Preparation method of ferromanganese phosphate precursor, positive electrode sheet and lithium battery

By using a sprayer and a particle size regulator in a high-temperature roasting device to form a precursor of ferromanganese phosphate of various particle sizes, the problem of insufficient particle size range in the prior art is solved, and high-pressure density manganese phosphate is achieved Lithium cathode material improves the electrochemical performance and energy density of lithium batteries.

CN118754088BActive Publication Date: 2024-11-26HUNAN YUNENG NEW ENERGY BATTERY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411237937.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-26
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The particle size D50 of the existing ferromanganese phosphate precursor prepared based on high-temperature roasting devices is within a particle size range, which cannot meet the theoretical compaction density of 3.6g/cm3 of lithium manganese phosphate positive electrode material.

Method used

Using an improved high-temperature roasting device, including a sprayer and a particle size regulator, the powdered ferromanganese phosphate precursor with at least 2 preset particle sizes is formed by spray roasting, and the sprayed droplets are moved in reverse direction by using the particle size regulator. Control the particle size and shape to form a graded bulk density, thereby improving compaction density.

Benefits of technology

The high-pressure density lithium manganese iron phosphate positive electrode material has been achieved, which improves the electrochemical performance and energy density, and improves the circulation performance of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754088B_ABST
    Figure CN118754088B_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of lithium batteries, and in particular, relates to a method for preparing a ferromanganese phosphate precursor, a positive electrode sheet and a lithium battery, the method comprising: preparing a precursor based on a high-temperature roasting device, the high-temperature roasting device comprising a vertical high-temperature roasting furnace, the high-temperature roasting furnace comprising a sprayer, a heater and a particle size regulator; the method comprising: a manganese source and hydrochloric acid generate a manganese-containing solution; an iron source, a phosphorus source and hydrochloric acid generate a ferrophosphorus solution; the manganese-containing solution, the ferrophosphorus solution and a dispersant are mixed to obtain a mixed solution; the mixed solution is preheated; the mixed solution is sent to a high-temperature roasting furnace; the high-temperature roasting furnace sprays and roasts the mixed solution in a carrier gas atmosphere, and forms at least two powdered ferromanganese phosphate precursors with preset particle sizes through the sprayer and the particle size regulator; the ferromanganese phosphate precursor is washed, ground, demagnetized and dried to obtain the ferromanganese phosphate precursor; the particle size of the ferromanganese phosphate precursor can be controlled by adjusting the suspension time of the droplets in the heating zone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of lithium batteries, and in particular relates to a method for preparing a ferromanganese phosphate precursor, a positive electrode sheet and a lithium battery. Background Art

[0002] At present, the primary particle size D50 of the ferromanganese phosphate precursor prepared by high-temperature calcination equipment is within a particle size range. However, the lithium ferromanganese phosphate positive electrode material prepared by the precursor within a particle size range cannot meet the needs of the scene, which is far from the 3.6g / cm 3 There is still a gap in the theoretical compaction density.

[0003] The existing technology has the problem that the high-temperature calcination device and preparation method of ferromanganese phosphate precursor cannot meet the demand. Summary of the invention

[0004] The embodiments of the present application provide a method for preparing a ferromanganese phosphate precursor, a positive electrode plate and a lithium battery, aiming to solve the problem that the high-temperature roasting device and preparation method of the ferromanganese phosphate precursor cannot meet the demand to a certain extent.

[0005] In the first aspect, an embodiment of the present application provides a method for preparing a ferromanganese phosphate precursor, wherein the ferromanganese phosphate precursor is prepared based on a high-temperature calcination device, wherein the high-temperature calcination device includes a first dissolution tank, a second dissolution tank, a mixing tank, a venturi processor, a pump, a valve, and a vertical high-temperature calcination furnace, wherein the high-temperature calcination furnace includes a sprayer arranged at the top, at least one group of heaters, and at least one particle size regulator, wherein the heaters are arranged at the middle and bottom of the outer surface of the high-temperature calcination furnace, and the particle size regulator is arranged inside the high-temperature calcination furnace corresponding to the position of the heaters. The device makes the sprayed droplets move in reverse to adjust the suspension time of the droplets to control the particle size of the ferromanganese phosphate precursor, the outlet of the first dissolving tank and the outlet of the second dissolving tank are connected to the first inlet of the mixing tank, the outlet at the bottom of the mixing tank is connected to the first inlet of the side wall of the venturi processor, the outlet at the bottom of the venturi processor is connected to the inlet of the pump, the outlet of the pump is respectively connected to the inlet at the top of the high-temperature roasting furnace and the second inlet of the side wall of the venturi processor, and the first outlet near the top of the high-temperature roasting furnace is connected to the third inlet at the top of the venturi processor;

[0006] The preparation method comprises:

[0007] S11, reacting a manganese source and hydrochloric acid in the first dissolution tank to generate a manganese-containing solution;

[0008] S12, reacting an iron source, a phosphorus source and hydrochloric acid in the second dissolution tank to generate a ferrophosphorus solution;

[0009] S2, uniformly mixing the manganese-containing solution, the ferrophosphorus solution and the dispersant in the mixing tank to obtain a mixed solution;

[0010] S3, sending the mixed solution in the mixing tank to the venturi processor for preheating through the pump;

[0011] S4, sending the preheated and concentrated mixed solution to the inlet of the high-temperature roasting furnace through the pump;

[0012] S5, the high temperature calcining furnace sprays and calcines the mixed solution in the atmosphere of the carrier gas, and forms at least two kinds of powdered manganese ferrophosphate precursors with preset particle sizes through the sprayer and the particle size regulator;

[0013] S6, washing, grinding, demagnetizing and drying the at least two kinds of ferromanganese phosphate precursors with preset particle sizes, respectively, to obtain at least two kinds of ferromanganese phosphate precursors with preset particle sizes.

[0014] The method for preparing a ferromanganese phosphate precursor based on a high-temperature calcination device provided in an embodiment of the present application, since the high-temperature calcination furnace includes a sprayer, a heater and a particle size regulator on the top, the heater is arranged at the middle and bottom of the outer surface of the high-temperature calcination furnace, and the particle size regulator is arranged inside the high-temperature calcination furnace corresponding to the position of the heater, the particle size regulator can make the droplets after spraying to move in the reverse direction to adjust the suspension time of the droplets in the heating zone to control the particle size of the ferromanganese phosphate precursor, and make the droplets after spraying in the heating zone interact with the downward spraying action and the upward reverse movement to form more uniform and closer to spherical particles, thereby forming at least two kinds of powdered ferromanganese phosphate precursors with preset particle sizes, and when the large-particle-size precursor and the small-particle-size precursor are mixed, the small-particle-size precursor can better fill the gaps between the large-particle-size precursors, so the large-particle-size precursor and the small-particle-size precursor form a graded packing density filling, thereby forming a lithium ferromanganese phosphate positive electrode material with a high compaction density.

[0015] In a second aspect, an embodiment of the present application provides a positive electrode plate, which is made of a positive electrode material prepared from a manganese ferrophosphate precursor as described in any one of the contents of the first aspect.

[0016] The positive electrode plate of the present application uses at least two kinds of manganese iron phosphate precursors with preset particle sizes to prepare a manganese iron phosphate lithium positive electrode material with a high compaction density, thereby improving the electrochemical performance of the positive electrode plate.

[0017] In a third aspect, an embodiment of the present application provides a lithium battery, characterized in that the lithium battery includes a positive electrode plate as described in the second aspect.

[0018] The lithium battery of the present application uses a positive electrode sheet made of lithium iron manganese phosphate obtained by the above-mentioned preparation method. Since the conductivity and compaction density of the lithium iron manganese phosphate positive electrode material are improved, the lithium battery has higher energy density and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0020] Figure 1 is a schematic structural diagram of a high-temperature roasting device provided in one embodiment of the present application;

[0021] Figure 2 It is a schematic flow chart of a method for preparing a ferromanganese phosphate precursor provided in one embodiment of the present application;

[0022] Figure 3 It is a top view schematic diagram showing that the jet holes of the spiral air pipe in the particle size regulator provided in one embodiment of the present application are distributed at intervals of preset angles;

[0023] Figure 4 This is a schematic structural diagram of staggered arrangement of jet holes in adjacent circles of a spiral air pipe provided by an embodiment of the present application;

[0024] Figure 5 This is a schematic diagram of a structure in which the jet holes of a spiral air pipe provided by an embodiment of the present application are distributed at preset angles and the diameters of the jet holes of each semicircle increase sequentially;

[0025] Figure 6 This is a schematic structural diagram of an embodiment of the present application in which the jet holes of adjacent circles of a spiral air pipe are staggered and the diameters of the jet holes of each semicircle increase sequentially;

[0026] Figure 7 This is a schematic diagram of a structure in which a nozzle is arranged in an air injection hole of a spiral air pipe provided in an embodiment of the present application;

[0027] Figure 8 It is a top view schematic diagram of a hollowed-out nozzle body provided by an embodiment of the present application;

[0028] Fig. 9 It is a schematic cross-sectional structure diagram of a nozzle in an air jet hole of a spiral air pipe provided by an embodiment of the present application when the nozzle does not perform air jetting;

[0029] Fig.10 It is a schematic cross-sectional structure diagram of a nozzle performing jetting in a jet hole of a spiral air pipe provided in an embodiment of the present application;

[0030] Fig.11 is a schematic structural diagram of a high temperature roasting device including three particle size regulators provided in another embodiment of the present application;

[0031] Reference numerals:

[0032] 1. First dissolving tank; 2. Second dissolving tank; 3. Mixing tank; 4. Venturi processor; 5. Pump; 6. Valve; 7. High-temperature roasting furnace; 71. Sprayer; 72. Heater; 73. Particle size regulator; 731. Spiral air pipe; 732. Air intake flow regulator; 733. Jet hole; 734. Nozzle; 7341. Guide sleeve; 7342. Nozzle body; 7343. One-way jet block. DETAILED DESCRIPTION

[0033] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0034] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0035] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, a~b (i.e. a and b), a~c, b~c, or a~b~c, where a, b, c can be single or multiple, respectively.

[0036] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. For example, without departing from the scope of the implementation regulations of this application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0037] The terms used in the embodiments of the present application are only for the purpose of describing specific implementation rules, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the implementation rules of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0038] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the implementation regulations of this application.

[0039] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0040] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0041] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0042] At present, the particle size D50 of the ferromanganese phosphate precursor prepared by the high-temperature roasting device is within a particle size range, but the lithium ferromanganese phosphate positive electrode material prepared by the precursor within a particle size range cannot meet the needs of the scene, and is far from the 3.6g / cm 3 There is still a gap in the theoretical compaction density.

[0043] like Figure 1As shown, the present application is based on a high temperature roasting device to prepare a ferromanganese phosphate precursor, the high temperature roasting device includes a first dissolving tank 1, a second dissolving tank 2, a mixing tank 3, a venturi processor 4, a pump 5, a valve 6 and a vertical high temperature roasting furnace 7, the high temperature roasting furnace 7 includes a sprayer 71 arranged at the top, at least one group of heaters 72 and at least one particle size regulator 73, the heater 72 is arranged at the middle and bottom of the outer surface of the high temperature roasting furnace 7, the particle size regulator 73 is arranged inside the high temperature roasting furnace 7 corresponding to the position of the heater 72, and the particle size regulator 73 is used The droplets after spraying move in reverse to adjust the suspension time of the droplets to control the particle size of the ferromanganese phosphate precursor. The outlet of the first dissolution tank 1 and the outlet of the second dissolution tank 2 are connected to the first inlet of the mixing tank 3, the outlet at the bottom of the mixing tank 3 is connected to the first inlet of the side wall of the venturi processor 4, the outlet at the bottom of the venturi processor 4 is connected to the inlet of the pump 5, the outlet of the pump 5 is respectively connected to the inlet at the top of the high-temperature roasting furnace 7 and the second inlet of the side wall of the venturi processor 4, and the first outlet near the top of the high-temperature roasting furnace 7 is connected to the third inlet at the top of the venturi processor 4.

[0044] like Figure 2 As shown, the first aspect of the embodiment of the present application provides a method for preparing a ferromanganese phosphate precursor, comprising:

[0045] S11, reacting a manganese source and hydrochloric acid in a first dissolution tank 1 to generate a manganese-containing solution.

[0046] S12, reacting the iron source, the phosphorus source and the hydrochloric acid in the second dissolving tank 2 to generate a ferrophosphorus solution.

[0047] S2, uniformly mixing the manganese-containing solution, the ferrophosphorus solution and the dispersant in a mixing tank 3 to obtain a mixed solution.

[0048] S3, the mixed solution in the mixing tank 3 is sent to the venturi processor 4 for preheating through the pump 5.

[0049] S4, the preheated and concentrated mixed solution is sent to the inlet of the high-temperature roasting furnace 7 through the pump 5.

[0050] S5, the high temperature calcining furnace 7 sprays and calcines the mixed solution in the atmosphere of the carrier gas, and forms at least two kinds of powdered manganese ferrophosphate precursors with preset particle sizes through the sprayer 71 and the particle size regulator 73.

[0051] S6, washing, grinding, demagnetizing and drying at least two kinds of ferromanganese phosphate precursors with preset particle sizes, respectively, to obtain at least two kinds of ferromanganese phosphate precursors with preset particle sizes.

[0052] In the method for preparing ferromanganese phosphate precursor based on a high-temperature roasting device provided in an embodiment of the present application, since the high-temperature roasting furnace 7 includes a sprayer 71, a heater 72 and a particle size regulator 73 at the top, the sprayer 71 at the top sprays droplets of atomized mixed solution downward, the heater 72 is arranged at the middle and bottom of the outer surface of the high-temperature roasting furnace 7, and the particle size regulator 73 is arranged inside the high-temperature roasting furnace 7 corresponding to the position of the heater 72. The particle size regulator 73 causes the sprayed droplets to move in the opposite direction relative to the landing direction of the sprayed droplets, that is, the particle size regulator 73 causes the sprayed droplets to move in the opposite direction toward the top of the high-temperature roasting furnace 7, thereby causing the droplets to interact with the spray atomization at the top downward and the reverse movement. On the one hand, it promotes the droplets to generate particles with more uniform particle size, more spherical shape and more thorough particle formation, and on the other hand, it controls the time for the droplets to move in the reverse direction to adjust the droplets in the heating The suspension time in the hot zone is used to control the particle size of the ferromanganese phosphate precursor. Since the particle size regulator 3 is located inside the high-temperature roasting furnace 7 corresponding to the position of the heater 72, the sprayed atomized droplets perform reverse motion in the heating area so that the heating and reverse motion can cooperate with each other. The longer the suspension time caused by the reverse motion, the longer the heating time, resulting in a greater reduction in the liquid component of the droplets and a smaller particle size of the generated particles. The shorter the suspension time caused by the reverse motion, the shorter the heating time, resulting in a less reduction in the liquid component of the droplets and a larger particle size of the generated particles, thereby forming at least two kinds of powdered ferromanganese phosphate precursors with preset particle sizes. When the large-particle-size precursor and the small-particle-size precursor are mixed, the small-particle-size precursor can better fill the gaps between the large-particle-size precursors, so the large-particle-size precursor and the small-particle-size precursor form a graded packing density filling, thereby forming a high-density lithium ferromanganese phosphate positive electrode material.

[0053] In one embodiment, the sprayer 71 includes an adjustable nozzle and a flow regulator (not shown). Figure 3As shown, the particle size regulator 73 includes a spiral air pipe 731 and an air intake flow regulator 732. The spiral air pipe 731 is provided with a plurality of jet holes 733 on one side close to the sprayer 71. The gas in the spiral air pipe 731 is a carrier gas. Step S5 includes: mixing the mixed solution with the carrier gas and setting the flow rate of the gas-liquid mixture through the flow regulator to a preset flow rate, and then adjusting the adjustable nozzle to a preset aperture to spray in a preset atomization mode; the droplets of the atomized mixed solution are sequentially evaporated, dried and calcined in a top-down direction, and the air intake flow rate of the carrier gas in the spiral air pipe 731 is adjusted by the air intake flow regulator 732 to form at least two kinds of powdered manganese ferrophosphate precursors with preset particle sizes. In this embodiment, the adjustable nozzle can adjust the aperture of the nozzle as required, thereby adjusting the diameter of the ejected droplets, and further adjusting the particle size of the ferromanganese phosphate precursor; the adjustable nozzle can also adjust the flow rate of the gas-liquid mixture of the mixed solution and the carrier gas through the flow regulator as required, thereby adjusting the pressure of the ejected droplets, and further adjusting the particle size of the ferromanganese phosphate precursor. In this embodiment, the plurality of jet holes 733 arranged on one side of the spiral air pipe 731 close to the sprayer 71 will eject the carrier gas according to the pressure of the inlet flow regulator 732, causing the droplets to move upward in the reverse direction under the action of the reverse jet, thereby adjusting the suspension time of the droplets ejected downward during the evaporation process, the drying process and the calcination process, and further adjusting the particle size of the ferromanganese phosphate precursor. It can be understood that the shorter the suspension time of the atomized droplets sprayed from the sprayer 71 during the evaporation treatment, drying treatment and calcination treatment, the less the solvent evaporation and pyrolysis of the atomized droplets will be, which reduces the drying and solidification effects of the atomized droplets, and thus the particle size of the ferromanganese phosphate precursor will be relatively large; and the longer the suspension time of the atomized droplets sprayed from the sprayer 71 during the evaporation treatment, drying treatment and calcination treatment, the more the solvent evaporation and pyrolysis of the atomized droplets will be, which promotes the drying and solidification of the atomized droplets, and thus the particle size of the ferromanganese phosphate precursor will be relatively small.

[0054] In some embodiments, compared with the prior art that sprays in only one direction, causing the droplets to be affected by gravity during the descent process, the particles of the ferromanganese phosphate precursor cannot form a shape close to a sphere, and the range of controlling the suspension time of the droplets is relatively small; the spiral air pipe 731 is provided with a plurality of jet holes 733 on one side close to the sprayer 71, and the jet holes of the spiral air pipe 731 are distributed at preset angles in a clockwise or counterclockwise direction, such as Figure 3 As shown, or the jet holes of adjacent circles of the spiral air pipe 731 are staggered, as shown in FIG. Figure 4As shown; thereby, the jet of the spiral air pipe 731 forms a uniformly covered reverse power in the heating zone of the high-temperature roasting furnace 7, so that more spray droplets can perform uniform reverse suspension movement in the heating zone, thereby forming particles of ferromanganese phosphate precursor with more uniform particle size and a shape closer to a sphere, and can control the suspension time in a larger range, thereby forming particles of ferromanganese phosphate precursor within a preset particle size range.

[0055] In one embodiment, since the diameters of the jet holes 733 are the same, the distribution of the jet holes 733 is relatively sparse as the spiral air pipe 731 moves outward, causing the reverse force on the droplets in the local area to be not uniform. Figure 5 As shown, the particle size regulator 73 includes a spiral air pipe 731 and an air intake flow regulator 732. The spiral air pipe 731 is provided with a plurality of jet holes 733 on one side close to the sprayer 71. The diameters of the jet holes in each semicircle of the spiral air pipe 731 increase successively along the spiral air pipe 731 from the inside to the outside. Since the diameter is smaller in the dense area of ​​the inner circle and then increases successively, the jet holes in the outer circle have a larger range of jet influence due to the larger diameter, thereby compensating for the disadvantage that the reverse force received by the droplets in the local area is not uniform enough, so that a uniformly covered reverse force is formed in the heating zone of the high-temperature roasting furnace 7, so that more spray droplets can perform uniform reverse suspension movement in the heating zone, thereby forming particles of ferromanganese phosphate precursor with more uniform particle size and shape closer to a sphere, and being able to control a larger range of suspension time, thereby forming particles of ferromanganese phosphate precursor with a preset particle size range.

[0056] In some embodiments, a plurality of jet holes 733 are provided on one side of the spiral air tube 731 close to the sprayer 71. The jet holes of the spiral air tube 731 are distributed at preset angles in a clockwise or counterclockwise direction and extend from the inside to the outside along the spiral air tube 731. The diameters of the jet holes in each semicircle of the spiral air tube 731 increase successively. Figure 5 Alternatively, the jet holes of adjacent circles of the spiral air pipe 731 are staggered and extend from the inside to the outside along the spiral air pipe 731, as shown in FIG. Figure 6 As shown, the diameter of the jet hole in each semicircular spiral air pipe 731 increases successively; it can further form a more uniformly covered reverse power in the heating zone of the high-temperature roasting furnace 7, so that more spray droplets can perform uniform reverse suspension movement in the heating zone, thereby forming particles of ferromanganese phosphate precursor with more uniform particle size and closer to spherical shape, and can control a larger range of suspension time, thereby forming particles of ferromanganese phosphate precursor within a preset particle size range.

[0057] In one embodiment, since it is necessary to adjust the suspension time of the droplets after spraying, when the jet hole is not jetting outward, some particles of the ferromanganese phosphate precursor will fall into it, causing partial blockage of the jet hole, or the gas ejected from the jet hole can only generate the corresponding reverse power in the area near the jet hole diameter, reducing the reverse power range generated by the jet hole jetting outward; Figure 7 As shown, in any of the jet holes 733, a nozzle 734 is provided, and the nozzle 734 includes a guide sleeve 7341, a nozzle body 7342 and a one-way jet block 7343. The nozzle body 7342 is in the shape of an inverted truncated cone with an opening at the bottom, and its diameter gradually increases along the direction from the spiral air pipe 731 to the sprayer 71. The guide sleeve 7341 is an elastic set provided on the outside of the nozzle body 7342. The diameter of the bottom of the nozzle body 7342 away from the sprayer 71 is smaller than the diameter of the corresponding jet hole 733, and the diameter of the top of the nozzle body 7342 close to the sprayer 71 is larger than the diameter of the corresponding jet hole 733. The top of the nozzle body 7342 is a hollow surface, as shown in FIG. Figure 8 As shown; the one-way jet block 7343 is an inverted truncated cone corresponding to the nozzle body 7342, the ratio between the height of the nozzle body 7342 and the height of the one-way jet block 7343 is (3-1.2):1, the height of the nozzle body 7342 is smaller than the diameter of the spiral air pipe 731 and larger than the thickness of the spiral air pipe 731; the guide sleeve 7341 is used to fix the nozzle 734 in the jet hole 733 by interference fit, and prevent the carrier gas from being ejected from the gap between the guide sleeve 7341 and the jet hole 733; as shown Fig. 9 As shown, when the spiral air pipe 731 is not jetting, the one-way jet block 7343 slides into the bottom along the inverted truncated cone of the nozzle body 7342 under the action of gravity, thereby blocking the jet hole 733, thereby avoiding the blockage of the jet hole; as shown in FIG. Fig.10 As shown, when the spiral air pipe 731 is jetting through the jet hole 733, the carrier gas enters from the opening at the bottom of the nozzle body 7342 to blow the one-way jet block 7343 toward the top of the nozzle body 7342, and is ejected through the gap between the one-way jet block 7343 and the nozzle body 7342, providing a reverse power in the opposite direction of the droplet falling direction, and expanding the reverse power range of the jet through the inverted truncated cone shape. It can be understood that along the spiral air pipe 731 extending from the inside to the outside, the diameter of the top of the nozzle body 7342 close to the sprayer 71 can also be gradually increased, so as to form a more uniform reverse power coverage area.

[0058] In another embodiment, Fig.11As shown, the evaporation zone corresponding to the evaporation treatment, the drying zone corresponding to the drying treatment, and the roasting zone corresponding to the roasting treatment are all provided with at least one group of heaters 72 and at least one particle size regulator 73, and the heaters 72 are respectively provided on the outer surface of the high-temperature roasting furnace 7 corresponding to the evaporation zone, the drying zone, and the roasting zone, and at least one particle size regulator 73 is respectively provided in the evaporation zone, the drying zone, and the roasting zone, wherein the heater 72 is a microwave heater, a gas heater, or a microwave heater and a gas heater; thereby, the suspension time of the atomized droplets can be controlled in the evaporation zone, the drying zone, and the roasting zone, respectively, further improving the ability to control the suspension time of the atomized droplets in the high-temperature roasting furnace 7, and the atomized droplets can be completely processed in each zone to form various required particle sizes of ferromanganese phosphate precursors. For example, the evaporation zone is a microwave heater, the drying zone is a microwave heater, and the roasting zone is a gas heater; or the evaporation zone, the drying zone, and the roasting zone are all microwave heaters; or the evaporation zone, the drying zone, and the roasting zone are all gas heaters.

[0059] In some embodiments, the mixed gas of the gas and carrier gas generated by the evaporation treatment, drying treatment and roasting treatment enters the third inlet of the venturi processor 4 through the first outlet near the top of the high-temperature roasting furnace 7, and the mixed solution is preheated and concentrated by the self-circulation of the venturi processor 4 and the pump 5 and the mixed gas, and the preheating and concentration is to evaporate 25wt%~35wt% of the water in the mixed solution. In this embodiment, the manganese-containing solution, the ferrophosphorus solution and the dispersant are uniformly mixed in the mixing tank 3 to obtain a mixed solution, which is sent to the venturi processor 4 for preheating and concentration, which can reduce the viscosity of the mixed solution, reduce the blockage of the sprayer 71, and concentrate 25wt%~35wt% of the water (for example, 30wt% of the water) in the mixed solution, which can reduce the heating energy consumption of the high-temperature roasting furnace 7, thereby reducing the cost of preparing the ferromanganese phosphate precursor.

[0060] In some embodiments, the preset particle size D50 is less than or equal to 800 nm. The preset particle size includes a first preset particle size and a second preset particle size, where the first preset particle size is greater than the second preset particle size. The inlet gas flow rate of the carrier gas in the spiral gas pipe 731 includes a first inlet gas flow rate and a second inlet gas flow rate, and the first inlet gas flow rate is less than the second inlet gas flow rate. Among them, by adjusting the inlet gas flow rate of the carrier gas in the spiral gas pipe 731 through the inlet gas flow rate regulator 732, powdery lithium iron phosphate precursors with at least two preset particle sizes are formed, including: the inlet gas flow rate regulator 732 adjusts the inlet gas flow rate of the carrier gas in the spiral gas pipe 731 to the first inlet gas flow rate to form a powdery lithium iron phosphate precursor with the first preset particle size; the inlet gas flow rate regulator 732 adjusts the inlet gas flow rate of the carrier gas in the spiral gas pipe 731 to the second inlet gas flow rate to form a powdery lithium iron phosphate precursor with the second preset particle size. In this embodiment, according to the particle size requirement of the lithium iron phosphate precursor, when the carrier gas in the spiral gas pipe 731 is adjusted to the smaller first inlet gas flow rate, the downward obstruction of the atomized droplets sprayed by the atomizer 71 is smaller, and the suspension time of the atomized droplets during evaporation treatment, drying treatment and roasting treatment is shorter. Then, the solvent evaporation and pyrolysis of the atomized droplets are less, reducing the drying and solidification effects of the atomized droplets. As a result, the particle size of the lithium iron phosphate precursor will be relatively large; while when the carrier gas in the spiral gas pipe 731 is adjusted to the larger second inlet gas flow rate, the downward obstruction of the atomized droplets sprayed by the atomizer 71 is larger, and the suspension time of the atomized droplets during evaporation treatment, drying treatment and roasting treatment is longer. Then, the solvent evaporation and pyrolysis of the atomized droplets are more, promoting the drying and solidification of the atomized droplets. As a result, the particle size of the lithium iron phosphate precursor will be relatively small.

[0061] In some embodiments, the first preset particle size is 400 nm < D501 ≤ 800 nm; and / or, the second preset particle size is 20 nm ≤ D502 ≤ 200 nm; the first inlet gas flow rate is 5NM 3 / h ≤ Q1 ≤ 30 Nm 3 / h, and the second inlet gas flow rate is 40 NM 3 / h ≤ Q2 ≤ 120 Nm 3 / h. In this embodiment, the smaller first inlet gas flow rate corresponds to the formation of a larger first preset particle size, and the larger second inlet gas flow rate corresponds to the formation of a smaller second preset particle size, thereby realizing the control of the particle size of the lithium iron phosphate precursor by adjusting the inlet gas flow rate of the spiral gas pipe 731.

[0062] In some other embodiments, the preset particle sizes further include a third preset particle size, which is greater than the second preset particle size and less than the first preset particle size. The inlet gas flow rate of the carrier gas in the spiral gas pipe 731 further includes a third inlet gas flow rate, which is less than the second inlet gas flow rate and greater than the first inlet gas flow rate. The third preset particle size is 300 nm < D503 ≤ 600 nm, and the third inlet gas flow rate is 30 NM 3 / h < Q3 < 10 NM 3 / h. In this embodiment, the third preset particle size is between the second preset particle size and the first preset particle size, and the third inlet gas flow rate is between the first inlet gas flow rate and the second inlet gas flow rate. The third inlet gas flow rate correspondingly forms the third preset particle size between the larger particles and the smaller particles, so as to realize the control of multiple particle sizes of the iron manganese phosphate precursor by adjusting the inlet gas flow rate of the spiral gas pipe 731.

[0063] It can be understood that the suspension time of the atomized droplets in the evaporation zone, drying zone and roasting zone can also be controlled by adjusting the ventilation time of the carrier gas in the spiral gas pipe 731 to form multiple particle sizes of the iron manganese phosphate precursor. Or, the suspension time of the atomized droplets in the evaporation zone, drying zone and roasting zone is controlled by adjusting the ventilation time and inlet gas flow rate of the carrier gas in the spiral gas pipe 731 at the same time to form multiple particle sizes of the iron manganese phosphate precursor.

[0064] In some embodiments, the preset atomization method is the two-fluid internal mixing gas atomization formed by the carrier gas and the mixed solution. Among them, the ratio of the flow rate of the carrier gas to the flow rate of the mixed solution is (50~400):1; and / or, the temperature of preheating and concentration is 65 °C~95 °C. In this embodiment, the flow rate of the carrier gas is much larger than that of the mixed solution, which is convenient for dispersing the mixed solution by the large-flow carrier gas to form atomized droplets. For example, the flow rate of the carrier gas is 30 Nm 3 / h~90 Nm 3 / h, and the flow rate of the mixed solution is 0.225 Nm 3 / h~0.6 Nm 3 / h.

[0065] In some embodiments, the temperature of the calcination treatment is 500°C to 1000°C; and / or, the time of the evaporation treatment, the drying treatment and the calcination treatment is 2 min to 5 min. Among them, the temperature of the evaporation treatment is 100-200°C, and the temperature of the drying treatment is 300-450°C. In this embodiment, the evaporation treatment is to evaporate the solvent of the atomized droplets, thereby reducing the particle size of the atomized droplets, and at the same time, it is convenient to accelerate the pyrolysis rate after removing the solvent; the drying treatment is to remove the solvent and water involved in the evaporated droplets, further reduce the particle size of the atomized droplets, and at the same time, it is convenient to accelerate the pyrolysis rate after removing the solvent; the calcination treatment is to heat the atomized droplets of manganese solution, ferrophosphorus solution and dispersant to undergo pyrolysis reaction to release reaction gas and retain solid spherical solid matter to form a powdered manganese ferrophosphate precursor.

[0066] In some embodiments, the mass ratio of manganese to hydrochloric acid in the ferromanganese phosphate precursor is 1:(5-20); and / or, the mass ratio of iron to hydrochloric acid in the ferromanganese phosphate precursor is 1:(5-20); and / or, the molar ratio of the sum of manganese and iron to phosphorus in the ferromanganese phosphate precursor is 1:(0.9-1.1); and / or, hydrochloric acid can also be nitric acid or sulfuric acid. In this embodiment, the ratios of manganese to hydrochloric acid, iron to hydrochloric acid, and manganese iron to phosphorus are defined to control the element ratio of manganese iron in the ferromanganese phosphate precursor, thereby improving the electrochemical performance of the positive electrode material prepared using the ferromanganese phosphate precursor.

[0067] In some embodiments, the amount of dispersant added is 0.5% to 2.0% of the total mass of the mixed solution of the manganese-containing solution, the ferrophosphorus solution and the dispersant. The mass percentage of the dispersant in this embodiment can effectively disperse the precursor without increasing the cost, thereby forming a precursor that meets the requirements in morphology, crystal form and particle size. For example, the dispersant is polyethylene glycol, which has good water solubility (can effectively disperse particles in a water-based system), low toxicity, biocompatibility, and surface activity (having hydrophobic and hydrophilic parts, which can reduce interfacial tension and stabilize the suspension).

[0068] In some embodiments, the phosphorus source includes at least one of ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, phosphoric acid, iron phosphate, lithium phosphate and lithium dihydrogen phosphate; and / or, the iron source includes metal iron powder, metal iron sheet, metal iron ingot, red iron oxide, ferric tetroxide, ferric oxyhydroxide, ferric sulfate, ferric nitrate, ferric phosphate, ferrous oxalate, ferrous trioxide, ferric chloride, ferrous chloride and its hydrates or a combination thereof; and / or, the manganese source includes metal manganese powder, metal manganese sheet, metal manganese ingot, manganese monoxide, manganese dioxide, manganese tetraoxide, manganese sulfate, manganese nitrate, manganese phosphate, manganese oxalate, manganese chloride and its hydrates or a combination thereof; and / or, the carrier gas includes one or more combinations of nitrogen, argon, helium, neon, krypton and xenon. In this embodiment, the sources of the phosphorus source, iron source, manganese source, carrier gas and dispersant are limited, which is convenient for reducing the cost of preparing the ferromanganese phosphate precursor and for selecting the corresponding type according to different needs.

[0069] The technical solution of the present application is illustrated below through specific embodiments and comparative examples.

[0070] Example 1

[0071] The high-temperature roasting device includes a first dissolving tank 1, a second dissolving tank 2, a mixing tank 3, a venturi processor 4, a pump 5, a valve 6 and a vertical high-temperature roasting furnace 7. The high-temperature roasting furnace 7 includes a sprayer 71 arranged on the top, 6 groups of heaters 72 and 2 particle size regulators 73, wherein 3 groups of microwave heaters are arranged in the evaporation zone, 2 groups of microwave heaters are arranged in the drying zone, and 1 group of gas heaters is arranged in the roasting zone; or 1 particle size regulator 73 is respectively arranged in the evaporation zone and the drying zone.

[0072] S11, by mass, 1 part of metallic manganese sheet and 5 parts of hydrochloric acid are reacted in a first dissolution tank 1 to generate a manganese-containing solution.

[0073] S12, 1 part of metal iron sheet, 1 part of ammonium phosphate and 5 parts of hydrochloric acid are reacted in the second dissolving tank 2 to generate ferrophosphorus solution.

[0074] S2, the manganese-containing solution, the ferrophosphorus solution and 1.0% of the total mass of the mixed solution by weight of the dispersant are uniformly mixed in a mixing tank 3 to obtain a mixed solution.

[0075] S3, the mixed solution in the mixing tank 3 is sent to the venturi processor 4 for preheating through the pump 5, and the preheating temperature is 80°C.

[0076] S4, the mixed solution that has been preheated and concentrated by 30 wt% is sent to the inlet of the high-temperature roasting furnace 7 through the pump 5.

[0077] S5. The high-temperature roasting furnace 7 performs spray pyrolysis on the mixed solution in a nitrogen atmosphere, and forms powdery manganese iron phosphate precursors with two preset particle sizes through the sprayer 71 and the particle size regulator 73;

[0078] Among them, the ratio of the air flow rate to the mixed solution flow rate is 200:1, the first preset particle size is 600 nm < D501 ≤ 700 nm; the second preset particle size is 200 nm ≤ D502 ≤ 300 nm, the first intake air flow rate is 25 Nm 3 / h, the second intake air flow rate is 35 Nm 3 / h, the evaporation treatment temperature is 150 °C, the drying treatment temperature is 350 °C, and the roasting treatment temperature is 800 °C; the total suspension time of the evaporation treatment, drying treatment, and roasting treatment corresponding to the first preset particle size is 3.5 min, and the total suspension time of the evaporation treatment, drying treatment, and roasting treatment corresponding to the second preset particle size is 4.0 min.

[0079] S6. Wash, grind, demagnetize, and dry the manganese iron phosphate precursors with two preset particle sizes respectively to obtain manganese iron phosphate precursors with two preset particle sizes.

[0080] Example 2: The difference from Example 1 is that one particle size regulator 73 is provided in each of the evaporation zone, drying zone, and roasting zone, and the parameters of the spray roasting in step S5 are adjusted to form manganese iron phosphate precursors with two preset particle sizes.

[0081] Among them, the ratio of the air flow rate to the mixed solution flow rate is 300:1, the first preset particle size is 700 nm < D501 ≤ 800 nm; the second preset particle size is 100 nm ≤ D502 ≤ 200 nm, the first intake air flow rate is 8 Nm 3 / h, the second intake air flow rate is 60 Nm 3 / h, the evaporation treatment temperature is 150 °C, the drying treatment temperature is 350 °C, and the roasting treatment temperature is 800 °C; the total suspension time of the evaporation treatment, drying treatment, and roasting treatment corresponding to the first preset particle size is 3.0 min, and the total suspension time of the evaporation treatment, drying treatment, and roasting treatment corresponding to the second preset particle size is 5.0 min.

[0082] Example 3: The difference from Example 1 is that one particle size regulator 73 is provided in each of the evaporation zone, drying zone, and roasting zone, and the parameters of the spray roasting in step S5 are adjusted to form manganese iron phosphate precursors with three preset particle sizes.

[0083] Among them, the ratio of the flow rate of air to the flow rate of the mixed solution is 400:1, the first preset particle size is 600 nm < D501 ≤ 700 nm; the second preset particle size is 100 nm ≤ D502 ≤ 200 nm, the third preset particle size is 400 nm ≤ D503 ≤ 500 nm, the first intake air flow rate is 25 Nm 3 / h, the second intake air flow rate is 60 Nm 3 / h, the third intake air flow rate is 20 Nm 3 / h, the temperature of the evaporation treatment is 150 °C, the temperature of the drying treatment is 350 °C, and the temperature of the calcination treatment is 800 °C; the total suspension time of the evaporation treatment, drying treatment and calcination treatment corresponding to the first preset particle size is 3.5 min, and the total suspension time of the evaporation treatment, drying treatment and calcination treatment corresponding to the second preset particle size is 5.0 min. The total suspension time of the evaporation treatment, drying treatment and calcination treatment corresponding to the third preset particle size is 4.5 min.

[0084] Comparative example: The difference from Example 1 is that the particle size regulator 73 is not provided, and only the manganese iron phosphate precursor and the lithium manganese iron phosphate cathode material with the second preset particle size are formed.

[0085] The manganese iron phosphate precursors prepared in Example 1, Example 2 and the comparative example were made into lithium manganese iron phosphate cathode materials and then assembled into coin cells to test the tap density. After testing, the tap densities of Example 1, Example 2 and the comparative example were 2.540 g / cm 3 , 2.650 g / cm 3 and 2.480 g / cm 3 .

[0086] It should be understood that the magnitudes of the sequence numbers of the steps in the above embodiments do not mean the order of execution. The order of execution of each process should be determined according to its function and internal logic, and should not constitute any limitation to the implementation process of the embodiments of the present application. In the above embodiments, the descriptions of the various embodiments have their own emphases. For parts not detailed or recorded in a certain embodiment, reference may be made to the relevant descriptions of other embodiments.

[0087] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the foregoing embodiments, those of ordinary skill in the art should understand that: they can still modify the technical solutions recorded in the foregoing embodiments, or perform equivalent replacements on some of the technical features; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for preparing a ferromanganese phosphate precursor, characterized in that: A ferromanganese phosphate precursor is prepared based on a high-temperature roasting device, the high-temperature roasting device includes a first dissolving tank, a second dissolving tank, a mixing tank, a venturi processor, a pump, a valve and a vertical high-temperature roasting furnace, the high-temperature roasting furnace includes a sprayer arranged at the top, at least one group of heaters and at least one particle size regulator, the heater is arranged at the middle and bottom of the outer surface of the high-temperature roasting furnace, the particle size regulator is arranged inside the high-temperature roasting furnace corresponding to the position of the heater, the particle size regulator makes the sprayed droplets move in reverse to adjust the suspension time of the droplets to control the particle size of the ferromanganese phosphate precursor, the outlet of the first dissolving tank and the outlet of the second dissolving tank are connected to the first inlet of the mixing tank, the outlet at the bottom of the mixing tank is connected to the first inlet of the side wall of the venturi processor, the outlet at the bottom of the venturi processor is connected to the inlet of the pump, the outlet of the pump is respectively connected to the inlet at the top of the high-temperature roasting furnace and the second inlet on the side wall of the venturi processor, and the first outlet near the top of the high-temperature roasting furnace is connected to the third inlet at the top of the venturi processor; Wherein, any of the particle size regulators comprises a spiral air pipe, wherein a plurality of jet holes are arranged on one side of the spiral air pipe close to the sprayer, and the diameters of the jet holes in each semicircle of the spiral air pipe increase successively from the inside to the outside along the spiral air pipe, and the jet holes of the spiral air pipe are distributed at preset angles in a clockwise or counterclockwise direction, or the jet holes of adjacent circles of the spiral air pipe are staggered; The preparation method comprises: S11, reacting a manganese source and hydrochloric acid in the first dissolution tank to generate a manganese-containing solution; S12, reacting an iron source, a phosphorus source and hydrochloric acid in the second dissolution tank to generate a ferrophosphorus solution; S2, uniformly mixing the manganese-containing solution, the ferrophosphorus solution and the dispersant in the mixing tank to obtain a mixed solution; S3, sending the mixed solution in the mixing tank to the venturi processor for preheating through the pump; S4, sending the preheated and concentrated mixed solution to the inlet of the high-temperature roasting furnace through the pump; S5, the high temperature calcining furnace sprays and calcines the mixed solution in the atmosphere of the carrier gas, and forms at least two kinds of powdered manganese ferrophosphate precursors with preset particle sizes through the sprayer and the particle size regulator; S6, washing, grinding, demagnetizing and drying the at least two kinds of ferromanganese phosphate precursors with preset particle sizes, respectively, to obtain at least two kinds of ferromanganese phosphate precursors with preset particle sizes.

2. The preparation method according to claim 1, characterized in that The sprayer includes an adjustable nozzle and a flow regulator, any of the particle size regulators also includes an air intake flow regulator, and the gas in the spiral air pipe is the carrier gas; Step S5 includes: Mixing the mixed solution with the carrier gas and setting the flow rate of the gas-liquid mixture through the flow regulator to a preset flow rate, and then adjusting the adjustable nozzle to a preset aperture to spray in a preset atomization mode; The droplets of the atomized mixed solution are subjected to evaporation treatment, drying treatment and calcination treatment in sequence from top to bottom, and the intake flow rate of the carrier gas in the spiral air pipe is adjusted by the intake flow regulator to form the powdered manganese ferrophosphate precursor with at least two preset particle sizes; The mixed gas of the gases generated by the evaporation treatment, the drying treatment and the calcination treatment and the carrier gas enters the third inlet of the venturi processor through the first outlet near the top of the high-temperature calcination furnace, and the mixed gas is preheated and concentrated on the mixed solution through the self-circulation of the venturi processor and the pump, and the preheating and concentration is to evaporate 25wt%~35wt% of the water in the mixed solution.

3. The preparation method according to claim 2, characterized in that The preset particle size is less than or equal to 800 nm, the preset particle size includes a first preset particle size and a second preset particle size, the first preset particle size is greater than the second preset particle size, the intake flow rate of the carrier gas in the spiral air pipe includes a first intake flow rate and a second intake flow rate, the first intake flow rate is less than the second intake flow rate; The powdered ferromanganese phosphate precursor having at least two preset particle sizes is formed by adjusting the intake flow rate of the carrier gas in the spiral air pipe through the intake flow rate regulator, comprising: The air intake flow rate regulator adjusts the air intake flow rate of the carrier gas in the spiral air pipe to the first air intake flow rate to form the powdered manganese ferrophosphate precursor with the first preset particle size; The air intake flow rate regulator adjusts the air intake flow rate of the carrier gas in the spiral air pipe to the second air intake flow rate to form the powdered manganese ferrophosphate precursor with the second preset particle size.

4. The preparation method according to claim 3, characterized in that The first preset particle size is 400 nm <D501≦800 nm; And / or, the second preset particle size is 20 nm≦D502≦200 nm.

5. The preparation method according to claim 2, characterized in that: The preset atomization mode is a two-fluid internal mixing gas flow atomization formed by the carrier gas and the mixed solution, wherein the ratio of the flow rate of the carrier gas to the flow rate of the mixed solution is (50-400):1; And / or, the preheating and concentration temperature is 65°C to 95°C.

6. The preparation method according to claim 2, characterized in that The calcination temperature is 500°C to 1000°C; And / or, the total time of the evaporation treatment, the drying treatment and the calcination treatment is 2 min to 5 min.

7. The preparation method according to claim 1, characterized in that: The mass ratio of manganese element in the ferromanganese phosphate precursor to the hydrochloric acid is 1:(5-20); And / or, the mass ratio of the iron element in the ferromanganese phosphate precursor to the hydrochloric acid is 1:(5-20); And / or, the molar ratio of the sum of manganese and iron elements to phosphorus in the ferromanganese phosphate precursor is 1:(0.9-1.1); And / or, the hydrochloric acid is replaced by nitric acid or sulfuric acid.

8. The preparation method according to claim 1, characterized in that: The phosphorus source includes at least one of ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, phosphoric acid, iron phosphate, lithium phosphate and lithium dihydrogen phosphate; And / or, the iron source comprises one or a combination of metallic iron powder, metallic iron flakes, metallic iron ingots, ferroferric oxide, ferric oxyhydroxide, ferric sulfate, ferric nitrate, ferric phosphate, ferrous oxalate, ferrous oxide, ferric chloride, ferrous chloride and ferrous chloride hydrate; And / or, the manganese source comprises one or a combination of metallic manganese powder, metallic manganese flakes, metallic manganese ingots, manganese monoxide, manganese dioxide, manganese tetraoxide, manganese sulfate, manganese nitrate, manganese phosphate, manganese oxalate, manganese chloride and manganese chloride hydrate.

9. A positive electrode sheet, characterized in that: The positive electrode plate is made of a positive electrode material prepared from a ferromanganese phosphate precursor obtained by the preparation method according to any one of claims 1 to 8.

10. A lithium battery, characterized in that: The lithium battery comprises the positive electrode sheet as claimed in claim 9.