate is first subjected to a quenching and tempering heat treatment process, with a quenching temperature of 950±10°C, a quenching heating rate of 1.5±0.2min / mm, a tempering temperature of 620±10°C, a tempering heating rate of 1.4±0.3min / mm, and air cooling after the quenching and tempering heat treatment.
8. The method for manufacturing a high-strength hydrogen storage container steel plate having excellent resistance to large linear energy according to claim 7, characterized in that: The smelting process includes top and bottom blowing in a converter, first adding Ti iron for deoxidation, then adding Al wire, Ca wire and Mg alloy wire, ensuring that the argon soft blowing time is 12-18 minutes; using an LF furnace for refining and adjusting the composition, the refining time is 30-60 minutes; then using RH vacuum treatment and further refining and adjusting the composition, ensuring that the molten steel temperature is 1600-1620°C, and the vacuum treatment time is 40-80 minutes.
9. The method for manufacturing a high-strength hydrogen storage container steel plate having excellent resistance to large linear energy according to claim 7, characterized in that: The pouring process is argon-protected pouring throughout the process, and the billet is cast using light reduction technology. The reduction amount is controlled at 2-5mm, the billet drawing speed is controlled at 0.9-1.3m / min, the secondary cooling water is controlled at 5000-6000L / min, the casting superheat is controlled at 20-40°C, and the billet straightening temperature is controlled at 960±30°C.
Citation Information
Patent Citations
Steel plate for high-quality low-temperature oil storage tank and production method of steel plate
CN116574981A
Corrosion-resistant ultra-large heat input welding steel plate and production method thereof
CN117070855A
Ultrahigh-strength welded structural steel having excellent toughness in welding heat-affected zones thereof, and production method therefor
CN105829565A
High strength steel material having excellent hydrogen-induced cracking resistance and low-temperature impact toughness and manufacturing method therefor
CN111492083A
High strength hot rolled steel having excellent scale adhesivness and a method of manufacturing the same
CN112739841A
Cited By
Manufacturing method of continuous casting slab for full-protection pouring of crude oil storage tank container steel
CN119819887A