Multilayer current collector welding method and equipment
Through the combined pressing method of intermediate and peripheral pressing, the problem of excessive gap between multi-layer current collector and pole column in lithium-ion battery welding is solved, and the reliability and welding quality of laser welding are improved.
Patent Information
- Application Number
- CN202411221797.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-02
AI Technical Summary
In the existing lithium-ion battery welding technology, the gap between the multi-layer current collector and the pole column is too large, which affects the quality of laser penetration welding and leads to the insolid welding.
The combined pressing method of intermediate block and peripheral block is adopted. The multi-layer current collector is pressed with the welded part of the pole column through the intermediate block, and the hollow area of the peripheral block is used for laser light after the intermediate block is removed. Welding ensures the tight fit between the multi-layer current collector and the pole column and reduces gaps.
It effectively reduces the gap between the multi-layer current collector and the pole column, improves the reliability and welding quality of laser welding, and ensures the full fusion area of the welding material.
Smart Images

Figure CN118752071B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion battery welding, and in particular to a welding method and equipment for multi-layer current collectors. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density and long cycle life, and are widely used in new energy power and energy storage equipment.
[0003] Due to the differences in battery structure design, there is a need to directly connect the multi-layer current collector to the battery cover. Under normal circumstances, the multi-layer current collector is welded and pressed by ultrasound, and then the multi-layer current collector is connected to the positive / negative poles inside the cover by laser penetration welding. Laser welding requires a certain fusion area to meet the flow requirement. However, since the upper layer of the material to be welded is a copper / aluminum current collector, there is still a small gap between the multi-layer current collectors pre-welded by ultrasound. The lower layer of the material to be welded is a copper / aluminum material with high reflectivity, with a smooth and flat surface, and is at the same level. During the laser welding process, the laser weld mark needs to be completed in a completely unobstructed situation, so a U-shaped contact flat pressure head is required to pre-press the welding area, so that the corresponding equipment is hollowed out at the weld mark.
[0004] This welding method has the following problems: the multilayer current collector in the ultrasonic welding area is no longer soft and thin, and has a certain hardness. When the center is hollowed out and the flat pressure head on all sides is directly pressed on the ultrasonic weld mark, it can only ensure that the multilayer current collector in the direct contact area of the U-shaped flat pressure head is in good contact with the pole, and there is still a risk of too large a gap between the multilayer current collector in the laser welding area and the lower pole. For laser penetration welding, the gap between the upper and lower layers of materials to be welded has a great influence on its welding quality. If the gap between the upper and lower layers of materials to be welded is slightly larger, for copper and aluminum materials with high reflectivity, the laser will be reflected multiple times on the surface of the upper and lower layers of materials to be welded, and the energy absorbed by the lower layer of material to be welded is greatly reduced, thereby reducing the fusion area between the two layers, thereby reducing the welding quality between the multilayer current collector and the pole. Summary of the invention
[0005] The main purpose of the present application is to provide a welding method and equipment for a multi-layer current collector, so as to solve the problem in the prior art that the gap between the multi-layer current collector and the pole during welding is too large, thereby affecting the quality of laser penetration welding.
[0006] One embodiment of the present application provides a welding method for a multi-layer current collector, comprising the following steps:
[0007] Place the pole on the welding table;
[0008] The battery cell is arranged close to the welding station, and the multi-layer current collector of the battery cell is arranged in contact with the pole;
[0009] Using an intermediate pressing block to press the multi-layer current collector and the to-be-welded portion of the pole;
[0010] The multi-layer current collector is pressed around the part to be welded of the pole by using a peripheral pressing block, wherein the interior of the peripheral pressing block has a hollow area, and the middle pressing block is located in the hollow area;
[0011] Removing the middle pressing block to expose the hollow area of the peripheral pressing block;
[0012] The laser welding head is moved above the portion to be welded, and the laser emitted by the laser welding head passes through the hollow area of the peripheral pressing block to weld the multi-layer current collector and the portion to be welded of the pole.
[0013] In one embodiment, the intermediate pressing block is a columnar structure;
[0014] The pole has a first surface that is in contact with the multi-layer current collector, and the first surface is protruded toward the multi-layer current collector;
[0015] The intermediate pressing block has a second surface for pressing the portion to be welded, the second surface is recessed in a direction away from the multilayer current collector, and the shapes of the second surface and the first surface match so that when the intermediate pressing block is used to press the portion to be welded, the multilayer current collector and the portion to be welded of the pole are tightly fitted.
[0016] In one embodiment, the first surface is an arcuate convex surface, and the second surface is an arcuate concave surface;
[0017] Alternatively, the first surface is composed of a first plane and a second plane, and the first plane and the second plane together form a convex shape, so that the height of the center position of the first surface is greater than the height of the two end positions of the first surface; the second surface is composed of a third plane and a fourth plane, and the third plane and the fourth plane together form a concave shape, so that the height of the center position of the second surface is greater than the height of the two end positions of the second surface.
[0018] In one embodiment, the peripheral pressing block comprises:
[0019] A body, wherein the hollow area is arranged inside the body;
[0020] A fixing member is arranged on the bottom surface of the main body and surrounds the hollow area; and
[0021] A movable part, arranged on the fixed part and connected to the fixed part through an elastic part;
[0022] When the peripheral pressing block presses the multi-layer current collector and the surroundings of the to-be-welded portion of the pole, the movable member is pressed around the to-be-welded portion, and the elastic member is in a compressed state and provides a pressing force for the movable member.
[0023] In one embodiment, the intermediate pressing block is a roller structure, and during the pressing process:
[0024] The roller structure rolls along the length direction of the hollow area, so as to tightly press the multi-layer current collector and the to-be-welded portion of the pole;
[0025] Then, the peripheral pressing block is used to press the multi-layer current collector and the surroundings of the part to be welded of the pole, and the roller structure is hidden.
[0026] In one embodiment, the intermediate pressing block is a roller structure;
[0027] The peripheral pressing block includes a first pressing rod, a second pressing rod, a third pressing rod and a fourth pressing rod, which are arranged together around the hollow area, and the first pressing rod and the second pressing rod are respectively arranged close to two short sides of the hollow area, and the third pressing rod and the fourth pressing rod are respectively arranged close to two long sides of the hollow area; during the pressing process:
[0028] Firstly, press the first pressing rod onto one of the short sides of the part to be welded;
[0029] Then, the roller structure is rolled along the length direction of the hollow area, and the rolling direction is from a position close to the first pressure rod to a position close to the second pressure rod;
[0030] Then, the second pressing rod is pressed onto the other short side of the part to be welded;
[0031] Then, the third pressing rod and the fourth pressing rod are pressed onto two long sides of the part to be welded respectively, and the roller structure is hidden.
[0032] In one embodiment, the peripheral pressing block comprises:
[0033] A body, wherein the hollow area is arranged inside the body;
[0034] A fixing member is arranged on the bottom surface of the body and surrounds the hollow area, and a moving track is arranged along the length direction of the hollow area on the fixing member, so that the roller structure is rolled along the moving track;
[0035] The first pressure rod, the second pressure rod, the third pressure rod and the fourth pressure rod are arranged on the fixing member and protrude from the fixing member, a first elastic member is arranged between the first pressure rod and the fixing member, and a second elastic member is arranged between the second pressure rod and the fixing member;
[0036] In the unpressed state, the length of the first pressing rod extending out of the fixing member is greater than the length of the second pressing rod extending out of the fixing member.
[0037] In one embodiment, a third elastic member is provided between the third pressure rod and the fixing member, and a fourth elastic member is provided between the fourth pressure rod and the fixing member;
[0038] In the unpressed state, the length of the second pressing rod extending out of the fixing member is greater than the length of the third pressing rod or the fourth pressing rod extending out of the fixing member.
[0039] In one embodiment, the third pressure rod and the fourth pressure rod are integrally arranged;
[0040] The fixing member is provided with a first magnetic member;
[0041] The third pressure rod and the fourth pressure rod are provided with a second magnetic member;
[0042] The first magnetic member and / or the second magnetic member are electromagnetic induction elements. When not pressed together, power is applied to attract the first magnetic member and the second magnetic member, so that the length of the third pressure rod and the fourth pressure rod extending out of the fixing member is less than the length of the second pressure rod extending out of the fixing member. When pressed together, reverse power is applied to repel the first magnetic member and the second magnetic member, so that the third pressure rod and the fourth pressure rod are pressed together in the peripheral area of the multi-layer current collector and the pole at the part to be welded.
[0043] Another embodiment of the present application further provides a multi-layer current collector welding device, including a welding table, a cell placement platform, an intermediate pressing block, a peripheral pressing block, and a laser welding head:
[0044] The welding table is used for placing the pole;
[0045] The battery cell placement platform is used to place the battery cells and to fit the multi-layer current collectors of the battery cells with the poles;
[0046] The intermediate pressing block is used to press the multi-layer current collector and the to-be-welded portion of the pole, and is removed after the peripheral pressing blocks are pressed to reveal the hollowed-out area of the peripheral pressing blocks;
[0047] A peripheral pressing block, used to press the multi-layer current collector and the surroundings of the to-be-welded portion of the pole after the intermediate pressing block presses the to-be-welded portion, wherein the peripheral pressing block has the hollow region inside, and the intermediate pressing block is located in the hollow region;
[0048] The laser welding head is located above the portion to be welded, and the laser emitted by the laser welding head passes through the hollow area of the peripheral pressing block to weld the multi-layer current collector and the portion to be welded of the pole.
[0049] The welding method and equipment of the multi-layer current collector of the present application have the following advantages and beneficial effects:
[0050] 1. In the welding method of the multilayer current collector provided in the present application, the gap between the multilayer current collector and the pole can be effectively reduced by first using an intermediate pressing block to press the multilayer current collector with the part to be welded of the pole, and then using a peripheral pressing block to press the multilayer current collector with the surrounding parts of the part to be welded of the pole, and then removing the intermediate pressing block to reveal the hollow area of the peripheral pressing block, thereby ensuring the reliability of laser welding. In fact, in the above welding method, even if there is a gap between the multilayer current collector and the pole due to the upward warping of the multilayer current collector, the gap can be effectively removed due to the pressing effect of the intermediate pressing block. Then, the peripheral pressing block is used to press the periphery of the welding area on the basis of maintaining the intermediate pressing block. At this time, if the intermediate pressing block is removed again, due to the pressing effect of the peripheral pressing block, the close fit between the multilayer current collector and the pole can be effectively maintained to avoid the multilayer current collector from returning to the state of upward warping due to the action of internal stress. At the same time, after removing the intermediate pressing block, the hollow area of the peripheral pressing block exposed facilitates the laser penetration welding operation of the laser welding head. During the laser penetration welding process, since the multi-layer current collector and the pole are in close contact, the laser will not be reflected multiple times on the surfaces of the upper and lower layers of the materials to be welded, but will be absorbed by the welding material to the greatest extent, thereby ensuring that there is a sufficient fusion area between the multi-layer current collector and the pole, thereby ensuring the reliability of laser penetration welding.
[0051] 2. In one embodiment, the pole has a first surface that fits with the multi-layer current collector, and the first surface is protruded toward the multi-layer current collector. The intermediate pressing block has a second surface for pressing the portion to be welded, and the second surface is concave in a direction away from the multi-layer current collector. Since the first surface of the pole is protruded toward the multi-layer current collector, even if the multi-layer current collector is warped upward, the protruding shape of the first surface of the pole can effectively reduce the gap between the pole and the multi-layer current collector. At this time, the portion to be welded is pressed again by the intermediate pressing block. Since the shape of the second surface of the intermediate pressing block matches the first surface, during the pressing process, the multi-layer current collector and the portion to be welded of the pole can fit tightly, thereby ensuring the reliability of laser penetration welding.
[0052] 3. In one embodiment, the first surface is composed of a first plane and a second plane. The first plane and the second plane together form a convex shape, so that the height of the center position of the first surface is greater than the height of the two end positions of the first surface. The second surface is composed of a third plane and a fourth plane. The third plane and the fourth plane together form a concave shape, so that the height of the center position of the second surface is greater than the height of the two end positions of the second surface. Through the combination of two planes, the first surface of the pole can effectively achieve a state of protruding toward the multilayer current collector. At this time, a certain height difference is formed between the center position of the pole and the two side positions, thereby reducing the gap between the multilayer current collector and the pole, thereby ensuring the reliability of subsequent laser penetration welding.
[0053] 4. In one embodiment, the peripheral pressing block includes a fixed part and a movable part. The movable part and the fixed part are connected by an elastic part. When the peripheral pressing block presses the multilayer current collector and the parts to be welded of the pole around, the movable part is pressed around the parts to be welded, and the elastic part is in a compressed state and provides a pressing force for the movable part. In the above embodiment, the pressing force of the movable part on the periphery of the parts to be welded is provided by the elastic part in a compressed state, thereby ensuring that the peripheral pressing block has a suitable pressing force on the periphery of the parts to be welded. The multilayer current collector will not be damaged due to excessive pressing force, nor will the multilayer current collector be restored to an upward warped state due to internal stress due to excessive pressing force, thereby ensuring the reliability of the subsequent laser penetration welding process.
[0054] 5. In one embodiment, the intermediate pressing block is a roller structure. During the pressing process, the roller structure rolls along the length direction of the hollow area, so that the multilayer current collector is tightly pressed with the part to be welded of the pole. Then the peripheral pressing block is used to press the multilayer current collector around the part to be welded of the pole, and the roller structure is hidden. By first rolling the roller structure along the length direction of the hollow area, the multilayer current collector is tightly pressed with the part to be welded of the pole. Then the peripheral pressing block is used to press the multilayer current collector around the part to be welded of the pole, the gap between the multilayer current collector and the pole can be effectively reduced, thereby ensuring the reliability of laser welding. In addition, due to the small size of the roller structure, the roller structure is hidden in the peripheral pressing block, and the subsequent removal of the intermediate pressing block can be realized. The above implementation method ensures the reliability of the subsequent laser penetration welding process while also ensuring the convenience of the laser penetration welding process.
[0055] 6. In one embodiment, the intermediate pressing block is a roller structure. The peripheral pressing block includes a first pressing rod, a second pressing rod, a third pressing rod and a fourth pressing rod. During the pressing process, the first pressing rod is first pressed on one of the short sides of the part to be welded; then the roller structure is rolled along the length direction of the hollow area, and the rolling direction is from the position close to the first pressing rod to the position close to the second pressing rod; then the second pressing rod is pressed on the other short side of the part to be welded; then the third pressing rod and the fourth pressing rod are respectively pressed on the two long sides of the part to be welded, and the roller structure is hidden. Through the pre-pressing of the first pressing rod, when the roller structure rolls along the length direction of the hollow area, the position of the multilayer current collector will not move at will, thereby ensuring that this process can effectively reduce the gap between the multilayer current collector and the pole. When the roller structure rolls to a position close to the second pressing rod, the second pressing rod is pressed again. At this time, since the first pressure rod and the second pressure rod are respectively arranged at the two ends of the hollow area, they can effectively keep the multilayer current collector and the pole in a tightly fitted state. Finally, the third pressure rod and the fourth pressure rod are respectively pressed on the two long sides of the part to be welded to achieve the final pressing.
[0056] 7. In one embodiment, the first pressure rod, the second pressure rod, the third pressure rod and the fourth pressure rod are arranged on the fixing member and protrude from the fixing member. A first elastic member is arranged between the first pressure rod and the fixing member, and a second elastic member is arranged between the second pressure rod and the fixing member. In the case of no pressing, the length of the first pressure rod extending out of the fixing member is greater than the length of the second pressure rod extending out of the fixing member. At this time, in the process of pressing down the peripheral pressure block, it can be ensured that the first pressure rod first contacts the periphery of the area to be welded, thereby realizing the pre-pressing action. After the rolling process of the roller structure along the length direction of the hollow area is completed, the peripheral pressure block is continued to be pressed downward, so that the second pressure rod can also contact the periphery of the area to be welded, thereby realizing the pressing function.
[0057] 8. In one embodiment, a third elastic member is provided between the third pressure rod and the fixing member, and a fourth elastic member is provided between the fourth pressure rod and the fixing member. In the case of no pressing, the length of the second pressure rod extending out of the fixing member is greater than the length of the third pressure rod or the fourth pressure rod extending out of the fixing member. At this time, when the second pressure rod is also pressed on the periphery of the area to be welded, the peripheral pressure block is continued to be pressed downward, so that the third pressure rod and the fourth pressure rod can be pressed on the two long sides of the area to be welded respectively. That is, through the above setting method, it can be achieved that in the process of pressing the peripheral pressure block downward, the first pressure rod is pre-pressed first, the second pressure rod is pressed, and then the third pressure rod and the fourth pressure rod are pressed. The above operation method is simple and convenient, and is easy to operate during the welding process.
[0058] 9. In one embodiment, the third pressure rod and the fourth pressure rod are integrally arranged. A first magnetic member is arranged on the fixing member. A second magnetic member is arranged on the third pressure rod and the fourth pressure rod. The first magnetic member and / or the second magnetic member are electromagnetic induction elements. In the case of no pressing, the first magnetic member and the second magnetic member are attracted by power, so that the length of the third pressure rod and the fourth pressure rod extending out of the fixing member is less than the length of the second pressure rod extending out of the fixing member. In the case of pressing, reverse power is applied to repel the first magnetic member and the second magnetic member, so that the third pressure rod and the fourth pressure rod are pressed in the peripheral area of the to-be-welded part of the multilayer current collector and the pole. That is, by providing the first magnetic member on the fixing member and the second magnetic member on the third pressure rod and the fourth pressure rod, in the case of no pressing, the first magnetic member and the second magnetic member are attracted by power, so that the length of the third pressure rod and the fourth pressure rod extending out of the fixing member is less than the length of the second pressure rod extending out of the fixing member. By setting the first magnetic part and the second magnetic part, it is also possible to achieve the process of pre-pressing the first pressure rod, then pressing the second pressure rod, and then pressing the third pressure rod and the fourth pressure rod during the process of pressing the peripheral pressure block downward. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0060] Figure 1 A schematic diagram of the steps of a welding method for a multi-layer current collector disclosed in one embodiment of the present application;
[0061] Figure 2 for Figure 1 A schematic diagram of the structure of the welding equipment used in the welding method;
[0062] Figure 3 for Figure 2 A schematic top view of a welding device in FIG.
[0063] Figure 4 for Figure 3 A schematic cross-sectional view of the welding equipment along the AA direction;
[0064] Figure 5 for Figure 2 A schematic diagram of the structure of the peripheral pressing block of the welding equipment;
[0065] Figure 6 A schematic diagram of the structure of a pole and an intermediate pressing block provided in another embodiment of the present application;
[0066] Figure 7 A schematic diagram of the structure of a pole and an intermediate pressing block provided in yet another embodiment of the present application;
[0067] Figure 8 A schematic structural diagram of a multi-layer current collector welding device provided in another embodiment of the present application;
[0068] Fig. 9 for Figure 8 A schematic top view of a welding device in FIG.
[0069] Fig.10 for Fig. 9 A schematic cross-sectional view of the welding equipment along the BB direction;
[0070] Fig.11 for Fig. 9 A schematic diagram of the structure of the peripheral pressing block in FIG.
[0071] Fig.12 This is a structural exploded view of a peripheral pressing block provided in another embodiment of the present application.
[0072] Reference numerals:
[0073] Welding equipment: 100, 300; welding table: 110, 310; middle pressing block: 120, 320; peripheral pressing block: 130, 330; battery cell: 20; multi-layer current collector: 21; pole: 22; hollow area: 131, 331; body: 132, 332; fixing member: 133, 333, 433; movable member: 134; elastic member: 135; first end: 1331; second end: 1332; first slot: 1333; second slot: 1334; first surface: 221 ; Second surface: 121; First plane: 2211; Second plane: 2212; Third plane: 1211; Fourth plane: 1212; Roller: 321; Traction rod: 322; Moving track: 3331; Accommodating portion: 3332; First pressure rod: 3341; Second pressure rod: 3342; Third pressure rod: 3343, 4343; Fourth pressure rod: 3344, 4344; First elastic member: 3345; Second elastic member: 3346; First magnetic member: 470; Second magnetic member: 460. DETAILED DESCRIPTION
[0074] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0075] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0076] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values of the parts and steps set forth in these embodiments do not limit the scope of the application. Meanwhile, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to actual proportional relationships. The technology, methods and equipment known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, and therefore, once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.
[0077] Please also see Figure 1 and Figure 4 One of the embodiments of the present application provides a method for welding a multilayer current collector. The method for welding a multilayer current collector is used to weld the multilayer current collector 21 of the battery cell 20 and the pole 22 together by laser penetration welding. In this embodiment, the method for welding a multilayer current collector is performed on a multilayer current collector welding device 100, and the multilayer current collector welding device 100 includes a welding table 110, an intermediate pressing block 120, a peripheral pressing block 130 and a laser welding head (not shown). The method for welding a multilayer current collector includes the following steps:
[0078] The pole 22 is placed on the welding table 110 .
[0079] The battery cell 20 is placed close to the welding platform 110 , and the multi-layer current collector 21 of the battery cell 20 is placed in contact with the pole 22 .
[0080] The intermediate pressing block 120 is used to press the multi-layer current collector 21 and the position to be welded of the pole 22 .
[0081] The peripheral pressing block 130 is used to press the multi-layer current collector 21 and the surroundings of the to-be-welded portion of the pole 22. The peripheral pressing block 130 has a hollow area 131 inside. The intermediate pressing block 120 is located in the hollow area 131.
[0082] The middle pressing block 120 is removed to expose the hollow area 131 of the peripheral pressing block 130 .
[0083] The laser welding head is moved to the upper part of the part to be welded. The laser emitted by the laser welding head passes through the hollow area 131 of the peripheral pressing block 130 to weld the multi-layer current collector 21 and the part to be welded of the pole 22 .
[0084] In the welding method of the multilayer current collector provided in the above embodiment, the gap between the multilayer current collector 21 and the pole 22 can be effectively reduced by first using the intermediate pressing block 120 to press the multilayer current collector 21 and the part to be welded of the pole 22, and then using the peripheral pressing block 130 to press the multilayer current collector 21 and the parts to be welded of the pole 22 around, and then removing the intermediate pressing block 120 to reveal the hollow area 131 of the peripheral pressing block 130, thereby ensuring the reliability of laser welding. In fact, in the above welding method, even if there is a gap between the multilayer current collector 21 and the pole 22 due to the upward warping of the multilayer current collector 21, the gap can be effectively removed due to the pressing effect of the intermediate pressing block 120. Then, the peripheral pressing block 130 is used to press the periphery of the welding area while maintaining the intermediate pressing block 120. At this time, if the middle pressing block is removed, the close fit between the multilayer current collector 21 and the pole 22 can be effectively maintained due to the compression of the peripheral pressing block 130, so as to prevent the multilayer current collector 21 from returning to the state of upward warping due to the internal stress. At the same time, after removing the middle pressing block 120, the hollow area 131 of the peripheral pressing block 130 exposed is convenient for the laser welding head to perform laser penetration welding. During the laser penetration welding process, due to the close fit between the multilayer current collector 21 and the pole 22, the laser will not be reflected multiple times on the surface of the upper and lower layers of the materials to be welded, but will be absorbed by the welding material to the greatest extent, thereby ensuring that there is enough fusion area between the multilayer current collector 21 and the pole 22, thereby ensuring the reliability of laser penetration welding.
[0085] In the present embodiment, the intermediate pressing block 120 is a columnar structure. The shape of the intermediate pressing block 120 corresponds to the shape of the hollow area 131 of the peripheral pressing block 130, so that after the intermediate pressing block 120 is pressed, the peripheral pressing block 130 can also be effectively pressed, and the intermediate pressing block 120 and the peripheral pressing block 130 will not interfere with each other. In the present embodiment, the upper surface of the pole 22, that is, the surface to be welded is a plane. The lower surface of the intermediate pressing block 120, that is, the pressing surface is also a plane. When the intermediate pressing block 120 is pressed down, due to the matching relationship between the lower surface of the intermediate pressing block 120 and the upper surface of the pole 22, the multilayer current collector 21 can be tightly attached to the upper surface of the pole 22.
[0086] It is understandable that the surface to be welded of the pole and the pressing surface of the intermediate pressing block are not limited to the above embodiments. Figure 6 In one embodiment, the intermediate pressing block 120 is a columnar structure.
[0087] The pole 22 has a first surface 221 that is in contact with the multi-layer current collector. The first surface 221 is protruding toward the multi-layer current collector.
[0088] The intermediate pressing block 120 has a second surface 121 for pressing the portion to be welded. The second surface 121 is concavely arranged in a direction away from the multi-layer current collector. The shapes of the second surface 121 and the first surface 221 match each other, so that when the intermediate pressing block 120 is used to press the portion to be welded, the multi-layer current collector and the portion to be welded of the pole 22 are closely fitted.
[0089] In this embodiment, since the first surface 221 of the pole 22 is protruding toward the multilayer current collector, even if the multilayer current collector is warped upward, the protruding shape of the first surface 221 of the pole 22 can effectively reduce the gap between the pole 22 and the multilayer current collector. At this time, the intermediate pressing block 120 is used to press the part to be welded. Since the shape of the second surface 121 of the intermediate pressing block 120 matches the first surface 221 of the pole 22, during the pressing process, the multilayer current collector and the part to be welded of the pole 22 can fit tightly, thereby ensuring the reliability of laser penetration welding. In this embodiment, the first surface 221 is an arc-shaped protruding surface. The second surface 121 is an arc-shaped concave surface.
[0090] It can be understood that the first surface of the pole and the second surface of the intermediate pressing block are not limited to the arc shape. Figure 7In one embodiment, the first surface 221 is composed of a first plane 2211 and a second plane 2212. The first plane 2211 and the second plane 2212 together form a convex shape, so that the height of the center position of the first surface 221 is greater than the height of the two end positions of the first surface 221. The second surface 121 is composed of a third plane 1211 and a fourth plane 1212. The third plane 1211 and the fourth plane 1212 together form a concave shape, so that the height of the center position of the second surface 121 is greater than the height of the two end positions of the second surface 121. At this time, when the intermediate pressing block 120 is pressed to the to-be-welded position between the multilayer current collector 21 and the pole 22, the matching relationship between the second surface 121 of the intermediate pressing block 120 and the first surface 221 of the pole 22 can make the multilayer current collector and the pole 22 fit more closely at the to-be-welded position to ensure the reliability of the subsequent laser penetration welding process.
[0091] In this embodiment, by means of a double-plane combination, the first surface of the pole 22 can effectively achieve a state of protruding toward the multi-layer current collector. At this time, a certain height difference is formed between the center position and the two sides of the pole 22, thereby reducing the gap between the multi-layer current collector and the pole 22, thereby ensuring the reliability of subsequent laser penetration welding.
[0092] Please also see Figure 5 In one embodiment, the peripheral pressing block 130 includes a main body 132 , a fixing part 133 and a movable part 134 .
[0093] The hollow area 131 is disposed inside the body 132 .
[0094] The fixing member 133 is disposed on the bottom surface of the body 132 and surrounds the hollow area 131 .
[0095] The movable member 134 is disposed on the fixed member 133 and connected to the fixed member 133 via an elastic member 135 .
[0096] When the peripheral pressing block 130 presses the multi-layer current collector 21 and the electrode 22 around the parts to be welded, the movable member 134 is pressed around the parts to be welded, and the elastic member 135 is in a compressed state and provides a pressing force for the movable member 134 .
[0097] In this embodiment, the peripheral pressing block 130 includes a fixing member 133 and a movable member 134. The movable member 134 and the fixing member 133 are connected by an elastic member 135. When the peripheral pressing block 130 presses the multi-layer current collector 21 and the surroundings of the part to be welded of the pole 22, the movable member 134 is pressed around the part to be welded, and the elastic member 135 is in a compressed state and provides a pressing force for the movable member 134. That is, the pressing force of the movable member 134 on the periphery of the part to be welded is provided by the elastic member 135 in a compressed state, thereby ensuring that the peripheral pressing block 130 has a suitable pressing force on the periphery of the part to be welded. The multi-layer current collector 21 will not be damaged due to excessive pressing force, nor will the multi-layer current collector 21 be restored to an upward warping state due to the effect of internal stress due to too small pressing force, thereby ensuring the reliability of the subsequent laser penetration welding process.
[0098] In this embodiment, the fixing member 133 has a first end 1331 and a second end 1332. The first end 1331 is provided with a first slot 1333, and the second end 1332 is provided with a second slot 1334. The two ends of the movable member 134 are respectively provided on the first slot 1333 and the second slot 1334, so as to achieve the fixing effect between the movable member 134 and the fixing member 133. In addition, the first slot 1333 and the second slot 1334 are extended from top to bottom, so that the end of the movable member 134 can move up and down along the first slot 1333 and the second slot 1334. In this embodiment, the elastic member 135 is a spring. In the process of pressing down the peripheral pressing block 130, the movable member 134 first contacts the surface of the multilayer current collector 21. When the peripheral pressing block 130 continues to press down, since the stroke of the movable member 134 has been limited, the fixing member 133 will continue to move downward, thereby compressing the elastic member 135. At this time, the elastic member 135 is in a compressed state and provides a pressing force for the movable member 134. When the peripheral pressing block 130 continues to press down until the fixing member 133 also contacts the surface of the multi-layer current collector 21, the peripheral pressing block 130 stops pressing down, thereby completing the pressing process of the peripheral pressing block 130.
[0099] It is understandable that the shape of the intermediate pressing block is not limited to the above embodiments. Figures 8 to 11 In another embodiment of the present application, the multi-layer current collector welding method is performed on a multi-layer current collector welding device 300, and the multi-layer current collector welding device 300 includes a welding table 310, an intermediate pressing block 320, a peripheral pressing block 330 and a laser welding head (not shown).
[0100] The welding method of the multi-layer current collector comprises the following steps:
[0101] The pole 22 is placed on the welding table 310 .
[0102] The battery cell 20 is placed close to the welding platform 310 , and the multi-layer current collector 21 of the battery cell 20 is placed in contact with the pole 22 .
[0103] The intermediate pressing block 320 is used to press the multi-layer current collector 21 and the position to be welded of the pole 22 .
[0104] The peripheral pressing block 330 is used to press the multi-layer current collector 21 and the surroundings of the to-be-welded portion of the pole 22. The peripheral pressing block 330 has a hollow area 331 inside. The middle pressing block 320 is located in the hollow area 331.
[0105] The middle pressing block 320 is removed to expose the hollow area 331 of the peripheral pressing block 330 .
[0106] The laser welding head is moved to the upper part of the part to be welded. The laser emitted by the laser welding head passes through the hollow area 331 of the peripheral pressing block 330 to weld the multi-layer current collector 21 and the part to be welded of the pole 22 .
[0107] Different from the previous embodiment, in this embodiment, the intermediate pressing block 320 is a roller structure. The roller structure can move along the hollow area 331 of the peripheral pressing block 330, so as to achieve the pressing of the welding part. At this time, during the pressing process:
[0108] The roller structure rolls along the length direction of the hollow area 331 , so as to tightly press the multi-layer current collector 21 and the to-be-welded portion of the pole 22 .
[0109] Then, the peripheral pressing block 330 is used to press the multi-layer current collector 21 and the electrode 22 around the parts to be welded, and the roller structure is hidden.
[0110] In this embodiment, the roller structure is first used to roll along the length direction of the hollow area 331, so that the multilayer current collector 21 and the part to be welded of the pole 22 are tightly pressed together. Then, the peripheral pressing block 330 is used to press the multilayer current collector 21 and the part to be welded of the pole 22 around, so that the gap between the multilayer current collector 21 and the pole 22 can be effectively reduced, thereby ensuring the reliability of laser welding. In addition, due to the small size of the roller structure, the roller structure is hidden in the peripheral pressing block 330, so that the subsequent removal of the intermediate pressing block 320 can be realized. The above implementation method ensures the reliability of the subsequent laser penetration welding process. At the same time, it also ensures the convenience of the laser penetration welding process.
[0111] In this embodiment, the roller structure includes a roller 321 and a traction rod 322. The traction rod 322 is used to drive the roller 321 to move in the hollow area 331 of the peripheral pressing block 330. Specifically, the peripheral pressing block 330 includes a body 332 and a fixing member 333. The hollow area 331 is arranged inside the body 332. The fixing member 333 is arranged on the bottom surface of the body 332 and surrounds the hollow area 331. The fixing member 333 is provided with a moving track 3331 arranged along the length direction of the hollow area 331, so that the roller structure is rolled along the moving track 3331. In this embodiment, the two ends of the roller 321 are respectively arranged in two moving tracks 3331 of the fixing member 333 arranged along the length direction of the hollow area 331, so that the roller 321 can move in the hollow area 331 of the peripheral pressing block 330.
[0112] Please also see Fig.11 In this embodiment, the peripheral pressing block 330 includes a first pressing rod 3341, a second pressing rod 3342, a third pressing rod 3343 and a fourth pressing rod 3344. The first pressing rod 3341, the second pressing rod 3342, the third pressing rod 3343 and the fourth pressing rod 3344 are arranged together around the hollow area 331. The first pressing rod 3341 and the second pressing rod 3342 are respectively arranged close to the two short sides of the hollow area 331. The third pressing rod 3343 and the fourth pressing rod 3344 are respectively arranged close to the two long sides of the hollow area 331. During the pressing process:
[0113] First, press the first pressing rod 3341 onto one of the short sides of the part to be welded.
[0114] Then, the roller structure is rolled along the length direction of the hollow area 331 , and the rolling direction is from a position close to the first pressing rod 3341 to a position close to the second pressing rod 3342 .
[0115] Then, the second pressing rod 3342 is pressed onto the other short side of the part to be welded.
[0116] Then, the third pressing rod 3343 and the fourth pressing rod 3344 are pressed onto the two long sides of the part to be welded respectively, and the roller structure is hidden.
[0117] In this embodiment, through the pre-pressing of the first pressure rod 3341, when the roller structure rolls along the length direction of the hollow area 331, the position of the multilayer current collector 21 will not move at will, thereby ensuring that this process can effectively reduce the gap between the multilayer current collector 21 and the pole 22. When the roller structure rolls to a position close to the second pressure rod 3342, the second pressure rod 3342 is pressed again. At this time, since the first pressure rod 3341 and the second pressure rod 3342 are respectively arranged at both ends of the hollow area 331, it can effectively keep the multilayer current collector 21 and the pole 22 in a tightly fitted state. Finally, the third pressure rod 3343 and the fourth pressure rod 3344 are respectively pressed on the two long sides of the part to be welded to achieve the final pressing. In this embodiment, the position of the fixing member 333 close to the second pressure rod 3342 is provided with a receiving portion 3332. The accommodating portion 3332 is disposed beside the hollow area 331 for accommodating the roller 321. When the roller 321 moves to the accommodating portion 3332, the hollow area 331 is just exposed to prevent the roller 321 from blocking the laser during subsequent laser penetration welding.
[0118] In one embodiment, the first pressure rod 3341, the second pressure rod 3342, the third pressure rod 3343 and the fourth pressure rod 3344 are disposed on the fixing member 333 and protrude from the fixing member 333. A first elastic member 3345 is disposed between the first pressure rod 3341 and the fixing member 333. A second elastic member 3346 is disposed between the second pressure rod 3342 and the fixing member 333.
[0119] In the unpressed state, the length of the first pressing rod 3341 extending out of the fixing member 333 is greater than the length of the second pressing rod 3342 extending out of the fixing member 333 .
[0120] In this embodiment, by providing a first elastic member 3345 between the first pressing rod 3341 and the fixing member 333, and providing a second elastic member 3346 between the second pressing rod 3342 and the fixing member 333, in the case of no pressing, the length of the first pressing rod 3341 extending out of the fixing member 333 is greater than the length of the second pressing rod 3342 extending out of the fixing member 333. At this time, during the process of pressing down the peripheral pressing block 330, it can be ensured that the first pressing rod 3341 first contacts the periphery of the area to be welded, thereby achieving a pre-pressing action. After the rolling process of the roller structure along the length direction of the hollow area 331 is completed, the peripheral pressing block 330 is continued to be pressed downward, that is, the second pressing rod 3342 can also contact the periphery of the area to be welded, thereby achieving the pressing function.
[0121] In this embodiment, a third elastic member (not shown) is disposed between the third pressing rod 3343 and the fixing member 333. A fourth elastic member (not shown) is disposed between the fourth pressing rod 3344 and the fixing member 333.
[0122] In the unpressed state, the length of the second pressing rod 3342 extending out of the fixing member 333 is greater than the length of the third pressing rod 3343 or the fourth pressing rod 3344 extending out of the fixing member 333 .
[0123] In this embodiment, a third elastic member is provided between the third pressing rod 3343 and the fixing member 333, and a fourth elastic member is provided between the fourth pressing rod 3344 and the fixing member 333. In the case of no pressing, the length of the second pressing rod 3342 extending out of the fixing member 333 is greater than the length of the third pressing rod 3343 or the fourth pressing rod 3344 extending out of the fixing member 333. At this time, when the second pressing rod 3342 is also pressed on the periphery of the area to be welded, the peripheral pressing block 330 is continuously pressed downward, so that the third pressing rod 3343 and the fourth pressing rod 3344 are respectively pressed on the two long sides of the area to be welded. That is, through the above setting, it can be realized that in the process of pressing the peripheral pressing block 330 downward, the first pressing rod 3341 is pre-pressed first, the second pressing rod 3342 is pressed, and then the third pressing rod 3343 and the fourth pressing rod 3344 are pressed. The above operation method is simple and convenient, and is easy to operate during the welding process.
[0124] It is understandable that the shapes and arrangements of the first pressure bar, the second pressure bar, the third pressure bar and the fourth pressure bar are not limited to the above embodiments. Fig.12 In one embodiment, the third pressure rod 4343 and the fourth pressure rod 4344 are integrally arranged.
[0125] The fixing member 433 is provided with a first magnetic member 470 .
[0126] The third pressing rod 4343 and the fourth pressing rod 4344 are provided with a second magnetic member 460 .
[0127] The first magnetic member 470 and / or the second magnetic member 460 are electromagnetic induction elements. In the case of no pressing, power is applied to make the first magnetic member 470 and the second magnetic member 460 attract each other, so that the length of the third pressure rod 4343 and the fourth pressure rod 4344 extending out of the fixing member 433 is less than the length of the second pressure rod extending out of the fixing member 433. In the case of pressing, reverse power is applied to repel the first magnetic member 470 and the second magnetic member 460, so that the third pressure rod 4343 and the fourth pressure rod 4344 are pressed in the peripheral area of the to-be-welded portion of the multilayer current collector 21 and the pole 22.
[0128] In this embodiment, by providing the first magnetic member 470 on the fixing member 433, and providing the second magnetic member 460 on the third pressure rod 4343 and the fourth pressure rod 4344, when not pressed together, power is turned on to make the first magnetic member 470 and the second magnetic member 460 attract each other, so that the length of the third pressure rod 4343 and the fourth pressure rod 4344 extending out of the fixing member 433 is less than the length of the second pressure rod extending out of the fixing member 433. By providing the first magnetic member 470 and the second magnetic member 460, it is also possible to achieve the process of first pre-pressing the first pressure rod, then pressing the second pressure rod, and then pressing the third pressure rod 4343 and the fourth pressure rod 4344 in the process of pressing the peripheral pressure block 430 downward.
[0129] Another embodiment of the present application further provides a multi-layer current collector welding device 100, including a welding table 110, a battery cell placement platform (not shown), an intermediate pressing block 120, a peripheral pressing block 130 and a laser welding head (not shown).
[0130] The welding table 110 is used to place the pole 22 .
[0131] The battery cell placement platform is used to place the battery cell 20 and to fit the multi-layer current collector 21 of the battery cell 20 with the pole 22 .
[0132] The intermediate pressing block 120 is used to press the multi-layer current collector 21 and the position to be welded of the pole 22 , and is removed after the peripheral pressing block 130 is pressed to expose the hollow area 131 of the peripheral pressing block 130 .
[0133] The peripheral pressing block 130 is used to press the multi-layer current collector 21 and the surroundings of the to-be-welded portion of the pole 22 after the intermediate pressing block 120 presses the to-be-welded portion. The peripheral pressing block 130 has the hollow region 131 inside. The intermediate pressing block 120 is located in the hollow region 131.
[0134] The laser welding head is located above the portion to be welded, and the laser emitted by the laser welding head passes through the hollow area 131 of the peripheral pressing block 130 to weld the portion to be welded between the multi-layer current collector 21 and the pole 22 .
[0135] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used herein to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" may include both "above" and "below". The device may also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used herein are interpreted accordingly.
[0136] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of this application.
[0137] The above are only preferred embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A welding method for a multi-layer current collector, characterized in that: The following steps are involved: Place the pole on the welding table; The battery cell is arranged close to the welding station, and the multi-layer current collector of the battery cell is arranged in contact with the pole; The multi-layer current collector is pressed onto the part of the pole to be welded by using an intermediate pressing block; the multi-layer current collector is pressed onto the parts of the pole to be welded by using a peripheral pressing block, wherein the peripheral pressing block has a hollow area inside, and the intermediate pressing block is located in the hollow area; Removing the middle pressing block to expose the hollow area of the peripheral pressing block; The laser welding head is moved above the portion to be welded, and the laser emitted by the laser welding head passes through the hollow area of the peripheral pressing block to weld the multi-layer current collector and the portion to be welded of the pole.
2. The welding method of multi-layer current collector according to claim 1, characterized in that: The intermediate pressing block is a columnar structure; The pole has a first surface that is in contact with the multi-layer current collector, and the first surface is protruded toward the multi-layer current collector; The intermediate pressing block has a second surface for pressing the portion to be welded, the second surface is recessed in a direction away from the multilayer current collector, and the shapes of the second surface and the first surface match so that when the intermediate pressing block is used to press the portion to be welded, the multilayer current collector and the portion to be welded of the pole are tightly fitted.
3. The welding method of multi-layer current collector according to claim 2, characterized in that: The first surface is an arc-shaped convex surface, and the second surface is an arc-shaped concave surface; Alternatively, the first surface is composed of a first plane and a second plane, and the first plane and the second plane together form a convex shape, so that the height of the center position of the first surface is greater than the height of the two end positions of the first surface; the second surface is composed of a third plane and a fourth plane, and the third plane and the fourth plane together form a concave shape, so that the height of the center position of the second surface is greater than the height of the two end positions of the second surface.
4. The welding method of multi-layer current collector according to claim 2, characterized in that: The peripheral pressing block comprises: A body, wherein the hollow area is arranged inside the body; A fixing member is arranged on the bottom surface of the main body and surrounds the hollow area; and A movable part, arranged on the fixed part and connected to the fixed part through an elastic part; When the peripheral pressing block presses the multi-layer current collector and the surroundings of the to-be-welded portion of the pole, the movable member is pressed around the to-be-welded portion, and the elastic member is in a compressed state and provides a pressing force for the movable member.
5. The welding method of multi-layer current collector according to claim 1, characterized in that: The intermediate pressing block is a roller structure. During the pressing process: The roller structure rolls along the length direction of the hollow area, so as to tightly press the multi-layer current collector and the to-be-welded portion of the pole; Then, the peripheral pressing block is used to press the multi-layer current collector and the surroundings of the to-be-welded portion of the pole, and the roller structure is hidden.
6. The welding method of multi-layer current collector according to claim 1, characterized in that: The intermediate pressing block is a roller structure; The peripheral pressing block includes a first pressing rod, a second pressing rod, a third pressing rod and a fourth pressing rod, which are arranged together around the hollow area, and the first pressing rod and the second pressing rod are respectively arranged close to two short sides of the hollow area, and the third pressing rod and the fourth pressing rod are respectively arranged close to two long sides of the hollow area; during the pressing process: Firstly, press the first pressing rod onto one of the short sides of the part to be welded; Then, the roller structure is rolled along the length direction of the hollow area, and the rolling direction is from a position close to the first pressure rod to a position close to the second pressure rod; Then, the second pressing rod is pressed onto the other short side of the part to be welded; Then, the third pressing rod and the fourth pressing rod are pressed onto two long sides of the part to be welded respectively, and the roller structure is hidden.
7. The welding method of multi-layer current collector according to claim 6, characterized in that: The peripheral pressing block also includes: A body, wherein the hollow area is arranged inside the body; A fixing member is arranged on the bottom surface of the body and surrounds the hollow area, and a moving track is arranged along the length direction of the hollow area on the fixing member, so that the roller structure is rolled along the moving track; The first pressure rod, the second pressure rod, the third pressure rod and the fourth pressure rod are arranged on the fixing member and protrude from the fixing member, a first elastic member is arranged between the first pressure rod and the fixing member, and a second elastic member is arranged between the second pressure rod and the fixing member; In the unpressed state, the length of the first pressing rod extending out of the fixing member is greater than the length of the second pressing rod extending out of the fixing member.
8. The welding method of multi-layer current collector according to claim 7, characterized in that: A third elastic member is provided between the third pressure rod and the fixing member, and a fourth elastic member is provided between the fourth pressure rod and the fixing member; In the unpressed state, the length of the second pressing rod extending out of the fixing member is greater than the length of the third pressing rod or the fourth pressing rod extending out of the fixing member.
9. The welding method of multi-layer current collector according to claim 7, characterized in that: The third pressure rod and the fourth pressure rod are integrally arranged; The fixing member is provided with a first magnetic member; The third pressure rod and the fourth pressure rod are provided with a second magnetic member; The first magnetic member and / or the second magnetic member are electromagnetic induction elements. When not pressed together, power is applied to attract the first magnetic member and the second magnetic member, so that the length of the third pressure rod and the fourth pressure rod extending out of the fixing member is less than the length of the second pressure rod extending out of the fixing member. When pressed together, reverse power is applied to repel the first magnetic member and the second magnetic member, so that the third pressure rod and the fourth pressure rod are pressed together in the peripheral area of the multi-layer current collector and the pole at the part to be welded.
10. A welding device for a multi-layer current collector, characterized in that: Including welding table, battery cell placement platform, middle pressing block, peripheral pressing block and laser welding head: The welding table is used to place the pole; The battery cell placement platform is used to place the battery cells and to fit the multi-layer current collectors of the battery cells with the poles; The intermediate pressing block is used to press the multi-layer current collector and the to-be-welded portion of the pole, and is removed after the peripheral pressing blocks are pressed to reveal the hollowed-out area of the peripheral pressing blocks; The peripheral pressing block is used to press the multi-layer current collector and the surroundings of the to-be-welded portion of the pole after the intermediate pressing block presses the to-be-welded portion, and the peripheral pressing block has the hollow area inside, and the intermediate pressing block is located in the hollow area; The laser welding head is located above the portion to be welded, and the laser emitted by the laser welding head passes through the hollow area of the peripheral pressing block to weld the multi-layer current collector and the portion to be welded of the pole.