Inorganic nanofiber composite scaffold as well as preparation method and application thereof
By distributing magnesium ions in inorganic nanofibers and modifying them with polydopamine, the problem of insufficient biocompatibility of bone repair materials is solved, achieving more effective bone repair and antibacterial effects, and is suitable for osteoporosis and tumor bone defects. treatment.
Patent Information
- Application Number
- CN202410712634.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-11
AI Technical Summary
Existing bone repair materials have problems with biocompatibility, leading to inflammation and rejection, affecting the repair effect and patients' quality of life.
It uses a composite scaffold in which magnesium ions are distributed in inorganic nanofibers, and is modified with polydopamine to improve biocompatibility and photothermal conversion performance, promote bone repair and inhibit bacterial growth.
It improves the biocompatibility and bone repair efficiency of bone repair materials, enhances the effect of photothermal treatment, reduces the risk of infection, and is suitable for the treatment of osteoporosis and tumor bone defects.
Smart Images

Figure CN118750643A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedical materials, and specifically relates to an inorganic nanofiber composite scaffold and a preparation method and application thereof. Background Art
[0002] As the trend of population aging continues to intensify, bone defects have become an important factor that threatens human health and affects the quality of life. Bone defect problems mainly include the treatment of osteoporosis and tumor bone defects, both of which cause great trouble to patients' lives. Osteoporosis is a common bone disease, which is characterized by decreased bone mass, slow repair, unstable internal fixation and high failure rate. This makes it difficult for traditional treatments to achieve ideal results. In the treatment of bone tumors, it is usually necessary to remove the bone tissue invaded by the tumor, but even so, tumor cells may still remain in the bone defect site, leading to secondary damage. Therefore, bone repair materials have become one of the important ways to solve the problem of bone defect repair.
[0003] The design of bone repair materials must take into account multiple aspects, including biocompatibility, mechanical tolerance, biodegradability, and induced regeneration. The combination of these properties affects the effect and safety of the material in the process of bone defect repair.
[0004] However, most bone repair materials on the market currently have poor biocompatibility. This may manifest as adverse reactions between the material and surrounding tissues, including inflammation, rejection, etc., thus affecting the repair effect and the patient's quality of life. Therefore, solving the problem of poor biocompatibility of bone repair materials is one of the key challenges that need to be urgently addressed in the current orthopedic field. Only by developing safer and more effective bone repair materials can we bring better treatment effects and quality of life to patients. Summary of the invention
[0005] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the present invention provides an inorganic nanofiber composite scaffold that overcomes the biocompatibility problem of traditional bone repair materials. Magnesium ions are distributed in the inorganic nanofiber substrate, which can repair bones well. After being modified with polydopamine, the biocompatibility of the composite scaffold is better and photothermal therapy can be better performed.
[0006] The invention also provides a method for preparing the inorganic nanofiber composite scaffold.
[0007] The present invention also provides an application of an inorganic nanofiber composite scaffold in preparing a bone repair material.
[0008] A first aspect of the present invention provides an inorganic nanofiber composite scaffold, comprising an inorganic nanofiber substrate, magnesium ions are distributed in the inorganic nanofiber substrate, and polydopamine is connected to the surface of the inorganic nanofiber substrate.
[0009] One of the technical solutions of the present invention regarding the inorganic nanofiber composite scaffold has at least the following beneficial effects:
[0010] Magnesium can promote bone growth and solve the problem of slow bone repair in osteoporosis. Based on the advantages of magnesium, the present invention selects to prepare magnesium-doped inorganic nanofiber composite scaffolds, which can strengthen bone repair by stimulating the function of osteoclasts, and can effectively solve the limitations of drug treatment and bone repair. Dopamine is an important building block of material surface modification methods. Because its product polydopamine has the advantages of easy preparation and modification, strong adhesion, biocompatibility, excellent photothermal conversion performance, fluorescence quenching, etc., and the photothermal properties of polydopamine enhance the photothermal conversion efficiency, can promote bone repair, and can inhibit the growth of bacteria during the repair process. Therefore, the present invention selects to prepare magnesium-doped inorganic nanofibers and polydopamine-modified composite scaffolds, which are suitable for various applications such as tumor bone defects.
[0011] The composite scaffold of the present invention overcomes the biocompatibility problem of traditional bone repair materials. Magnesium ions are distributed in the inorganic nanofiber substrate, which can repair bones well. After being modified with polydopamine, the composite scaffold has better biocompatibility and can better perform photothermal therapy.
[0012] In the composite stent of the present invention, the magnesium ions are distributed inside the inorganic nanofibers, and compared with those distributed on the fiber surface, the sustained action is more lasting and the effect is better.
[0013] According to some embodiments of the present invention, the diameter of the inorganic nanofiber substrate is 200-3000 nm.
[0014] Compared with common fibers such as silk (usually with a diameter of 13 μm-18 μm), the fiber of the present invention has a diameter of 200-3000 nm, a higher specific surface area, and can be modified with more polydopamine on the surface, resulting in better material effects.
[0015] According to some embodiments of the present invention, the inorganic nanofiber substrate comprises silicate glass fibers.
[0016] According to some embodiments of the present invention, the content of magnesium in the inorganic nanofiber substrate is 0.5 wt % to 10 wt %.
[0017] According to some embodiments of the present invention, the content of magnesium in the inorganic nanofibers can be any value among 0.5w%, 1w%, 2w%, 3w%, 4w%, 5w%, 6w%, 7w%, 8w%, 9w%, 10wt% or a range formed by any two of them.
[0018] According to some embodiments of the present invention, the content of polydopamine on the surface of the inorganic nanofiber substrate is 0.5 wt % to 3 wt %.
[0019] According to some embodiments of the present invention, the pore size of the inorganic nanofiber composite scaffold is 100 μm to 400 μm.
[0020] The pore size of the inorganic nanofiber composite scaffold is 100μm to 400μm, which can provide enough space to promote the invasion, settlement and growth of surrounding tissue cells, and is conducive to the combination and regeneration of the scaffold and surrounding tissues. The internal structure of the scaffold pores is reasonable, which helps to effectively transport nutrients to the inside of the scaffold, and can also quickly discharge metabolic products to maintain the normal metabolic function of the tissue. The appropriate pore size can reduce the weight of the scaffold and the stiffness of the material while maintaining sufficient material strength, so as to better simulate the mechanical properties of natural tissues.
[0021] A pore size below 100 μm may limit the invasion and growth of cells, resulting in a weak bond between the scaffold and surrounding tissues, affecting the repair effect; a pore size above 400 μm may cause the mechanical strength of the scaffold to decrease, reducing the stability and reliability of the scaffold, and may also prevent cells from effectively settling and growing, affecting the tissue regeneration process.
[0022] Therefore, controlling the pore size of inorganic nanofiber composite scaffolds within the range of 100 μm to 400 μm can maximize the biological and mechanical functions of the scaffolds and promote tissue repair and regeneration.
[0023] According to some embodiments of the present invention, axial grooves are distributed on the surface of the inorganic nanofiber substrate.
[0024] The presence of axial grooves can significantly increase the effective contact area of the scaffold surface, provide more bioactive areas, and facilitate cell attachment and growth. The directionality of the grooves can provide growth guidance for the surrounding cells, help the cells to arrange and grow in a specific direction, and promote the directional regeneration of tissues. The groove structure can provide a channel for cell migration, which is conducive to the migration and diffusion of cells on the scaffold surface, thereby promoting tissue regeneration and repair. The grooves can also provide more biological adhesion sites, enhance the bonding between the scaffold and the surrounding tissues, and improve the implantation stability and long-term effects of the scaffold. The groove structure can be used as a carrier to control and regulate the release of bioactive substances on the scaffold, thereby achieving precise regulation of the tissue regeneration process.
[0025] Therefore, the axial grooves in the inorganic nanofiber composite scaffolds can improve the bioactivity, tissue compatibility and functionality of the scaffolds, help promote tissue repair and regeneration, and enhance the clinical effects and application prospects of the scaffolds.
[0026] A second aspect of the present invention provides a method for preparing an inorganic nanofiber composite scaffold, comprising the following steps:
[0027] S1: mixing an inorganic salt solution containing magnesium ions with a template polymer to prepare a spinning suspension, electrospinning to obtain inorganic nanofibers, and calcining the inorganic nanofibers;
[0028] S2: dispersing the inorganic nanofibers obtained in step S1 in a liquid to obtain a fiber dispersion, and mixing the dispersion with a stent thickener to prepare a stent suspension;
[0029] S3: freeze-forming the scaffold suspension to obtain a scaffold blank, and immersing the scaffold blank in a dopamine solution to obtain the inorganic nanofiber composite scaffold.
[0030] A technical solution in the method for preparing an inorganic nanofiber composite scaffold of the present invention has at least the following beneficial effects:
[0031] The preparation method of the inorganic nanofiber composite scaffold of the present invention can accurately control the morphology and arrangement of the inorganic nanofibers through electrostatic spinning and freeze molding in liquid, thereby adjusting the pore structure and pore size of the scaffold to make it more in line with the needs of tissue engineering.
[0032] After the inorganic nanofibers are mixed with the scaffold thickener, a fiber dispersion is formed, which is conducive to uniformly dispersing the nanofibers in the scaffold, thereby enhancing the biocompatibility and bioactivity of the scaffold.
[0033] By combining calcined inorganic nanofibers and scaffold thickeners, the mechanical properties and stability of the scaffold can be effectively improved, enhancing its durability and reliability in vivo.
[0034] After soaking in dopamine solution, the surface of the scaffold is connected with polydopamine, which is beneficial to the adhesion and growth of cells and promotes the tissue regeneration and repair process.
[0035] The preparation method of the inorganic nanofiber composite scaffold of the present invention has simple operation and clear steps, does not require complicated equipment and conditions, is suitable for large-scale production, and has high engineering practicality and economy.
[0036] In step S1:
[0037] The inorganic salt solution contains magnesium ions, and the solvent includes at least one of anhydrous ethanol, N,N-dimethylformamide, dichloromethane and hexafluoroisopropanol.
[0038] The function of the magnesium source is to provide magnesium ions. In the inorganic salt solution, the concentration of magnesium element ranges from 0.05wt% to 10wt%.
[0039] The magnesium source includes at least one of magnesium chloride, magnesium oxide, magnesium nitride, magnesium hydroxide and magnesium-containing nitrate.
[0040] The role of silicon source is to provide silicon ions, which participate in the physiological process of regulating bone formation and bone calcification and play an important role in bone metabolism. In the inorganic salt solution, the concentration range of silicon element is 0.05wt% to 13wt%.
[0041] Silicon sources include ethyl silicate.
[0042] The role of the calcium source is to provide calcium ions, which can not only regulate the proliferation and differentiation of various cells (mesenchymal stem cells, osteoblasts and osteoclasts) in the bone repair stage, but also regulate osteogenesis by promoting the formation of new blood vessels at the bone defect and promoting the release of growth factors. The concentration range of calcium in the inorganic salt solution is 0.01wt% to 15wt%.
[0043] Calcium sources include calcium nitrate tetrahydrate.
[0044] The role of the acidic catalyst is to make the substances react better. In the inorganic salt solution, the concentration range of the catalyst is 1wt% to 2wt%.
[0045] The acidic catalyst includes at least one of acetic acid, hydrochloric acid and phosphoric acid.
[0046] According to some embodiments of the present invention, the template polymer comprises an alcohol-soluble template polymer or a water-soluble template polymer.
[0047] According to some embodiments of the invention, the template polymer comprises polyvinyl butyral, polyvinyl alcohol or polyvinyl pyrrolidone.
[0048] According to some embodiments of the present invention, the template polymer can be first dissolved in alcohol or water to prepare a template polymer solution, in which the concentration of the template polymer is 5 wt % to 15 wt %.
[0049] According to some embodiments of the present invention, the mass ratio of the template polymer to the inorganic salt solution containing magnesium ions is 1:(1-5).
[0050] According to some embodiments of the present invention, the spinning room temperature of the electrospinning is 25°C to 40°C.
[0051] According to some embodiments of the present invention, the humidity of the electrospinning is 35% to 50%.
[0052] According to some embodiments of the present invention, the perfusion rate of the electrospinning is 0.5 mL / h to 3 mL / h.
[0053] According to some embodiments of the present invention, the drum speed of the electrospinning is 5 rpm to 100 rpm.
[0054] According to some embodiments of the present invention, the spinning voltage of the electrospinning is 10 kV to 30 kV.
[0055] According to some embodiments of the present invention, the calcination temperature is 600°C to 800°C.
[0056] According to some embodiments of the present invention, the calcination time is 6 h to 12 h.
[0057] In step S2:
[0058] The inorganic nanofibers obtained in step S1 are dispersed in a liquid, which may be deionized water. The dispersion may be performed by breaking the fibers into a fiber dispersion liquid using a high-speed homogenizer.
[0059] The stent viscosity enhancing agent includes at least one of a chitosan solution and alginate.
[0060] The stent thickener can be first prepared with solvent acetic acid to prepare a stent thickener solution, and the concentration of the stent thickener in the stent thickener solution is in the range of 2wt% to 5wt%.
[0061] In step S3:
[0062] The scaffold suspension is freeze-formed, and the freezing is vacuum freezing. The prepared scaffold suspension can be filled into a mold made of a thermoplastic plate and put into a refrigerator for freezing. The temperature can be -80°C and the freezing time can be 1h to 2h. The scaffold blank is obtained by vacuum freeze drying technology.
[0063] The mold made of thermoplastic board can be a 1 cm×1 cm×1 cm mold made of thermoplastic (PET) board.
[0064] The stent blank can be cut into small discs of uniform thickness and diameter, and an appropriate amount of dopamine solution is added to soak the small discs. The soaking time in the polydopamine solution can be 12h to 24h. The concentration of polydopamine can be 0.5wt% to 1.5wt%. Then, deionized water is added for washing, and the discs are placed in an ultra-low temperature refrigerator for freezing and then vacuum freeze-dried. The vacuum freeze-drying time can be 24h to 48h.
[0065] By controlling the concentration of dopamine, inorganic nanofiber scaffolds modified with dopamine at different concentrations can be obtained.
[0066] Finally, the prepared composite stent can be sterilized as needed, and the sterilization methods include ultraviolet irradiation sterilization, X-ray irradiation sterilization, gamma ray irradiation sterilization, and 75% alcohol sterilization.
[0067] The third aspect of the present invention provides the use of an inorganic nanofiber composite scaffold or an inorganic nanofiber composite scaffold prepared by the method of the present invention in the preparation of a bone repair material.
[0068] The present invention provides a technical solution for the application of inorganic nanofiber composite scaffolds in the preparation of bone repair materials, which has at least the following beneficial effects:
[0069] The inorganic nanofiber composite scaffold of the present invention, or the inorganic nanofiber composite scaffold prepared by the method of the present invention, when used in the preparation of bone repair materials, magnesium ions as bioactive elements can promote bone growth and bone tissue regeneration, solving the problem of slow repair speed of traditional bone repair materials in the treatment of osteoporosis, thereby accelerating the speed of fracture healing and bone defect repair. The surface of the dopamine-modified composite scaffold has good biocompatibility and adhesion, can promote the attachment and growth of bone cells, enhance the bone repair effect, and can also inhibit the growth of bacteria during the repair process, reducing the risk of infection. The dopamine-modified composite scaffold has excellent photothermal conversion performance, can improve the efficiency of photothermal therapy, and further promote the repair and regeneration of bone tissue.
[0070] Magnesium ions are distributed inside the inorganic nanofibers. Compared with magnesium ions distributed on the surface, their effect is more lasting and can continuously promote bone growth and repair, making the therapeutic effect of the scaffold more lasting and stable.
[0071] By introducing magnesium ions and modifying dopamine, the biocompatibility problem of traditional bone repair materials was effectively overcome, making the composite scaffold more suitable for clinical applications and reducing the treatment risk for patients. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] Figure 1 This is the SEM image of the inorganic nanofibers prepared in Example 1.
[0073] Figure 2 The figure and SEM image of the unmodified scaffold prepared in Example 1.
[0074] Figure 3 This is a diagram of the mechanical properties of the stent prepared in Example 1.
[0075] Figure 4 This is a photo of the stent modified with polydopamine prepared in Example 1.
[0076] Figure 5 It is a wet thermal imaging and temperature rise data diagram of the polydopamine scaffold prepared in Example 1.
[0077] Figure 6 The inhibition zones of the polydopamine-modified scaffold prepared in Example 1 in Escherichia coli solution (a) and Staphylococcus aureus solution (b).
[0078] Figure 7 This is a cell map of the magnesium-doped inorganic nanofiber scaffold prepared in Example 1.
[0079] Figure 8 This is a CT image of a rat skull defect repaired 12 weeks after the polydopamine scaffold of Example 1 was implanted. DETAILED DESCRIPTION
[0080] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0081] In the first aspect, in some embodiments of the present invention, the inorganic nanofiber composite scaffold comprises an inorganic nanofiber substrate, magnesium ions are distributed in the inorganic nanofiber substrate, and polydopamine is connected to the surface of the inorganic nanofiber substrate.
[0082] It can be understood that magnesium can promote bone growth and solve the problem of slow bone repair in osteoporosis. Based on the advantages of magnesium, the present invention selects to prepare an inorganic nanofiber composite scaffold doped with magnesium, which can strengthen bone repair by stimulating the function of osteoclasts, and can effectively solve the limitations of drug therapy and bone repair. Dopamine is an important building block of material surface modification methods. Because its product polydopamine has the advantages of easy preparation and modification, strong adhesion, biocompatibility, excellent photothermal conversion performance, fluorescence quenching, etc., and the photothermal properties of polydopamine enhance the photothermal conversion efficiency, can promote bone repair, and can inhibit the growth of bacteria during the repair process. Therefore, the present invention selects to prepare a composite scaffold modified by polydopamine of magnesium-doped inorganic nanofibers, which is suitable for various applications such as tumor bone defects.
[0083] It can also be understood that the composite scaffold of the present invention overcomes the biocompatibility problem of traditional bone repair materials. Magnesium ions are distributed in the inorganic nanofiber substrate, which can repair bones well. After being modified with polydopamine, the composite scaffold has better biocompatibility and can better perform photothermal therapy.
[0084] It should be noted that, in the composite stent of the present invention, the magnesium ions are distributed inside the inorganic nanofibers, which has a more lasting effect and a better effect than when they are distributed on the fiber surface.
[0085] In combination with the first aspect, in some embodiments of the present invention, the diameter of the inorganic nanofiber substrate is 200-3000 nm.
[0086] Compared with common fibers such as silk (usually with a diameter of 13 μm-18 μm), the fiber of the present invention has a diameter of 200-3000 nm, a higher specific surface area, and can be modified with more polydopamine on the surface, resulting in better material effects.
[0087] In conjunction with the first aspect, in some embodiments of the present invention, the inorganic nanofiber substrate includes silicate glass fibers.
[0088] In combination with the first aspect, in some embodiments of the present invention, the content of magnesium in the inorganic nanofiber substrate is 0.5 wt % to 10 wt %.
[0089] In combination with the first aspect, in some embodiments of the present invention, the content of magnesium in the inorganic nanofiber substrate can be any value among 0.5w%, 1w%, 2w%, 3w%, 4w%, 5w%, 6w%, 7w%, 8w%, 9w% or a range formed by any two of them.
[0090] In combination with the first aspect, in some embodiments of the present invention, the content of polydopamine on the surface of the inorganic nanofiber substrate is 0.5 wt % to 3 wt %.
[0091] In combination with the first aspect, in some embodiments of the present invention, the pore size of the inorganic nanofiber composite scaffold is 100 μm to 400 μm.
[0092] The pore size of the inorganic nanofiber composite scaffold is 100μm to 400μm, which can provide enough space to promote the invasion, settlement and growth of surrounding tissue cells, and is conducive to the combination and regeneration of the scaffold and surrounding tissues. The internal structure of the scaffold pores is reasonable, which helps to effectively transport nutrients to the inside of the scaffold, and can also quickly discharge metabolic products to maintain the normal metabolic function of the tissue. The appropriate pore size can reduce the weight of the scaffold and the stiffness of the material while maintaining sufficient material strength, so as to better simulate the mechanical properties of natural tissues.
[0093] A pore size below 100 μm may limit the invasion and growth of cells, resulting in a weak bond between the scaffold and surrounding tissues, affecting the repair effect; a pore size above 400 μm may cause the mechanical strength of the scaffold to decrease, reducing the stability and reliability of the scaffold, and may also prevent cells from effectively settling and growing, affecting the tissue regeneration process.
[0094] Therefore, controlling the pore size of inorganic nanofiber composite scaffolds within the range of 100 μm to 400 μm can maximize the biological and mechanical functions of the scaffolds and promote tissue repair and regeneration.
[0095] In combination with the first aspect, in some embodiments of the present invention, axial grooves are distributed on the surface of the inorganic nanofiber substrate.
[0096] The presence of axial grooves can significantly increase the effective contact area of the scaffold surface, provide more bioactive areas, and facilitate cell attachment and growth. The directionality of the grooves can provide growth guidance for the surrounding cells, help the cells to arrange and grow in a specific direction, and promote the directional regeneration of tissues. The groove structure can provide a channel for cell migration, which is conducive to the migration and diffusion of cells on the scaffold surface, thereby promoting tissue regeneration and repair. The grooves can also provide more biological adhesion sites, enhance the bonding force between the scaffold and the surrounding tissues, and improve the implantation stability and long-term effects of the scaffold. The groove structure can be used as a carrier to control and regulate the release of bioactive substances on the scaffold, so as to achieve precise regulation of the tissue regeneration process. The grooves may be caused by the removal of PVB during the calcination process. If the calcination temperature is not enough or the calcination time is not enough, grooves cannot be formed on the fiber surface.
[0097] Therefore, the axial grooves in the inorganic nanofiber composite scaffolds can improve the bioactivity, tissue compatibility and functionality of the scaffolds, help promote tissue repair and regeneration, and improve the clinical effects and application prospects of the scaffolds.
[0098] In a second aspect, some embodiments of the present invention provide a method for preparing an inorganic nanofiber composite scaffold, comprising the following steps:
[0099] S1: mixing an inorganic salt solution containing magnesium ions with a template polymer to prepare a spinning suspension, electrospinning to obtain inorganic nanofibers, and calcining the inorganic nanofibers;
[0100] S2: dispersing the inorganic nanofibers obtained in step S1 in a liquid to obtain a fiber dispersion, and mixing the dispersion with a stent thickener to prepare a stent suspension;
[0101] S3: freeze-forming the scaffold suspension to obtain a scaffold blank, and immersing the scaffold blank in a dopamine solution to obtain the inorganic nanofiber composite scaffold.
[0102] It can be understood that the preparation method of the inorganic nanofiber composite scaffold of the present invention can accurately control the morphology and arrangement of inorganic nanofibers through electrospinning and freeze-forming in liquid, thereby adjusting the pore structure and pore size of the scaffold to make it more in line with the needs of tissue engineering.
[0103] After the inorganic nanofibers are mixed with the scaffold thickener, a fiber dispersion is formed, which is conducive to uniformly dispersing the nanofibers in the scaffold, thereby enhancing the biocompatibility and bioactivity of the scaffold.
[0104] By combining calcined inorganic nanofibers and scaffold thickeners, the mechanical properties and stability of the scaffold can be effectively improved, enhancing its durability and reliability in vivo.
[0105] After soaking in dopamine solution, the surface of the scaffold is connected with polydopamine, which is beneficial to the adhesion and growth of cells and promotes the tissue regeneration and repair process.
[0106] The preparation method of the inorganic nanofiber composite scaffold of the present invention has simple operation and clear steps, does not require complicated equipment and conditions, is suitable for large-scale production, and has high engineering practicality and economy.
[0107] Furthermore, in step S1:
[0108] The inorganic salt solution contains magnesium ions, and the solvent includes at least one of anhydrous ethanol, N,N-dimethylformamide, dichloromethane and hexafluoroisopropanol.
[0109] The function of the magnesium source is to provide magnesium ions. In the inorganic salt solution, the concentration of magnesium element ranges from 0.05wt% to 10wt%.
[0110] The magnesium source includes at least one of magnesium chloride, magnesium oxide, magnesium nitride, magnesium hydroxide and magnesium-containing nitrate.
[0111] The role of silicon source is to provide silicon ions, which participate in the physiological process of regulating bone formation and bone calcification and play an important role in bone metabolism. In the inorganic salt solution, the concentration range of silicon element is 0.05wt% to 13wt%.
[0112] Silicon sources include ethyl silicate.
[0113] The role of the calcium source is to provide calcium ions, which can not only regulate the proliferation and differentiation of various cells (mesenchymal stem cells, osteoblasts and osteoclasts) in the bone repair stage, but also regulate osteogenesis by promoting the formation of new blood vessels at the bone defect and promoting the release of growth factors. The concentration range of calcium in the inorganic salt solution is 0.01wt% to 15wt%.
[0114] Calcium sources include calcium nitrate tetrahydrate.
[0115] The role of the acidic catalyst is to make the substances react better. In the inorganic salt solution, the concentration range of the catalyst is 1wt% to 2wt%.
[0116] The acidic catalyst includes at least one of acetic acid, hydrochloric acid and phosphoric acid.
[0117] The acidic catalyst includes at least one of acetic acid, hydrochloric acid and phosphoric acid.
[0118] In conjunction with the second aspect, in some embodiments of the present invention, the template polymer includes an alcohol-soluble template polymer or a water-soluble template polymer.
[0119] In conjunction with the second aspect, in some embodiments of the present invention, the template polymer includes polyvinyl butyral, polyvinyl alcohol or polyvinyl pyrrolidone.
[0120] In combination with the second aspect, in some embodiments of the present invention, the template polymer may be first dissolved in alcohol or water to prepare a template polymer solution, in which the concentration of the template polymer is 5 wt % to 15 wt %.
[0121] In combination with the second aspect, in some embodiments of the present invention, the mass ratio of the template polymer to the inorganic salt solution containing magnesium ions is 1:1-5.
[0122] In combination with the second aspect, in some embodiments of the present invention, the spinning room temperature of electrospinning is 25°C to 40°C.
[0123] In combination with the second aspect, in some embodiments of the present invention, the humidity of electrospinning is 35% to 50%.
[0124] In combination with the second aspect, in some embodiments of the present invention, the perfusion rate of electrospinning is 0.5 mL / h to 3 mL / h.
[0125] In combination with the second aspect, in some embodiments of the present invention, the drum speed of electrospinning is 5 rpm to 100 rpm.
[0126] In combination with the second aspect, in some embodiments of the present invention, the spinning voltage of electrospinning is 10 kV to 30 kV.
[0127] In combination with the second aspect, in some embodiments of the present invention, the calcination temperature is 600°C to 800°C.
[0128] In combination with the second aspect, in some embodiments of the present invention, the calcination time is 6 hours to 12 hours.
[0129] In step S2:
[0130] The inorganic nanofibers obtained in step S1 are dispersed in a liquid, which may be deionized water. The dispersion may be performed by breaking the fibers into a fiber dispersion liquid using a high-speed homogenizer.
[0131] The stent viscosity enhancing agent includes at least one of a chitosan solution and alginate.
[0132] The stent thickener can be first prepared with solvent acetic acid to prepare a stent thickener solution, and the concentration of the stent thickener in the stent thickener solution is in the range of 2wt% to 5wt%.
[0133] In step S3:
[0134] The scaffold suspension is freeze-formed, and the freezing is vacuum freezing. The prepared scaffold suspension can be filled into a mold made of a thermoplastic plate and put into a refrigerator for freezing. The temperature can be -80°C and the freezing time can be 1h to 2h. The scaffold blank is obtained by vacuum freeze drying technology.
[0135] The mold made of thermoplastic board can be a 1cm×1cm×1cm mold made of thermoplastic (PET) board, and molds of other shapes and sizes can also be selected according to needs.
[0136] The stent blank can be cut into small discs of uniform thickness and diameter, and an appropriate amount of dopamine solution is added to soak the small discs. The soaking time in the polydopamine solution can be 12h to 24h. The concentration of polydopamine can be 0.5wt% to 1.5wt%. Then, deionized water is added for washing, and the discs are placed in an ultra-low temperature refrigerator for freezing and then vacuum freeze-dried. The vacuum freeze-drying time can be 24h to 48h.
[0137] By controlling the concentration of dopamine, inorganic nanofiber scaffolds modified with dopamine at different concentrations can be obtained.
[0138] Finally, the prepared composite stent can be sterilized as needed, and the sterilization methods include ultraviolet irradiation sterilization, X-ray irradiation sterilization, and gamma ray irradiation sterilization.
[0139] In the third aspect, some embodiments of the present invention provide use of an inorganic nanofiber composite scaffold or an inorganic nanofiber composite scaffold prepared by the method of the present invention in the preparation of a bone repair material.
[0140] The inorganic nanofiber composite scaffold of the present invention, or the inorganic nanofiber composite scaffold prepared by the method of the present invention, when used in the preparation of bone repair materials, magnesium ions as bioactive elements can promote bone growth and bone tissue regeneration, solving the problem of slow repair speed of traditional bone repair materials in the treatment of osteoporosis, thereby accelerating the speed of fracture healing and bone defect repair. The surface of the dopamine-modified composite scaffold has good biocompatibility and adhesion, can promote the attachment and growth of bone cells, enhance the bone repair effect, and can also inhibit the growth of bacteria during the repair process, reducing the risk of infection. The dopamine-modified composite scaffold has excellent photothermal conversion performance, can improve the efficiency of photothermal therapy, and further promote the repair and regeneration of bone tissue.
[0141] Magnesium ions are distributed inside the inorganic nanofibers. Compared with magnesium ions distributed on the surface, their effect is more lasting and can continuously promote bone growth and repair, making the therapeutic effect of the scaffold more lasting and stable.
[0142] By introducing magnesium ions and modifying dopamine, the biocompatibility problem of traditional bone repair materials was effectively overcome, making the composite scaffold more suitable for clinical applications and reducing the treatment risk for patients.
[0143] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0144] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0145] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.
[0146] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.
[0147] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0148] Example 1
[0149] An inorganic nanofiber composite scaffold was prepared, specifically:
[0150] In the first step, 4g PVB powder is mixed with 36mL of anhydrous ethanol. PVB powder is added to the stirring table to prevent incomplete dissolution in the anhydrous ethanol. The stirring time is 2-3h to prepare a 10% PVB solution. Inorganic salt solution preparation: add 8g anhydrous ethanol, 1.2g ultrapure water, 0.4g glacial acetic acid, 0.096g anhydrous magnesium chloride, 8.5g ethyl silicate, 2.36g calcium nitrate tetrahydrate, and stir for 1h. The above two solutions are mixed in a mass ratio of 1:2, placed on a magnetic stirrer for stirring to form a spinning suspension;
[0151] In the second step, the spinning suspension is sucked into the needle tube. The spinning suspension is used to prepare the fiber through the electrospinning device. The temperature of the spinning room is 25-30℃, the humidity is 35%-45%, the infusion speed is 1mL / h, the roller speed is 65r / min, and the spinning voltage is 20kv;
[0152] The third step is to place the fiber membrane formed by electrospinning in a muffle furnace and calcine it at 800°C for 8 hours.
[0153] The fourth step is to take 1g of calcined inorganic nanofibers and add 50mL of deionized water, and use a high-speed homogenizer to break up the fibers to prepare a fiber dispersion. Take 0.1mol acetic acid solution as the solvent, measure 19.6mL and add 0.4g of chitosan particles, stir evenly to prepare a 2% chitosan acetic acid solution. Take 50mL of the prepared fiber dispersion and 2% chitosan acetic acid solution in a ratio of 7:3, mix thoroughly and evenly to prepare a suspension of the scaffold;
[0154] Step 5: Fill the prepared scaffold suspension into a mold made of thermoplastic plate and place it in a refrigerator at -80°C for 2 hours. After vacuum freeze drying for 48 hours, a three-dimensional bionic scaffold is obtained.
[0155] The sixth step is to cut the prepared inorganic nanofiber scaffold into small discs of uniform thickness and diameter, add 1% polydopamine solution to soak the small discs, react for 24 hours, add deionized water to wash 2-3 times, put into -80℃ ultra-low temperature refrigerator to freeze for 30 minutes, and vacuum freeze-dry for 48 hours to obtain a scaffold modified with polydopamine, i.e., an inorganic nanofiber composite scaffold.
[0156] The inorganic nanofiber composite scaffold prepared in this embodiment has axial grooves distributed on the surface of the inorganic nanofiber substrate. After testing, the diameter of the inorganic nanofiber substrate is 2μm~3μm, the magnesium content in the inorganic nanofiber substrate is 0.6wt%, the polydopamine content on the surface of the inorganic nanofiber substrate is 1wt%, and the pore size of the inorganic nanofiber composite scaffold is 100μm~400μm.
[0157] Example 2
[0158] An inorganic nanofiber composite scaffold was prepared, specifically:
[0159] In the first step, 4g PVB powder is mixed with 16mL anhydrous ethanol. PVB powder is added to the stirring table to prevent incomplete dissolution in the anhydrous ethanol. The stirring time is 2-3h to prepare a 5% PVB solution. Inorganic salt solution preparation: add 8g anhydrous ethanol, 1.2g ultrapure water, 0.4g glacial acetic acid, 0.096g anhydrous magnesium chloride, 8.5g ethyl silicate, 2.36g calcium nitrate tetrahydrate, and stir for 1h. The above two solutions are mixed in a mass ratio of 1:4, placed on a magnetic stirrer for stirring to form a spinning suspension;
[0160] In the second step, the spinning suspension is sucked into the needle tube. The spinning suspension is used to prepare the fiber through the electrospinning device. The temperature of the spinning room is 25-30℃, the humidity is 35%-45%, the infusion speed is 1mL / h, the roller speed is 65r / min, and the spinning voltage is 20kv;
[0161] The third step is to place the fiber membrane formed by electrospinning in a muffle furnace and calcine it at 800°C for 8 hours.
[0162] The fourth step is to take 1g of calcined inorganic nanofibers and add 50mL of deionized water, and use a high-speed homogenizer to break up the fibers to prepare a fiber dispersion. Take 0.1mol acetic acid solution as the solvent, measure 19.6mL and add 0.4g of chitosan particles, stir evenly to prepare a 2% chitosan acetic acid solution. Take 50mL of the prepared fiber dispersion and 2% chitosan acetic acid solution in a ratio of 7:3, mix thoroughly and evenly to prepare a suspension of the scaffold;
[0163] Step 5: Fill the prepared scaffold suspension into a mold made of thermoplastic plate and place it in a refrigerator at -80°C for 2 hours. After vacuum freeze drying for 48 hours, a three-dimensional bionic scaffold is obtained.
[0164] The sixth step is to cut the prepared inorganic nanofiber scaffold into small discs of uniform thickness and diameter, add 0.5% polydopamine solution to soak the small discs for 24 hours, add deionized water to wash 2-3 times, put them in a -80°C ultra-low temperature refrigerator and freeze them for 30 minutes, and vacuum freeze-dry them for 48 hours to obtain a scaffold modified with polydopamine, i.e., an inorganic nanofiber composite scaffold.
[0165] The inorganic nanofiber composite scaffold prepared in this embodiment has axial grooves distributed on the surface of the inorganic nanofiber substrate. After testing, the diameter of the inorganic nanofiber substrate is 2μm~3μm, the magnesium content in the inorganic nanofiber substrate is 0.8wt%, the polydopamine content on the surface of the inorganic nanofiber substrate is 0.5wt%, and the pore size of the inorganic nanofiber composite scaffold is 100μm~400μm.
[0166] Example 3
[0167] An inorganic nanofiber composite scaffold was prepared, specifically:
[0168] In the first step, 4g PVB powder is mixed with 56mL anhydrous ethanol. PVB powder is added to the stirring table to prevent incomplete dissolution in the anhydrous ethanol. The stirring time is 2-3h to prepare a 15% PVB solution. Inorganic salt solution preparation: add 8g anhydrous ethanol, 1.2g ultrapure water, 0.4g glacial acetic acid, 0.096g anhydrous magnesium chloride, 8.5g ethyl silicate, 2.36g calcium nitrate tetrahydrate, and stir for 1h. The above two solutions are mixed in a mass ratio of 1:5, placed on a magnetic stirrer for stirring to form a spinning suspension;
[0169] In the second step, the spinning suspension is sucked into the needle tube. The spinning suspension is used to prepare the fiber through the electrospinning device. The temperature of the spinning room is 25-30℃, the humidity is 35%-45%, the infusion speed is 1mL / h, the roller speed is 65r / min, and the spinning voltage is 20kv;
[0170] The third step is to place the fiber membrane formed by electrospinning in a muffle furnace and calcine it at 800°C for 10 hours.
[0171] The fourth step is to take 1g of calcined inorganic nanofibers and add 50mL of deionized water, and use a high-speed homogenizer to break up the fibers to prepare a fiber dispersion. Take 0.1mol acetic acid solution as the solvent, measure 19.6mL and add 0.4g of chitosan particles, stir evenly to prepare a 2% chitosan acetic acid solution. Take 50mL of the prepared fiber dispersion and 2% chitosan acetic acid solution in a ratio of 7:3, mix thoroughly and evenly to prepare a suspension of the scaffold;
[0172] Step 5: Fill the prepared scaffold suspension into a mold made of thermoplastic plate and place it in a refrigerator at -80°C for 2 hours. After vacuum freeze drying for 48 hours, a three-dimensional bionic scaffold is obtained.
[0173] The sixth step is to cut the prepared inorganic nanofiber scaffold into small discs of uniform thickness and diameter, add 1.5% polydopamine solution to soak the small discs for 24 hours, add deionized water to wash 2-3 times, put them in a -80°C ultra-low temperature refrigerator to freeze for 30 minutes, and vacuum freeze-dry for 48 hours to obtain a scaffold modified with polydopamine, i.e., an inorganic nanofiber composite scaffold.
[0174] The inorganic nanofiber composite scaffold prepared in this embodiment has axial grooves distributed on the surface of the inorganic nanofiber substrate. After testing, the diameter of the inorganic nanofiber substrate is 2μm~3μm, the magnesium content in the inorganic nanofiber substrate is 0.8wt%, the polydopamine content on the surface of the inorganic nanofiber substrate is 1.5wt%, and the pore size of the inorganic nanofiber composite scaffold is 100μm~400μm.
[0175] Example 4
[0176] An inorganic nanofiber composite scaffold was prepared, specifically:
[0177] In the first step, 4g of PVA powder is mixed with 25℃ distilled water, stirred for 10-15 minutes to fully disperse the particles, and then heated to 95℃ while stirring (hot-melt PVA). Prepare an inorganic salt solution, add 8g of anhydrous ethanol, 1.2g of ultrapure water, 0.4g of glacial acetic acid, 0.096g of anhydrous magnesium chloride, 8.5g of ethyl silicate, and 2.36g of calcium nitrate tetrahydrate, and stir for 1h. Mix the above two solutions in a ratio of 1:3, place on a magnetic stirrer and stir for 1-2h to make a spinning suspension;
[0178] The second step is to suck the spinning suspension with a needle. The spinning suspension is passed through an electrospinning device to prepare fibers. The temperature in the spinning room is 30-34°C, the humidity is 45%-50%, the infusion speed is 0.8mL / h, the drum speed is 65r / min, and the spinning voltage is 10kv;
[0179] The third step is to place the fiber membrane formed by electrospinning in a muffle furnace and calcine it at 800°C for 10 hours.
[0180] The fourth step is to take the calcined inorganic nanofibers and add deionized water, and use a high-speed homogenizer to break the fibers into a fiber dispersion. Mix the sodium alginate powder with deionized water, stir evenly to make a 2% sodium alginate solution, and soak it in a calcium ion solution for cross-linking. Mix the cross-linked sodium alginate with the fiber dispersion, and mix them thoroughly to make a suspension of the scaffold;
[0181] Step 5: Fill the prepared scaffold suspension into a mold made of thermoplastic plate and freeze it in a refrigerator at -80°C for 2 hours. Then, vacuum freeze-dry for 48 hours to obtain a three-dimensional bionic scaffold.
[0182] The sixth step is to cut the prepared inorganic nanofiber scaffold into small discs of uniform thickness and diameter, add 2% polydopamine solution to soak the small discs for 24 hours, add deionized water to wash 2-3 times, put them in a -80°C ultra-low temperature refrigerator to freeze for 30 minutes, and vacuum freeze-dry for 48 hours to obtain a scaffold modified with polydopamine, i.e., an inorganic nanofiber composite scaffold.
[0183] The inorganic nanofiber composite scaffold prepared in this embodiment has axial grooves distributed on the surface of the inorganic nanofiber substrate. After testing, the diameter of the inorganic nanofiber substrate is 2μm~3μm, the magnesium content in the inorganic nanofiber substrate is 0.6wt%, the polydopamine content on the surface of the inorganic nanofiber substrate is 0.5wt%, and the pore size of the inorganic nanofiber composite scaffold is 100μm~400μm.
[0184] Comparative Example 1
[0185] The difference between this comparative example and Example 1 is that after electrospinning, the nanofibers are immersed in an inorganic salt solution containing magnesium ions, and the magnesium ions are distributed on the surface of the composite scaffold, rather than inside the nanofibers. The specific preparation method is:
[0186] (1) hot pressing the stacked multi-layer flat silk to obtain a hot pressed silk fiber substrate;
[0187] (2) soaking the hot-pressed silk fiber substrate in a ternary solution, taking it out and freeze-drying it to obtain a pretreated silk fiber substrate, wherein the ternary solution includes CaCl2, ethanol and water;
[0188] (3) The pretreated silk fiber substrate is immersed in a solution containing 0.01 wt % of magnesium ions to perform modification, thereby obtaining a silk scaffold material modified with polydopamine and magnesium ions.
[0189] The stent prepared in this comparative example was tested and found that the magnesium content on the surface of the inorganic nanofiber substrate was 0.01 wt %, and the polydopamine content on the surface of the inorganic nanofiber substrate was 0.3 wt %.
[0190] Comparative Example 2
[0191] The difference between this comparative example and Example 1 is that the calcination temperature is 400° C., and the surface of the composite scaffold fiber finally obtained has no grooves.
[0192] Performance Testing
[0193] In summary, the polydopamine-modified composite scaffold prepared above has excellent photothermal conversion performance and biocompatibility. It also has antibacterial effects while providing treatment, and can effectively promote bone repair and inhibit tumor growth.
[0194] Taking Example 1 as an example, Figure 1 As shown, the diameter distribution of the magnesium-doped inorganic nanofibers is uniform, and there are grooves along the longitudinal surface of the fibers. The reason for the grooves is presumably the removal of PVB during the calcination process.
[0195] like Figure 2 As shown, the pore size of the prepared scaffold should be between 100 μm and 400 μm.
[0196] like Figure 3 As shown, the prepared stent has good resilience and elasticity.
[0197] like Figure 7 As shown, the magnification is 200 times, from Figure 7 It can be seen that there are mostly green living cells and fewer dead cells, indicating that the prepared scaffold has excellent biocompatibility.
[0198] The three-dimensional scaffold modified with polydopamine prepared in Example 1 was subjected to photothermal effect measurement and cut into small discs with a diameter of 1 cm and a thickness of 0.2 cm. Figure 4 As shown, the wet sample is placed under 2W infrared light. Figure 5 As shown in the wet infrared imaging of the three-dimensional scaffold, the maximum temperature of the three-dimensional scaffold in Example 1 of the present invention in the wet state reaches 83°C and becomes basically stable within 2-3 minutes, indicating that the scaffold modified with polydopamine has a good photothermal effect.
[0199] The antibacterial performance of the three-dimensional scaffold modified with polydopamine prepared in Example 1 was tested. After Escherichia coli and Staphylococcus aureus were diluted 20 times respectively, three small discs of the scaffold modified with polydopamine were prepared and placed in 100 μl of Escherichia coli and Staphylococcus aureus solutions respectively.
[0200] like Figure 6 As shown, an obvious inhibition zone was formed around the polydopamine scaffold, indicating that the scaffold modified with polydopamine had excellent antibacterial properties.
[0201] Furthermore, the polydopamine-modified scaffold was made into a small disc with a diameter of 1 cm and a thickness of 0.2 cm for the treatment of skull defects in mice.
[0202] like Figure 8 As shown, after twelve weeks, observation of the mouse skull CT revealed obvious bone growth in the mouse head, proving that the scaffold has excellent osteogenic repair ability and good osteogenic activity, and can be used as a bone tissue regeneration scaffold in bone tissue repair.
[0203] In the scaffold of Comparative Example 1, magnesium ions are distributed on the surface of the composite scaffold. Compared with Example 1, magnesium ions are included in the fiber spinning and are distributed inside the nanofibers, resulting in a relatively slow release, which can avoid the cytotoxicity caused by excessive release of magnesium ions, thereby inhibiting the mineralization and maturation of bone tissue.
[0204] The scaffold of comparative example 2 has no grooves on the fiber surface, and the effective contact area of the scaffold surface is small, which is not conducive to cell attachment and growth. Compared with the scaffold of example 1, the biological activity, tissue compatibility and functionality of the scaffold are deteriorated.
[0205] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. An inorganic nanofiber composite scaffold, characterized in that: The invention comprises an inorganic nanofiber substrate, magnesium ions are distributed in the inorganic nanofiber substrate, and polydopamine is connected to the surface of the inorganic nanofiber substrate.
2. The inorganic nanofiber composite scaffold according to claim 1, characterized in that: The pore size of the inorganic nanofiber composite scaffold is 100 μm to 400 μm.
3. The inorganic nanofiber composite scaffold according to claim 1, characterized in that: Axial grooves are distributed on the surface of the inorganic nanofiber substrate.
4. A method for preparing the inorganic nanofiber composite scaffold according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: mixing an inorganic salt solution containing magnesium ions with a template polymer to prepare a spinning suspension, electrospinning to obtain inorganic nanofibers, and calcining the inorganic nanofibers; S2: dispersing the inorganic nanofibers obtained in step S1 in a liquid to obtain a fiber dispersion, and mixing the dispersion with a stent thickener to prepare a stent suspension; S3: freeze-forming the scaffold suspension to obtain a scaffold blank, and immersing the scaffold blank in a dopamine solution to obtain the inorganic nanofiber composite scaffold.
5. The method according to claim 4, characterized in that The inorganic salt solution containing magnesium ions contains a magnesium source, a silicon source, a calcium source and an acidic catalyst.
6. The method according to claim 4, characterized in that The template polymer includes an alcohol-soluble template polymer or a water-soluble template polymer.
7. The method according to claim 4, characterized in that The stent viscosity enhancer includes at least one of chitosan and alginate.
8. The method according to claim 4, characterized in that The process parameters of the electrospinning include: a spinning room temperature of 25°C to 40°C; and / or a humidity of 35% to 50%; and / or an infusion speed of 0.5mL / h to 3mL / h; and / or a roller speed of 5rpm to 100rpm; and / or a spinning voltage of 10kV to 30kV.
9. The method according to claim 4, characterized in that The calcination temperature is 600°C to 800°C.
10. Use of the inorganic nanofiber composite scaffold according to any one of claims 1 to 3 or the inorganic nanofiber composite scaffold prepared by the method according to any one of claims 4 to 9 in the preparation of bone repair materials.