Preparation of high-fluidity spherical silicon micropowder by self-propagating low-temperature combustion

Through the combination of self-propagation low-temperature combustion process and screen circulation pipeline, the problems of complex preparation process and insufficient fluidity of spherical silicon micropowder are solved, and high-efficiency and low-energy consumption of high-flow spherical silicon micropowder preparation is achieved, avoiding mechanical activation Difficulty in feeding caused by too small particle size.

CN118754138BActive Publication Date: 2024-12-06SINOMA JIANGSU SOLAR ENERGY NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410743526.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-12-06
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

In the prior art, the preparation process of spherical silicon micropowder is complex, with high energy consumption and insufficient fluidity, which leads to the inability to achieve industrial production and the feeding of fine powder after mechanical activation is difficult.

Method used

The self-propagation low-temperature combustion process is adopted, and the self-propagation low-temperature combustion reaction is fed into the suspended combustion furnace through the first screw feeder, eliminating the spray drying process, setting up screens and circulation pipes to ensure the appropriate particle size, and avoiding the inflow caused by too small particle size. The material is difficult, streamline the process flow and reduce energy consumption.

Benefits of technology

The preparation of high-flow spherical silicon micropowder has been achieved, which has improved the work efficiency, reduced the preparation time and equipment requirements, and improved the spherical degree and fluidity of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754138B_ABST
    Figure CN118754138B_ABST
Patent Text Reader

Abstract

The present invention discloses a self-propagating low-temperature combustion preparation process of high-fluidity spherical silicon micropowder, wherein the silicon powder is pretreated, and after the pretreatment, the silicon powder is fed into a suspension combustion furnace at a temperature of 1000°C through a first screw feeder to undergo a self-propagating low-temperature combustion reaction in an air atmosphere; after cooling, the high-fluidity spherical silicon micropowder is collected; during the self-propagating low-temperature combustion reaction, the air flow velocity is maintained at 20L / min; the pretreatment process is to activate the silicon powder through an activation device; a second screw feeder is arranged below the outlet of the activation device, a collection pipe is arranged at the outlet of the second screw feeder, a collection tank is arranged below the collection pipe, a fine activated silicon powder collection port is arranged between the outlet and the second screw feeder, and a plug is arranged on the fine activated silicon powder collection port; the second screw feeder is the same as the first screw feeder. The present invention avoids the problem of feeding difficulty caused by too small particle size after mechanical activation; and eliminates the spray drying process, simplifies the preparation process, and reduces energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a self-propagating low-temperature combustion preparation process of high-fluidity spherical silicon micropowder. Background Art

[0002] Spherical silicon micropowder is widely used in integrated circuit packaging due to its excellent fluidity and low thermal expansion coefficient. However, chemical methods such as microemulsion method and sol-gel method are used to emulsify, concentrate and granulate high-purity organic silane or water glass to obtain high-purity silicon micropowder, and then calcine and spheroidize to obtain high-purity and low-radioactive spherical silicon micropowder. The product prepared by this method has high purity but the process is complicated, and the samples often have shortcomings such as rough surface, low bulk density, insufficient fluidity and low filling degree, which affect their performance and make it impossible to achieve industrial production.

[0003] Patent publication number CN102795632B: A method for preparing ultrafine silicon powder by self-propagating low-temperature combustion, which first prepares sodium silicate, then prepares silicate sol, then prepares a mixed combustion liquid, then removes carbon impurities and anneals to obtain ultrafine silicon powder. The process requires the preparation of multiple intermediates, and finally removes carbon impurities and anneals. The process is complex and energy-intensive.

[0004] In the paper "Preparation and Performance of High-Purity and Low-Radioactive Spherical Silicon Micropowder" published in Volume 57, Issue 10 of Micro-Nano Electronics Technology in October 2020, Li Xiaodong mentioned that Zhu Yuan used the self-propagating low-temperature combustion method to prepare spherical silicon dioxide. In the paper "Powder Spheroidization Mechanism in Suspended Combustion Synthesized Silica" published in Volume 36, Supplement 1 of Rare Metal Materials and Engineering in August 2007, Zhu Yuan mentioned: Si powder is mechanically activated by adding NH4Cl to obtain activated Si powder, polyethylene oxide is added, and spherical agglomerates of particle size are obtained by spray drying. It is sent to a suspended combustion furnace, oxidized at a certain airflow velocity, air pressure and temperature, and combustion undergoes a self-propagating reaction to obtain the product. Since the original silicon powder has a particle size of tens of microns, its activity is low, which is not conducive to the occurrence of combustion synthesis reaction; although the reaction activity of the powder after ball milling is improved, the viscosity forces such as van der Waals force and electrostatic force between particles caused by its reduced particle size (about 2 microns) are sharply enhanced, becoming Class C particles, or sticky particles, which will bring difficulties to feeding; so it adopts spray drying of the activated fine powder to form spherical agglomerates with a particle size of about tens of microns for feeding and then sending it to the suspension combustion furnace for self-propagating low-temperature combustion to prepare spherical silicon micropowder. Therefore, it has to add a spray drying process, which makes the preparation process complicated, energy-intensive, and low in efficiency. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects in the prior art and provide a self-propagating low-temperature combustion preparation process for high-fluidity spherical silicon micropowder, so as to avoid the problem of feeding difficulty caused by too small particle size after mechanical activation; and to eliminate the spray drying process, simplify the preparation process, reduce energy consumption, reduce the equipment required for preparation, reduce preparation costs, improve work efficiency, and reduce preparation time.

[0006] To achieve the above object, the technical solution of the present invention is to design a self-propagating low-temperature combustion preparation process for high-fluidity spherical silicon powder, which is composed of the following process steps performed in sequence:

[0007] The silicon powder is pretreated and fed into a suspension combustion furnace at a temperature of 1000°C through a first screw feeder to undergo a self-propagating low-temperature combustion reaction in an air atmosphere; after cooling, the high-fluidity spherical silicon powder is collected;

[0008] During the self-propagating low-temperature combustion reaction, the airflow velocity is maintained at 20L / min; the pretreatment process is to activate the silicon powder through the activation equipment; a screen is set at the outlet of the activation equipment; a second screw feeder is set behind the discharge direction of the outlet of the activation equipment, a collection pipe is set at the outlet of the second screw feeder, a collection tank is set behind the discharge direction of the collection pipe, a fine activated silicon powder collection port is set between the outlet and the second screw feeder, and a plug is set on the fine activated silicon powder collection port; the second screw feeder is the same as the first screw feeder. The reaction products of the self-propagating low-temperature combustion reaction leave the hot zone with the airflow, and are collected after cooling in the cooler to obtain high-fluidity spherical silicon powder. By setting a screen, it is ensured that the silicon powder obtained is smaller than the required particle size (such as about 35 microns), and then setting a second screw feeder that is the same as the first screw feeder in front of the suspension combustion furnace can ensure that if too much small-size silicon powder is obtained, it will cause material blockage, so it can avoid the collected silicon powder particle size being too small, and it can avoid the problem of difficulty in feeding the suspension combustion furnace caused by the particle size after mechanical activation being too small; and it eliminates the spray drying process, simplifies the preparation process, reduces energy consumption, reduces the equipment required for preparation, reduces preparation costs, improves work efficiency, and reduces preparation time. Avoid the problem of insufficient fluidity of spherical silicon micropowder prepared by existing preparation methods such as microemulsion method, sol-gel method, etc., and adopt the self-propagating low-temperature combustion preparation process to achieve silicon powder particles in a microgravity field, good spherical degree after combustion, and high fluidity.

[0009] A further technical solution is that the activation equipment is a vibrating ball mill, and the aperture of the mesh on the screen is 30 to 35 microns; the vibrating ball mill is provided with a circulation pipeline connected to the inner cavity of the body to be used for re-introducing silicon powder larger than 35 microns into the activation equipment for further activation, and the circulation pipeline is located in front of the screen along the discharge direction. A circulation pump is provided on the circulation pipeline to ensure that silicon powder larger than 35 microns is re-introduced into the activation equipment for further activation. The circulation pump can generally be a powder delivery pump. The setting of the circulation pipeline can prevent large-particle silicon powder from accumulating at the screen and affecting the discharge. After such a setting, the discharge amount of silicon powder of the required particle size can be guaranteed, and the feed amount of the suspension combustion furnace can be reached earlier to carry out self-propagating low-temperature combustion to prepare high-fluidity spherical silicon micropowder.

[0010] A further technical solution is that after the silicon powder is pretreated, the pretreated silicon powder is first transferred from the collection tank to the barrel, and the silicon powder in the barrel is then fed to the first screw feeder, and the first screw feeder feeds to the bottom of the suspension combustion furnace; while feeding to the suspension combustion furnace, preheated air is also introduced into the suspension combustion furnace to ensure that the silicon powder is in a suspended state in the suspension combustion furnace; after the silicon powder reacts in the suspension combustion furnace, it is discharged from the air outlet above the suspension combustion furnace, and then separated in the cyclone dust collector to obtain high-fluidity spherical silicon micropowder. After the silicon powder reacts in the suspension combustion furnace, it is carried out of the top of the suspension combustion furnace by a mixture of water vapor and combustion products, and is separated from the hot gas in the cyclone dust collector of alumina. The preheated air is also introduced from the bottom of the suspension combustion furnace (air is introduced into the suspension combustion furnace through an air pipe independent of the silicon powder feed pipe).

[0011] A further technical solution is that the particle size of the silicon powder before pretreatment is 40 to 50 microns;

[0012] When the second screw feeder is blocked during pretreatment, the activated silicon powder that is not of small particle size in the collection tank is transferred to the barrel; at the same time, the activation equipment and the circulation pump on the circulation pipeline are stopped, and the plug is pulled out to collect the fine activated silicon powder for subsequent screening and grading.

[0013] A further technical solution is that when the silicon powder in the barrel reaches the feed amount of the suspension combustion furnace, the suspension combustion furnace starts to work, and at the same time, the circulation pump on the circulation pipeline starts to work.

[0014] A further technical solution is to restart the suspension combustion furnace and the circulation pump on the circulation pipeline to continue pretreating the remaining silicon powder after collecting the fine activated silicon powder between the outlet and the second screw feeder; or to add silicon powder to the activation equipment to continue pretreatment until the amount of activated silicon powder that is not small-particle size in the collection tank reaches the feed amount of the suspension combustion furnace.

[0015] The cleaning of the second screw feeder after blockage is a prior art, and the general process is: turning off the power, disassembling the screw machine, and reassembling the machine after mechanical cleaning, which will not be repeated.

[0016] The advantages and beneficial effects of the present invention are: avoiding the problem of insufficient fluidity of spherical silicon micropowder prepared by existing preparation methods such as microemulsion method, sol-gel method, etc., and adopting a self-propagating low-temperature combustion preparation process to achieve silicon powder particles in a microgravity field, with a good degree of sphericity and high fluidity after combustion.

[0017] The setting of the circulation pipeline can prevent large-sized silicon powder from accumulating on the screen and affecting the discharge. This setting can ensure the discharge amount of silicon powder with the required particle size, and reach the feed amount of the suspension combustion furnace earlier to carry out self-propagating low-temperature combustion to prepare high-fluidity spherical silicon powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of silicon powder pretreatment related equipment in Example 1 of a self-propagating low-temperature combustion preparation process of high-fluidity spherical silicon micropowder of the present invention;

[0019] Figure 2 yes Figure 1 A top view of the activation device in FIG.

[0020] Figure 3 yes Figure 2 AA section view;

[0021] Figure 4 yes Figure 2 A three-dimensional schematic diagram of

[0022] Figure 5 It is the relevant silicon micropowder preparation equipment involved in the preparation process of the present invention;

[0023] Figure 6 yes Figure 5 A three-dimensional schematic diagram of a medium cyclone dust collector;

[0024] Figure 7 is a schematic diagram of a second embodiment of the present invention;

[0025] Figure 8 yes Figure 7 A top view of the activation device;

[0026] Fig. 9 yes Figure 8 An enlarged schematic diagram of the middle oval circle A;

[0027] Fig.10 is a schematic diagram of Embodiment 3 of the present invention;

[0028] Fig.11 is a schematic diagram of an activation device in Embodiment 4 of the present invention;

[0029] Fig.12 yes Fig.11Top view after removing the baffle and airbag;

[0030] Fig.13 It is a schematic diagram of the activation device in the fifth embodiment of the present invention.

[0031] In the figure: 1. first screw feeder; 2. suspension combustion furnace; 3. screen; 4. second screw feeder; 5. cyclone dust collector; 6. collecting tank; 7. plug; 8. circulation pipe; 9. barrel; 10. cylindrical barrel; 11. base frame; 12. side plate; 13. fixing rod; 14. limiting ring; 15. collar; 16. metal spike; 17. rubber layer; 18. rubber ring; 19. parallel plate; 20. feed port; 21. rotating rod; 22. reduction motor; 23. motor seat; 24. elastic rubber skin layer; 25. handle; 26. baffle; 27. air bag; 28. air inlet; 29. ​​air outlet; 30. sprocket chain mechanism; 31. elliptical top ball. DETAILED DESCRIPTION

[0032] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.

[0033] Embodiment 1: Figures 1 to 6 As shown (for ease of illustration, Figures 2 to 4 The present invention is a self-propagating low-temperature combustion preparation process of high-fluidity spherical silicon micropowder, which is composed of the following process steps performed in sequence:

[0034] Pre-treat the silicon powder, and feed the pre-treated silicon powder into a suspension combustion furnace 2 at a temperature of 1000°C through a first screw feeder 1 to undergo a self-propagating low-temperature combustion reaction in an air atmosphere; collect and obtain high-fluidity spherical silicon micropowder after cooling;

[0035] During the self-propagating low-temperature combustion reaction process, the air flow velocity is maintained at 20L / min; the pretreatment process is to activate the silicon powder through an activation device; a screen 3 is arranged at the outlet of the activation device; a second screw feeder 4 is arranged behind the discharge direction of the outlet of the activation device, a collecting pipe is arranged at the outlet of the second screw feeder 4, a collecting tank 6 is arranged behind the discharge direction of the collecting pipe, a fine activated silicon powder collection port is arranged between the outlet and the second screw feeder 4, and a plug 7 is arranged on the fine activated silicon powder collection port; the second screw feeder 4 is the same as the first screw feeder 1.

[0036] The activation equipment is a vibrating ball mill, and the aperture of the sieve holes on the screen 3 is 30 to 35 microns; a circulation pipe 8 connected to the inner cavity of the vibrating ball mill is arranged on the body of the vibrating ball mill for re-introducing silicon powder larger than 35 microns into the activation equipment for further activation, and the circulation pipe 8 is located in front of the screen 3 along the discharge direction.

[0037] After pretreatment of silicon powder, the pretreated silicon powder is first transferred from the collection tank 6 to the barrel 9, and the silicon powder in the barrel 9 is then fed to the first screw feeder 1, and the first screw feeder 1 feeds to the bottom of the suspension combustion furnace 2; while feeding to the suspension combustion furnace 2, preheated air is also introduced into the suspension combustion furnace 2 to ensure that the silicon powder is in a suspended state in the suspension combustion furnace 2; after the silicon powder reacts in the suspension combustion furnace 2, it is discharged from the air outlet above the suspension combustion furnace 2, and then separated in the cyclone dust collector 5 to obtain high-flowability spherical silicon micropowder. The particle size of the silicon powder before pretreatment is 40 to 50 microns; when the pretreatment reaches the second screw feeder 4 blocking material, the activated silicon powder in the collection tank 6 that is not of small particle size is transferred to the barrel 9; at the same time, the activation equipment and the circulation pump on the circulation pipeline 8 are stopped and the plug 7 is pulled out to collect the fine activated silicon powder for subsequent screening and classification. When the silicon powder in the barrel 9 reaches the feed amount of the suspension combustion furnace 2, the suspension combustion furnace 2 works, and the circulation pump on the circulation pipeline 8 works at the same time. After collecting the fine activated silicon powder between the outlet and the second screw feeder 4, restart the suspension combustion furnace 2 and the circulation pump on the circulation pipe 8 to continue pretreating the remaining silicon powder; or add silicon powder to the activation equipment to continue pretreating until the amount of activated silicon powder that is not small-particle size in the collection tank 6 reaches the feed amount of the suspension combustion furnace 2. A screw feeder is arranged below the outlet, a collecting pipe is arranged at the outlet of the screw feeder, a collecting tank 6 is arranged below the collecting pipe, a fine activated silicon powder collecting port is arranged between the outlet and the screw feeder, and a plug 7 is arranged on the fine activated silicon powder collecting port; (the screw feeder and the screw feeder in front of the suspension combustion furnace 2 have exactly the same specifications, dimensions, power and other parameters). If blockage occurs, it means that the particle size of the activated silicon powder is small, which means that if it is used for feeding the suspension combustion furnace 2 later, feeding will also be difficult. In this case, activation is stopped immediately, and the activated silicon powder that meets the particle size requirements and has been collected is used as silicon powder for subsequent self-propagating low-temperature combustion preparation. For silicon powder that is blocked, that is, silicon powder with a smaller particle size, the fine activated silicon powder is collected by pulling out the plug 7 (that is, taken out from the activation equipment), and after screening and grading, it can be used for other purposes according to the particle size of the silicon powder. (The particle size of the material after ball milling is generally controlled by process parameters, including mill speed, charging rate, grinding medium type and grinding ball size. The operator will set the appropriate speed, charging rate and select the grinding medium type and grinding ball size based on experience; however, in this embodiment, it is still necessary to conduct several tests before starting to obtain the appropriate process parameters before preparation)

[0038] Therefore, the preparation process of this embodiment is as follows: Si powder is mechanically activated to obtain activated Si powder with a particle size of about 35 microns, which is then fed into the suspension combustion furnace 2 and oxidized at a certain air flow velocity, air pressure and temperature, and burned to produce a self-propagating reaction;

[0039] A more optimal technical solution is that the activation equipment (a ball mill in this embodiment) has its rotation axis inclined to the horizontal plane and the inclination direction is gradually inclined downward along the discharge direction. In this way, when the ball mill is started, once the silicon powder is ball-milled to a particle size that can pass through the filter holes of the screen 3, the material is discharged, and the large particle size material larger than the filter holes of the screen 3 is continuously circulated to the inner cavity of the ball mill for mechanical activation ball milling.

[0040] Since the circulation pipe 8 and the circulation pump are fixedly arranged on the outer surface of the ball mill body, the size of the base frame 11 of the ball mill is slightly larger than that of the ball mill of the same specification to avoid interference with the movement of the circulation pipe 8 (and the circulation pump) rotating with the cylindrical barrel 10.

[0041] Therefore, the main idea of ​​this embodiment is to activate it properly to avoid the problem of the prior art that the particle size after activation is too small and the feeding is difficult; while in this embodiment, proper activation can complete the combustion synthesis reaction, and because the particle size is not very small, the problem of feeding difficulty is solved.

[0042] Embodiment 2: The difference from Embodiment 1 is that Figures 7 to 9 As shown (for ease of illustration, Figure 8 , Fig. 9Only part of the pointed assembly is shown), the activation device no longer uses a vibrating ball mill, and the structure of the activation device is: it includes a pair of relatively parallel side plates 12, the side plates are inclined to the horizontal plane, and a plurality of fixing rods are arranged on the side plates 12 from top to bottom, and a silicon powder mechanical activation impact body structure is fixed on the fixing rod 13 (refer to the gap between the shaft and the sleeve, which is usually calculated by the ratio of the shaft diameter to the sleeve inner diameter, and the conventional ratio is generally between 0.001 and 0.005. For example, if the shaft diameter is 50mm, the theoretical value of the inner diameter of the sleeve is 50mm+0.001mm×50mm=50.05mm~50mm+0.005mm×50mm=50.25mm; since the required particle size of the silicon powder after activation is micron-level, this embodiment In the embodiment, a direct fixing method is adopted to avoid the rotating impact body structure itself having too much mobility due to the large gap and failing to achieve the purpose of mechanically activating the silicon powder). The impact body structure on the fixed rod 13 covers the entire length of the fixed rod. The limiting ring 14 of the impact body structure is fixedly arranged on the fixed rod (that is, the limiting ring 14 is located at both ends of the fixed rod). The impact body structure includes a collar 15 fixedly arranged on the fixed rod 13. A plurality of ring spike assemblies are fixedly arranged on the collar 15. Each ring of spike assemblies is arranged in a circular array. The spike assemblies include a metal spike 16 and a rubber layer 17 covering the outer surface thereof (that is, the metal spike is fixedly connected to the rubber layer). The spike assembly is fixedly connected to the collar 15 through a rubber ring 18. The rubber ring 18 is formed integrally with the rubber layer 17. The aforementioned spike assembly is also arranged on the limiting ring 14, but the rubber ring in the spike assembly on the limiting ring is fixedly connected to the limiting ring. The spacing between adjacent fixed rods 13 is larger than the outer diameter of the collar 15, and the larger size is the size of the spike assembly. The spike assemblies on adjacent fixed rods 13 are staggered (similar to the meshing of gears, which ensures that the silicon powder poured from the feed port is always collided during the falling process to cause surface defects of the powder to increase the reactivity of the powder). The size of the spike assembly is between 5 microns and 35 microns. The size of the spike assembly on the fixed rod 13 can be gradually reduced from top to bottom to achieve the purpose of gradually strengthening mechanical activation (because the original mechanical activation method is no longer used, but the silicon powder is poured into the silicon powder from the upper feed port of the activation equipment, and the inclined body is used to make the silicon powder fall due to its own weight, and hit the impact body during the fall, and the silicon powder is mechanically activated through the spike structure on the impact body. Therefore, the activation time is now shorter, so even if the impact body is set smaller or even smaller than the lower limit of the required silicon powder particle size after activation of 30 microns, it does not mean that it can be mechanically activated to about 5 microns; so this setting can obtain the required particle size of activated silicon powder).The body of the activation device is composed of the above-mentioned two side plates 12 and another pair of parallel plates 19 formed by the side plates (the spacing between the parallel plates 19 and the ring 15 is also the size of the spike assembly, so that the problem of silicon powder sliding down the inner wall of the body not being mechanically activated can be avoided; and in this embodiment, the rubber ring 18 is used for fixed connection (to avoid the metal spike 16 from hitting the outer surface of the ring, a metal spike 16 with a length smaller than the rubber layer 17 can be used, that is, the metal spike 16 is arranged close to the tip of the rubber layer 17), that is, the movable arrangement is used, even if the spike assembly hits the parallel plates 19, it is extremely difficult for the spike assembly to be damaged), the upper opening of the rectangular cylinder surrounded by the side plates and the parallel plates is the feed port 20 for silicon powder, and a circulation pipe 8 and a circulation pump can also be set on the body, so that the silicon powder can circulate several times in the body of the activation device to avoid the problem of too little silicon powder meeting the standard caused by only one time. A screen 3 is arranged at the lower opening of the rectangular cylinder surrounded by the side plates and the parallel plates, and the aperture of the screen holes on the screen 3 is 30 to 35 microns.

[0043] Pour 40-50 micron silicon powder into the body of the activation equipment from the feed port, and start the circulation pump at the same time. The silicon powder will collide with the impact body structure on the fixed rod and be mechanically activated. The spike assembly and the ring fixed on the fixed rod have a certain degree of mobility to avoid damage to the spike assembly on the impact body structure after long-term work, which will not play a role in mechanically activating the powder. When the second screw feeder 4 is blocked during pretreatment, the activated silicon powder that is not of small particle size in the collection tank 6 is transferred to the barrel; at the same time, stop the activation equipment and the circulation pump on the circulation pipeline 8, and pull out the plug 7 to collect the fine activated silicon powder for subsequent screening and grading. Although the degree of mechanical activation is relatively small when the powder falls by its own weight and cooperates with the impact body structure, the problem of insufficient activation caused by falling can be strengthened by cooperating with the circulation pump for multiple times.

[0044] Embodiment 3: The difference from Embodiment 2 is that Fig.10 As shown (for ease of illustration, Fig.10Only one reduction motor is shown), the side plate 12 is no longer a fixed rod from top to bottom, but a rotating rod 21 rotatably arranged with the side plate, one end of the rotating rod extends beyond the body and is fixedly connected to the output shaft of the reduction motor 22 (the reduction motor is fixedly connected to the side plate 12 through the motor seat 23) to enhance the effect of mechanical activation. Although the rotating rod is driven by the reduction motor 22, there will inevitably be shaking or vibration, but the collar 15 on the impact body structure is fixedly connected to the rotating rod 21; and the spike assembly is fixedly connected to the collar through a rubber ring, so the spike assembly can allow collision, and can still play the role of mechanically activating the powder without worrying about the problem of collision and damage of the spike assemblies on adjacent rotating rods that are easily caused by this driving method; it can accept collisions between the spike assemblies, and cooperate with the inclined body to allow the powder to fall freely {that is, the powder stays in the body for a shorter time}, which can achieve the required degree of reducing the powder particle size, activating the powder while avoiding the problem of the powder being mechanically activated to a particle size that is too small and difficult to feed).

[0045] Embodiment 4: The difference from Embodiment 2 is that Fig.11 , Fig.12 As shown (same as Example 2, Fig.11The lower port is still provided with the same structure, including the second screw feeder, etc., which are not shown for the convenience of illustration and to avoid repetition). The upper and lower layers of elastic rubber layers 24 are fixedly bonded on both sides of the side plate 12. The side plate 12 is no longer a fixed rod from top to bottom, but a rotating rod 21 rotatably arranged with the side plate. One end of the rotating rod extends beyond the body and is fixedly connected to the handle 25. A fixed baffle 26 is arranged on the outer side of the side plate opposite to the elastic rubber layer 24 (the baffle 26 can be fixedly arranged on the frame of the activation device, and the body enclosed by the side plate and the elastic rubber layer 24 is also fixedly connected to the frame). An airbag 27 is fixedly arranged on the inner side of the baffle 26, and the non-fixed side of the airbag is arranged facing the elastic rubber layer 24. An air inlet 28 and an air outlet 29 are respectively arranged at the upper and lower ends of the airbag, and proportional valves are arranged at the air inlet and the air outlet; 40-50 micron silicon powder is fed from the feed port Pour it into the body of the activation device, and at the same time, inject gas into the airbag 27 through the air inlet 28 (open the proportional valve of the air inlet 28 to the maximum) to expand the airbag. Due to the obstruction of the baffle 26, the airbag 27 bulges toward the elastic rubber layer 24. The handle 25 is manually turned to drive the ring 15 fixed on the rotating rod 21 to rotate, so that the silicon powder hits the impact body structure on the rotating ring 15 when falling. When the handle is manually turned and a large resistance is obviously felt, it means that the airbag has expanded to the point that the elastic rubber layer 24 has abutted against the ring (or more accurately, against the impact body structure), then the opening of the proportional valve of the air outlet 29 is opened, and the opening of the proportional valve of the air inlet 28 is reduced at the same time, so that the expansion degree of the airbag can be appropriately reduced; when the resistance is obviously reduced when the handle is turned, the opening of the proportional valve of the air inlet 28 is increased, and the opening of the proportional valve of the air outlet 29 is reduced.

[0046] After such arrangement, there is no longer the problem that the distance between the parallel plate and the collar is difficult to control accurately (unlike the previous embodiment), which may easily cause the sharp object assembly to hit the parallel plate or the distance from the parallel plate is greater than the final required silicon powder particle size, resulting in low mechanical activation efficiency. By setting up the active intermittent "parallel plate" (the elastic rubber layer 24 on both sides of the side plate is equivalent to replacing the "parallel plate" of the previous embodiment), the silicon powder can always hit the inner wall of the machine body during the falling process in the machine body, avoiding the problem of poor distance control faced by the fixed side wall of the machine body (such as the parallel plate method used in the previous embodiment). It also reduces the accuracy requirements for installation.

[0047] Embodiment 5: The difference from Embodiment 4 is that Fig.13As shown, a reduction motor 22 is fixedly arranged on the side panel 12, and upper and lower layers of elastic rubber layers 24 are fixedly bonded on both sides of the side panel 12. A rotating rod rotatably arranged with the side panel is arranged on the side panel 12 from top to bottom, and one end of the rotating rod protrudes beyond the body and is connected to the reduction motor 22. An air bag 27 is fixedly arranged on the outer side of the side panel opposite to the elastic rubber layer 24, and a fixed sprocket chain mechanism 30 is arranged on the outer side of the side panel opposite to the air bag 27. The sprocket chain mechanism 30 can be fixedly arranged on the frame of the activation device body; an elliptical top ball 31 is fixedly arranged on the chain of the sprocket chain mechanism, and the elliptical top ball 31 can be a metal material in the middle and a rubber material covered on the outside to prevent the elastic rubber layer 24 from being easily damaged when the elliptical top ball of hard material directly hits it. Before the start of work, the airbag 27 is inflated until it is nearly full of air; 40-50 micron silicon powder is poured into the body of the activation equipment from the feed port, and the reduction motor 22 is started to rotate the rotating rod, that is, to drive the ring to rotate, and the sprocket chain mechanism 30 is started at the same time, so that no manual operation is required. Since the airbag 27 is almost filled with air but not full, and the airbag 27 is fixed on the outside of the elastic rubber skin layer 24, with the start of the sprocket chain mechanism, there will be an intermittent situation where the elliptical top ball 31 presses the airbag 27, and it is the different parts of the airbag 27 that are pressed. In order to ensure that the airbag 27 is always pressed, an elliptical top ball 31 can be fixed on both sides of the chain. When the airbag 27 is pressed by the elliptical top ball 31, the elastic rubber skin layer 24 is pressed against the ring.

[0048] There is no longer any concern about the problem that the distance between the parallel plate and the collar is difficult to control accurately (unlike in Example 3), which may easily cause the pointed object assembly to hit the parallel plate or the distance from the parallel plate is greater than the final required silicon powder particle size, resulting in low mechanical activation efficiency. By setting up an active intermittent "parallel plate" (the elastic rubber layer 24 on both sides of the side plate is equivalent to replacing the "parallel plate" in Example 3), the silicon powder can always hit the inner wall of the body during the falling process in the body, avoiding the problem of poor distance control faced by using a fixed side wall of the body (such as the parallel plate method in Example 3). It also reduces the accuracy requirements for installation. And the entire process does not require human participation, which reduces dependence on labor and reduces production costs.

[0049] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A self-propagating low-temperature combustion preparation process for high-fluidity spherical silicon powder, characterized in that: It consists of the following process steps performed in sequence: The silicon powder is pretreated and fed into a suspension combustion furnace at a temperature of 1000°C through a first screw feeder to undergo a self-propagating low-temperature combustion reaction in an air atmosphere; after cooling, the high-fluidity spherical silicon powder is collected; During the self-propagating low-temperature combustion reaction, the air flow rate is maintained at 20L / min; the pretreatment process is to activate the silicon powder through an activation device; a screen is provided at the outlet of the activation device; a second screw feeder is provided at the rear of the discharge direction of the outlet of the activation device, a collecting pipe is provided at the outlet of the second screw feeder, a collecting tank is provided at the rear of the discharge direction of the collecting pipe, a fine activated silicon powder collection port is provided between the outlet and the second screw feeder, and a plug is provided on the fine activated silicon powder collection port; the second screw feeder is the same as the first screw feeder; The activation equipment is a vibrating ball mill, and the mesh size of the mesh is 30-35 microns; a circulation pipeline connected to the inner cavity of the vibrating ball mill is arranged on the body of the vibrating ball mill to re-introduce silicon powder larger than 35 microns into the activation equipment for further activation, and the circulation pipeline is located in front of the mesh along the discharge direction; The particle size of the silicon powder before pretreatment is 40-50 microns; When the second screw feeder is blocked during pretreatment, the activated silicon powder that is not of small particle size in the collection tank is transferred to the barrel; at the same time, the activation equipment and the circulation pump on the circulation pipeline are stopped, and the plug is pulled out to collect the fine activated silicon powder for subsequent screening and grading.

2. The self-propagating low-temperature combustion preparation process of high-fluidity spherical silicon powder according to claim 1 is characterized in that: After the silicon powder is pretreated, the pretreated silicon powder is first transferred from the collection tank to the barrel, and the silicon powder in the barrel is then fed to the first screw feeder, and the first screw feeder feeds to the bottom of the suspension combustion furnace; while feeding to the suspension combustion furnace, preheated air is also introduced into the suspension combustion furnace to ensure that the silicon powder is in a suspended state in the suspension combustion furnace; after the silicon powder reacts in the suspension combustion furnace, it is discharged from the air outlet above the suspension combustion furnace, and then separated in a cyclone dust collector to obtain high-fluidity spherical silicon micropowder.

3. The self-propagating low-temperature combustion preparation process of high-fluidity spherical silicon powder according to claim 1 is characterized in that: When the silicon powder in the barrel reaches the feed amount of the suspension combustion furnace, the suspension combustion furnace starts working, and the circulation pump on the circulation pipeline starts working at the same time.

4. The self-propagating low-temperature combustion preparation process of high-fluidity spherical silicon powder according to claim 2 is characterized in that: After collecting the fine activated silicon powder between the outlet and the second screw feeder, restart the suspension combustion furnace and the circulation pump on the circulation pipeline to continue pre-treating the remaining silicon powder; Alternatively, silicon powder is added to the activation device to continue pretreatment until the amount of activated silicon powder that is not of small particle size in the collection tank reaches the feed amount of the suspension combustion furnace.