Defluorination method for high-purity niobium hydroxide
By adjusting the neutralization, precipitation, cooling, pressing and washing steps in the defluoridation process of high-purity niobium hydroxide, and using normal temperature cooling water and dilute ammonia water, the problem of water and energy consumption in the defluoridation process of high-purity niobium hydroxide was solved and the water and energy consumption was achieved. consumption savings and improvement in fluoride reduction efficiency.
Patent Information
- Application Number
- CN202410779481.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-11
AI Technical Summary
The existing high-purity niobium hydroxide fluoride reduction process consumes a large amount of water, resulting in sewage production and increased energy consumption. It is necessary to develop a water-saving fluoride reduction method to reduce production costs.
A high-purity niobium hydroxide defluoridation method is adopted. Through the steps of neutralization and precipitation, cooling, pressing, air blowing and washing, normal temperature cooling water and dilute ammonia water are used for treatment, and the process flow is adjusted to reduce water and energy consumption.
It reduces the water consumption of niobium oxide per ton products, reduces the generation of sewage, reduces the energy consumption in the cooling and pulping and washing processes, and shortens the fluoride reduction time.
Smart Images

Figure CN118754200A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of defluorination of niobium hydroxide, and in particular to a method for defluorination of high-purity niobium hydroxide. Background Art
[0002] High-purity niobium hydroxide is an intermediate product for the preparation of high-purity niobium oxide. Ordinary fluoroniobic acid solution is extracted with 2-octanol to obtain high-purity fluoroniobic acid solution. A certain amount of ammonia is added to the high-purity fluoroniobic acid solution to generate high-purity niobium hydroxide slurry. After filter pressing, the fluorine content of the high-purity niobium hydroxide filter cake is about 8% to 15%, which cannot be directly used as a subsequent calcination feed. It needs to be washed to reduce the fluorine content before it can finally become a qualified high-purity niobium hydroxide containing fluorine for calcination into high-purity niobium oxide.
[0003] Chinese invention patent application CN103936072B, "A process for producing crystalline high-purity niobium oxide by directly using decomposition supernatant", discloses a process for producing crystalline high-purity niobium oxide by directly using supernatant, and the amount of pure water used for washing is 60-80 liters / kgNb2O5. Chinese invention patent application CN104445407B, "A method for preparing granular niobium oxide and granular niobium oxide prepared therefrom", discloses a method for preparing granular niobium oxide, and in the step of washing and defluorination, the filter cake is washed and defluorinated with 60-70°C ammonia-containing pure water.
[0004] The water consumption for defluorination of high-purity niobium hydroxide is 60 to 80 cubic meters per ton of product. In order to reduce the wastewater generated in the defluorination process of high-purity niobium hydroxide, it is necessary to develop a method with good defluorination effect and water saving, so as to reduce the water consumption in the washing stage of producing high-purity niobium hydroxide, thereby reducing the cost of producing high-purity niobium hydroxide. Summary of the invention
[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a method for removing fluorine from high-purity niobium hydroxide.
[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0007] A method for removing fluorine from high-purity niobium hydroxide comprises the following steps:
[0008] S1, the first stage of neutralization precipitation, pumping X liters of high-purity fluoroniobic acid solution with a niobium oxide concentration of 150-155 g / L and an acidity of 5-5.5 N into the two neutralization precipitation tanks, respectively, turning on the first agitator of the neutralization precipitation tank for stirring, setting the feed liquid temperature of each of the two neutralization precipitation tanks to be lower than 102-104 ° C, intermittently passing normal temperature cooling water into the cooling water rings of the two neutralization precipitation tanks, and passing a flow rate of 115-125 Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 6, and then the ammonia gas is stopped;
[0009] S2, the first cooling, the first agitator of the neutralization sedimentation tank continues to stir, and the room temperature cooling water with a flow rate of 5-20L / min is respectively passed into the cooling water rings of the two neutralization sedimentation tanks until the temperature of the feed liquid in each of the two neutralization sedimentation tanks drops to 50-60°C, and the room temperature cooling water is stopped;
[0010] S3, the second stage of neutralization and precipitation, the first agitator of the neutralization precipitation tank continues to stir, the temperature of the feed liquid in each of the two neutralization precipitation tanks is set to be lower than 90-95°C, and the cooling water rings of the two neutralization precipitation tanks are intermittently introduced into the cooling water rings of the two neutralization precipitation tanks, and the flow rate of the two neutralization precipitation tanks is 80-110Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 10, and then the ammonia gas is stopped;
[0011] S4, the second cooling, the first agitator of the neutralization precipitation tank continues to stir, and the room temperature cooling water with a flow rate of 5-20L / min is respectively passed into the cooling water rings of the two neutralization precipitation tanks until the temperature of the feed liquid in each of the two neutralization precipitation tanks drops to 70-75°C, and the room temperature cooling water is stopped;
[0012] S5, the first squeezing and the first air blowing, using a pump to pump the liquid in the two neutralization and sedimentation tanks into a chamber type diaphragm filter press, controlling the chamber type diaphragm filter press to perform the first squeezing, and then controlling the chamber type diaphragm filter press to perform the first air blowing;
[0013] S6, first slurrying, preparing 1X to 1.034X liters of dilute ammonia water A at room temperature in two slurrying tanks respectively, placing the high-purity niobium hydroxide filter cake in the chamber diaphragm filter press after the first air blowing into the two slurrying tanks respectively, turning on the second agitator of the slurrying tank to stir the high-purity niobium hydroxide filter cake and dilute ammonia water A at room temperature in the slurrying tank to obtain high-purity niobium hydroxide slurry;
[0014] S7, first washing, pumping the high-purity niobium hydroxide slurry prepared for the first time in the two slurry making tanks into the chamber diaphragm filter press with a pump, preparing 2.6X to 2.687X liters of normal temperature dilute ammonia water B in each of the two washing tanks, and each time using the normal temperature dilute ammonia water B in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the first washing;
[0015] S8, second squeezing and second air blowing, controlling the chamber type diaphragm filter press to perform the second squeezing at a pressure of 0.4 MPa, and then controlling the chamber type diaphragm filter press to perform the second air blowing;
[0016] S9, second slurrying, preparing 1X to 1.034X liters of dilute ammonia water A at room temperature in two slurrying tanks respectively, placing the high-purity niobium hydroxide filter cake in the chamber diaphragm filter press after the second air blowing into the two slurrying tanks respectively, turning on the second agitator of the slurrying tank to stir the high-purity niobium hydroxide filter cake and dilute ammonia water A at room temperature in the slurrying tank to obtain high-purity niobium hydroxide slurry;
[0017] S10, second washing, pumping the high-purity niobium hydroxide slurry obtained in the two slurry making tanks into the chamber diaphragm filter press by pumping, respectively preparing 2.6X to 2.687X liters of normal temperature dilute ammonia water B in two washing tanks, and each time using the normal temperature dilute ammonia water B in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the second washing;
[0018] S11, the third pressing, controlling the chamber type diaphragm filter press to perform the third pressing;
[0019] S12, washing for the third time, using 1.15X to 1.25X liters of high-purity water at room temperature to circulate and wash the high-purity niobium hydroxide cake formed by the third squeezing in the chamber-type diaphragm filter press for the third time;
[0020] S13, the fourth pressing, controlling the chamber type diaphragm filter press to perform the fourth pressing.
[0021] Wherein, the temperature of the normal temperature cooling water is 20-30°C.
[0022] The room temperature dilute ammonia water A is prepared by mixing room temperature ammonia water with a mass fraction of 25% and room temperature high purity water in a ratio of 1:19.
[0023] The room temperature dilute ammonia water B is prepared by adding ammonia gas from a purification tank into room temperature high purity water, and the concentration of the room temperature dilute ammonia water B is 1 mol / L.
[0024] Among them, the first pressing time is 10 minutes, the first air blowing time is 10 minutes, the second pressing time is 10 minutes, the second air blowing time is 10 minutes, the third pressing time is 10 minutes, the fourth pressing time is 25 minutes, the first washing time is 60 minutes, the second washing time is 60 minutes, the third washing time is 40 minutes, the stirring time during the first pulping is 40 minutes, and the stirring time during the second pulping is 40 minutes.
[0025] Among them, the pressure of the first pressing is 0.5Mpa, the pressure of the first air blowing is 0.45Mpa, the pressure of the second pressing is 0.4Mpa, the pressure of the second air blowing is 0.35Mpa, the pressure of the third pressing is 0.6Mpa, and the pressure of the fourth pressing is 0.8Mpa.
[0026] Wherein, the first agitator of the neutralization sedimentation tank stirs at a frequency of 35HZ, and the second agitator of the pulping tank stirs at a frequency of 35HZ.
[0027] Among them, the neutralization sedimentation tank includes a conical steel-lined plastic tank with a diameter of 1.8 meters and a height of 3 meters. The conical steel-lined plastic tank is equipped with a first agitator, a radar level meter, a thermometer and a PH test probe. The first agitator adopts a first double-blade stirring paddle. The outer wall of the neutralization sedimentation tank is provided with a cooling water ring sleeve that is close to the outer wall of the neutralization sedimentation tank. The cooling water ring sleeve is welded with PVC plastic with a thickness of 0.5 cm. The ring distance of the cooling water ring sleeve is 5 cm and the height is 2 meters.
[0028] Among them, a spiral sawtooth crushing device is installed at the entrance of the high-purity niobium hydroxide filter cake of the slurry tank, and the spiral sawtooth crushing device includes a driving motor, a rotating shaft, and two parallel seat bearings. The two ends of the rotating shaft are respectively interference-mounted in the bearing inner rings of the seat bearings, one end of the rotating shaft is connected to the motor shaft of the driving motor through a coupling, and a plurality of saw teeth arranged in a spiral shape are fixedly connected to the middle part of the rotating shaft.
[0029] The pulping tank is equipped with three vertical baffles. The second agitator of the pulping tank adopts a second double-blade stirring paddle. The blade inclination angle of the second double-blade stirring paddle is 5-10°. The volume of the pulping tank is 16m 3 .
[0030] The beneficial effects of the present invention are as follows: the method for defluorinating high-purity niobium hydroxide reduces the water consumption per ton of niobium hydroxide product, thereby reducing the sewage generated in the process of defluorinating high-purity niobium hydroxide; normal temperature cooling water is used for cooling, and there is no need to cool the normal temperature cooling water, thereby reducing the energy consumption of the cooling process; normal temperature dilute ammonia water is used without the need for additional heating, thereby reducing the energy consumption of the pulping and washing processes; and the defluorinating time is shortened by adjusting the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0032] Figure 1 This is a flow chart of the method for removing fluorine from high-purity niobium hydroxide in Example 1 of the present invention;
[0033] Figure 2 It is a structural schematic diagram of the neutralization sedimentation tank in the present invention;
[0034] Explanation of the reference numerals in the figure: neutralization sedimentation tank 1, first agitator 2, radar level meter 3, thermometer 4, PH test probe 5, cooling water ring 6. DETAILED DESCRIPTION
[0035] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments.
[0036] like Figure 1 The embodiment 1 shown is a method for removing fluorine from high-purity niobium hydroxide, comprising the following steps:
[0037] S1, the first stage of neutralization precipitation, pump 4927 liters of high-purity fluoroniobic acid solution with a niobium oxide concentration of 151.6 g / L and an acidity of 5.2N into the two neutralization precipitation tanks respectively, start the first agitator of the neutralization precipitation tank to stir at a frequency of 35HZ, set the feed liquid temperature of each of the two neutralization precipitation tanks to be lower than 102°C, intermittently pass normal temperature cooling water into the cooling water rings of the two neutralization precipitation tanks, and pass 120Nm3 of cooling water into the two neutralization precipitation tanks respectively. 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 6, and then the ammonia gas is stopped;
[0038] S2, the first cooling, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, and the normal temperature cooling water with a flow rate of 10L / min is passed into the cooling water rings of the two neutralization precipitation tanks respectively until the temperature of the feed liquid in each of the two neutralization precipitation tanks drops to 50°C, and the normal temperature cooling water is stopped;
[0039] S3, the second stage of neutralization and precipitation, the first agitator of the neutralization and precipitation tank continues to stir at a frequency of 35HZ, the temperature of the feed liquid in each of the two neutralization and precipitation tanks is set to be lower than 95°C, and the cooling water rings of the two neutralization and precipitation tanks are intermittently introduced into the cooling water rings of the two neutralization and precipitation tanks, and the flow rate of 80Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 10, and then the ammonia gas is stopped;
[0040] S4, the second cooling, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, and the room temperature cooling water with a flow rate of 10L / min is respectively passed into the cooling water rings of the two neutralization precipitation tanks until the temperature of the feed liquid in each of the two neutralization precipitation tanks drops to 70°C and the room temperature cooling water is stopped;
[0041] S5, the first pressing and the first air blowing, the liquid in the two neutralization and sedimentation tanks is pumped into a chamber diaphragm filter press by a pump, the chamber diaphragm filter press is controlled to perform the first pressing, and then the chamber diaphragm filter press is controlled to perform the first air blowing, the pressure of the first pressing is 0.5Mpa, the pressure of the first air blowing is 0.45Mpa, the time of the first pressing is 10 minutes, and the time of the first air blowing is 10 minutes;
[0042] S6. First slurrying: 5000 liters of dilute ammonia water A at room temperature are prepared in two slurrying tanks respectively, and the high-purity niobium hydroxide filter cake in the chamber diaphragm filter press after the first air blowing is placed in the two slurrying tanks respectively, and the second agitator of the slurrying tank is turned on to stir the high-purity niobium hydroxide filter cake and dilute ammonia water A at room temperature in the slurrying tank at a frequency of 35 Hz to obtain high-purity niobium hydroxide slurry. The stirring time for the first slurrying is 40 minutes;
[0043] S7, first washing, pump the high-purity niobium hydroxide slurry prepared in the two slurry making tanks into the chamber diaphragm filter press by pumping, prepare 13,000 liters of dilute ammonia water B at room temperature in each of the two washing tanks, and use the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the first washing each time, and the first washing time is 60 minutes;
[0044] S8, second pressing and second air blowing, controlling the chamber diaphragm filter press to perform the second pressing at a pressure of 0.4 MPa, and then controlling the chamber diaphragm filter press to perform the second air blowing, the pressure of the second pressing is 0.4 MPa, the pressure of the second air blowing is 0.35 MPa, the second pressing time is 10 minutes, and the second air blowing time is 10 minutes;
[0045] S9, second pulping, prepare 5000 liters of room temperature dilute ammonia water A in each of the two pulping tanks, put the high purity niobium hydroxide filter cake in the chamber diaphragm filter press after the second air blowing into the two pulping tanks respectively, start the second agitator of the pulping tank to stir the high purity niobium hydroxide filter cake and room temperature dilute ammonia water A in the pulping tank at a frequency of 35HZ to obtain high purity niobium hydroxide slurry, and the stirring time during the second pulping is 40 minutes;
[0046] S10, second washing, pumping the high-purity niobium hydroxide slurry obtained in the two slurry making tanks into the chamber diaphragm filter press by pumping, respectively preparing 13,000 liters of dilute ammonia water B at room temperature in the two washing tanks, and each time using the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the second washing, the second washing time is 60 minutes;
[0047] S11, the third pressing, controlling the chamber type diaphragm filter press to perform the third pressing, the pressure of the third pressing is 0.6Mpa, and the third pressing time is 10 minutes;
[0048] S12, third washing, using 6000 liters of high-purity water at room temperature to circulate and wash the high-purity niobium hydroxide cake formed by the third squeezing in the chamber diaphragm filter press for a third time, and the third washing time is 40 minutes;
[0049] S13, the fourth pressing, controlling the chamber-type diaphragm filter press to perform the fourth pressing, the pressure of the fourth pressing is 0.8 MPa, and the fourth pressing time is 25 minutes.
[0050] After the fourth pressing, the high-purity niobium hydroxide filter cake was unloaded from the chamber diaphragm filter press. Sampling and analysis showed that the high-purity niobium hydroxide filter cake in Example 1 contained 58.2% niobium oxide and 0.17% fluorine.
[0051] The physical particle abundance analysis of the high-purity niobium hydroxide filter cake in Example 1 was performed using a laser particle size analyzer, and the results showed that D10 = 1.51 μm, D25 = 4.13 μm, D50 = 10.46 μm, D75 = 17.42 μm, and D90 = 24.12 μm.
[0052] The amount of high-purity water used in Example 1 is 4×13+2×10+6=78m 3 The amount of niobium oxide in the high-purity fluoroniobate solution is 1.5 tons, and the amount of water used for defluorination per ton of high-purity niobium oxide is 78 / 1.5=52m 3 .
[0053] Example 2, a method for removing fluorine from high-purity niobium hydroxide, comprising the following steps:
[0054] S1, the first stage of neutralization precipitation, pump 4896 liters of high-purity fluoroniobic acid solution with a niobium oxide concentration of 153.2 g / L and an acidity of 5.3N into the two neutralization precipitation tanks respectively, start the first agitator of the neutralization precipitation tank to stir at a frequency of 35HZ, set the feed liquid temperature of each of the two neutralization precipitation tanks to be lower than 103°C, and intermittently pass normal temperature cooling water into the cooling water rings of the two neutralization precipitation tanks, and pass 120Nm3 of cooling water into the two neutralization precipitation tanks respectively. 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 6, and then the ammonia gas is stopped;
[0055] S2, the first cooling, the first agitator of the neutralization sedimentation tank continues to stir at a frequency of 35HZ, and the normal temperature cooling water with a flow rate of 10L / min is respectively introduced into the cooling water rings of the two neutralization sedimentation tanks until the temperature of the feed liquid in each of the two neutralization sedimentation tanks drops to 54°C, and the normal temperature cooling water is stopped;
[0056] S3, the second stage of neutralization and precipitation, the first agitator of the neutralization and precipitation tank continues to stir at a frequency of 35HZ, the temperature of the feed liquid in each of the two neutralization and precipitation tanks is set to be lower than 95°C, and the cooling water rings of the two neutralization and precipitation tanks are intermittently introduced into the cooling water rings of the two neutralization and precipitation tanks, and the flow rate of 100Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 10, and then the ammonia gas is stopped;
[0057] S4, the second cooling, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, and the normal temperature cooling water with a flow rate of 10L / min is respectively introduced into the cooling water rings of the two neutralization precipitation tanks until the temperature of the feed liquid in each of the two neutralization precipitation tanks drops to 72°C, and the normal temperature cooling water is stopped;
[0058] S5, the first pressing and the first air blowing, the liquid in the two neutralization and sedimentation tanks is pumped into a chamber diaphragm filter press by a pump, the chamber diaphragm filter press is controlled to perform the first pressing, and then the chamber diaphragm filter press is controlled to perform the first air blowing, the pressure of the first pressing is 0.5Mpa, the pressure of the first air blowing is 0.45Mpa, the time of the first pressing is 10 minutes, and the time of the first air blowing is 10 minutes;
[0059] S6. First slurrying: 5000 liters of dilute ammonia water A at room temperature are prepared in two slurrying tanks respectively, and the high-purity niobium hydroxide filter cake in the chamber diaphragm filter press after the first air blowing is placed in the two slurrying tanks respectively, and the second agitator of the slurrying tank is turned on to stir the high-purity niobium hydroxide filter cake and dilute ammonia water A at room temperature in the slurrying tank at a frequency of 35 Hz to obtain high-purity niobium hydroxide slurry. The stirring time for the first slurrying is 40 minutes;
[0060] S7, first washing, pump the high-purity niobium hydroxide slurry prepared in the two slurry making tanks into the chamber diaphragm filter press by pumping, prepare 13,000 liters of dilute ammonia water B at room temperature in each of the two washing tanks, and use the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the first washing each time, and the first washing time is 60 minutes;
[0061] S8, second pressing and second air blowing, controlling the chamber diaphragm filter press to perform the second pressing at a pressure of 0.4 MPa, and then controlling the chamber diaphragm filter press to perform the second air blowing, the pressure of the second pressing is 0.4 MPa, the pressure of the second air blowing is 0.35 MPa, the second pressing time is 10 minutes, and the second air blowing time is 10 minutes;
[0062] S9, second pulping, prepare 5000 liters of room temperature dilute ammonia water A in each of the two pulping tanks, put the high purity niobium hydroxide filter cake in the chamber diaphragm filter press after the second air blowing into the two pulping tanks respectively, start the second agitator of the pulping tank to stir the high purity niobium hydroxide filter cake and room temperature dilute ammonia water A in the pulping tank at a frequency of 35HZ to obtain high purity niobium hydroxide slurry, and the stirring time during the second pulping is 40 minutes;
[0063] S10, second washing, pumping the high-purity niobium hydroxide slurry obtained in the two slurry making tanks into the chamber diaphragm filter press by pumping, respectively preparing 13,000 liters of dilute ammonia water B at room temperature in the two washing tanks, and each time using the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the second washing, the second washing time is 60 minutes;
[0064] S11, the third pressing, controlling the chamber type diaphragm filter press to perform the third pressing, the pressure of the third pressing is 0.6Mpa, and the third pressing time is 10 minutes;
[0065] S12, third washing, using 6000 liters of high-purity water at room temperature to circulate and wash the high-purity niobium hydroxide cake formed by the third squeezing in the chamber diaphragm filter press for a third time, and the third washing time is 40 minutes;
[0066] S13, the fourth pressing, controlling the chamber-type diaphragm filter press to perform the fourth pressing, the pressure of the fourth pressing is 0.8 MPa, and the fourth pressing time is 25 minutes.
[0067] After the fourth pressing, the high-purity niobium hydroxide filter cake was unloaded from the chamber diaphragm filter press. Sampling and analysis showed that the high-purity niobium hydroxide filter cake in Example 2 contained 59.6% niobium oxide and 0.18% fluorine.
[0068] The physical particle abundance analysis of the high-purity niobium hydroxide filter cake in Example 2 was performed using a laser particle size analyzer, and the results showed that D10 = 2.68 μm, D25 = 5.71 μm, D50 = 12.68 μm, D75 = 18.95 μm, and D90 = 25.14 μm.
[0069] The amount of high-purity water used in Example 2 is 4×13+2×10+6=78m 3 The amount of niobium oxide in the high-purity fluoroniobate solution is 1.5 tons, and the amount of water used for defluorination per ton of high-purity niobium oxide is 78 / 1.5=52m 3 .
[0070] Example 3, a method for removing fluorine from high-purity niobium hydroxide, comprising the following steps:
[0071] S1, the first stage of neutralization precipitation, pump 4867 liters of high-purity fluoroniobic acid solution with a niobium oxide concentration of 154.1 g / L and an acidity of 5.3N into the two neutralization precipitation tanks respectively, start the first agitator of the neutralization precipitation tank to stir at a frequency of 35HZ, set the feed liquid temperature of each of the two neutralization precipitation tanks to be lower than 104°C, and intermittently pass normal temperature cooling water into the cooling water rings of the two neutralization precipitation tanks, and pass a flow rate of 120Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 6, and then the ammonia gas is stopped;
[0072] S2, first cooling, the first agitator of the neutralization sedimentation tank continues to stir at a frequency of 35HZ, and the normal temperature cooling water with a flow rate of 10L / min is passed into the cooling water rings of the two neutralization sedimentation tanks respectively until the temperature of the feed liquid in each of the two neutralization sedimentation tanks drops to 52°C, and the normal temperature cooling water is stopped;
[0073] S3, the second stage of neutralization precipitation, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, the temperature of the feed liquid in each of the two neutralization precipitation tanks is set to be lower than 95°C, and the cooling water rings of the two neutralization precipitation tanks are intermittently introduced into the cooling water rings of the two neutralization precipitation tanks, and the flow rate of 110Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 10, and then the ammonia gas is stopped;
[0074] S4, the second cooling, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, and the room temperature cooling water with a flow rate of 10L / min is respectively passed into the cooling water rings of the two neutralization precipitation tanks until the temperature of the feed liquid in each of the two neutralization precipitation tanks drops to 75°C and the room temperature cooling water is stopped;
[0075] S5, the first pressing and the first air blowing, the liquid in the two neutralization and sedimentation tanks is pumped into a chamber diaphragm filter press by a pump, the chamber diaphragm filter press is controlled to perform the first pressing, and then the chamber diaphragm filter press is controlled to perform the first air blowing, the pressure of the first pressing is 0.5Mpa, the pressure of the first air blowing is 0.45Mpa, the time of the first pressing is 10 minutes, and the time of the first air blowing is 10 minutes;
[0076] S6. First slurrying: 5000 liters of dilute ammonia water A at room temperature are prepared in two slurrying tanks respectively, and the high-purity niobium hydroxide filter cake in the chamber diaphragm filter press after the first air blowing is placed in the two slurrying tanks respectively, and the second agitator of the slurrying tank is turned on to stir the high-purity niobium hydroxide filter cake and dilute ammonia water A at room temperature in the slurrying tank at a frequency of 35 Hz to obtain high-purity niobium hydroxide slurry. The stirring time for the first slurrying is 40 minutes;
[0077] S7, first washing, pump the high-purity niobium hydroxide slurry prepared in the two slurry making tanks into the chamber diaphragm filter press by pumping, prepare 13,000 liters of dilute ammonia water B at room temperature in each of the two washing tanks, and use the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the first washing each time, and the first washing time is 60 minutes;
[0078] S8, second pressing and second air blowing, controlling the chamber diaphragm filter press to perform the second pressing at a pressure of 0.4 MPa, and then controlling the chamber diaphragm filter press to perform the second air blowing, the pressure of the second pressing is 0.4 MPa, the pressure of the second air blowing is 0.35 MPa, the second pressing time is 10 minutes, and the second air blowing time is 10 minutes;
[0079] S9, second pulping, prepare 5000 liters of room temperature dilute ammonia water A in each of the two pulping tanks, put the high purity niobium hydroxide filter cake in the chamber diaphragm filter press after the second air blowing into the two pulping tanks respectively, start the second agitator of the pulping tank to stir the high purity niobium hydroxide filter cake and room temperature dilute ammonia water A in the pulping tank at a frequency of 35HZ to obtain high purity niobium hydroxide slurry, and the stirring time during the second pulping is 40 minutes;
[0080] S10, second washing, pumping the high-purity niobium hydroxide slurry obtained in the two slurry making tanks into the chamber diaphragm filter press by pumping, respectively preparing 13,000 liters of dilute ammonia water B at room temperature in the two washing tanks, and each time using the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the second washing, the second washing time is 60 minutes;
[0081] S11, the third pressing, controlling the chamber type diaphragm filter press to perform the third pressing, the pressure of the third pressing is 0.6Mpa, and the third pressing time is 10 minutes;
[0082] S12, third washing, using 6000 liters of high-purity water at room temperature to circulate and wash the high-purity niobium hydroxide cake formed by the third squeezing in the chamber diaphragm filter press for a third time, and the third washing time is 40 minutes;
[0083] S13, the fourth pressing, controlling the chamber-type diaphragm filter press to perform the fourth pressing, the pressure of the fourth pressing is 0.8 MPa, and the fourth pressing time is 25 minutes.
[0084] After the fourth pressing, the high-purity niobium hydroxide filter cake was unloaded from the chamber diaphragm filter press. Sampling and analysis showed that the high-purity niobium hydroxide filter cake in Example 3 contained 57.5% niobium oxide and 0.19% fluorine.
[0085] The physical particle abundance analysis of the high-purity niobium hydroxide filter cake in Example 3 was performed using a laser particle size analyzer, and the results showed that D10 = 1.77 μm, D25 = 4.85 μm, D50 = 11.83 μm, D75 = 18.25 μm, and D90 = 25.37 μm.
[0086] The amount of high-purity water used in Example 3 is 4×13+2×10+6=78m 3 The amount of niobium oxide in the high-purity fluoroniobate solution is 1.5 tons, and the amount of water used for defluorination per ton of high-purity niobium oxide is 78 / 1.5=52m 3 .
[0087] Comparative Example 1, a method for removing fluorine from high-purity niobium hydroxide, comprising the following steps:
[0088] S1, the first stage of neutralization precipitation, pump 4964 liters of high-purity fluoroniobic acid solution with a niobium oxide concentration of 151.1 g / L and an acidity of 5.1N into the two neutralization precipitation tanks respectively, start the first agitator of the neutralization precipitation tank to stir at a frequency of 35HZ, set the feed liquid temperature of each of the two neutralization precipitation tanks to be lower than 102°C, and intermittently pass normal temperature cooling water into the cooling water rings of the two neutralization precipitation tanks, and pass 120Nm3 of cooling water into the two neutralization precipitation tanks respectively. 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 6, and then the ammonia gas is stopped;
[0089] S2, the first cooling, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, and the normal temperature cooling water with a flow rate of 10L / min is passed into the cooling water rings of the two neutralization precipitation tanks respectively until the temperature of the feed liquid in each of the two neutralization precipitation tanks drops to 53°C, and the normal temperature cooling water is stopped;
[0090] S3, the second stage of neutralization precipitation, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, the temperature of the feed liquid in each of the two neutralization precipitation tanks is set to be lower than 95°C, and the cooling water rings of the two neutralization precipitation tanks are intermittently introduced into the cooling water rings of the two neutralization precipitation tanks, and the flow rate of 130Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 10, and then the ammonia gas is stopped;
[0091] S4, the second cooling, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, and the room temperature cooling water with a flow rate of 10L / min is respectively passed into the cooling water rings of the two neutralization precipitation tanks until the temperature of the feed liquid in each of the two neutralization precipitation tanks drops to 70°C and the room temperature cooling water is stopped;
[0092] S5, the first pressing and the first air blowing, the liquid in the two neutralization and sedimentation tanks is pumped into a chamber diaphragm filter press by a pump, the chamber diaphragm filter press is controlled to perform the first pressing, and then the chamber diaphragm filter press is controlled to perform the first air blowing, the pressure of the first pressing is 0.5Mpa, the pressure of the first air blowing is 0.45Mpa, the time of the first pressing is 10 minutes, and the time of the first air blowing is 10 minutes;
[0093] S6. First slurrying: 5000 liters of dilute ammonia water A at room temperature are prepared in two slurrying tanks respectively, and the high-purity niobium hydroxide filter cake in the chamber diaphragm filter press after the first air blowing is placed in the two slurrying tanks respectively, and the second agitator of the slurrying tank is turned on to stir the high-purity niobium hydroxide filter cake and dilute ammonia water A at room temperature in the slurrying tank at a frequency of 35 Hz to obtain high-purity niobium hydroxide slurry. The stirring time for the first slurrying is 40 minutes;
[0094] S7, first washing, pump the high-purity niobium hydroxide slurry prepared in the two slurry making tanks into the chamber diaphragm filter press by pumping, prepare 13,000 liters of dilute ammonia water B at room temperature in each of the two washing tanks, and use the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the first washing each time, and the first washing time is 60 minutes;
[0095] S8, second pressing and second air blowing, controlling the chamber diaphragm filter press to perform the second pressing at a pressure of 0.4 MPa, and then controlling the chamber diaphragm filter press to perform the second air blowing, the pressure of the second pressing is 0.4 MPa, the pressure of the second air blowing is 0.35 MPa, the second pressing time is 10 minutes, and the second air blowing time is 10 minutes;
[0096] S9, second pulping, prepare 5000 liters of room temperature dilute ammonia water A in each of the two pulping tanks, put the high purity niobium hydroxide filter cake in the chamber diaphragm filter press after the second air blowing into the two pulping tanks respectively, start the second agitator of the pulping tank to stir the high purity niobium hydroxide filter cake and room temperature dilute ammonia water A in the pulping tank at a frequency of 35HZ to obtain high purity niobium hydroxide slurry, and the stirring time during the second pulping is 40 minutes;
[0097] S10, second washing, pumping the high-purity niobium hydroxide slurry obtained in the two slurry making tanks into the chamber diaphragm filter press by pumping, respectively preparing 13,000 liters of dilute ammonia water B at room temperature in the two washing tanks, and each time using the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the second washing, the second washing time is 60 minutes;
[0098] S11, the third pressing, controlling the chamber type diaphragm filter press to perform the third pressing, the pressure of the third pressing is 0.6Mpa, and the third pressing time is 10 minutes;
[0099] S12, third washing, using 6000 liters of high-purity water at room temperature to circulate and wash the high-purity niobium hydroxide cake formed by the third squeezing in the chamber diaphragm filter press for a third time, and the third washing time is 40 minutes;
[0100] S13, the fourth pressing, controlling the chamber-type diaphragm filter press to perform the fourth pressing, the pressure of the fourth pressing is 0.8 MPa, and the fourth pressing time is 25 minutes.
[0101] After the fourth pressing, the high-purity niobium hydroxide filter cake was unloaded from the chamber diaphragm filter press. Sampling and analysis showed that the high-purity niobium hydroxide filter cake in Comparative Example 1 contained 57.5% niobium oxide and 0.59% fluorine.
[0102] The physical particle abundance analysis of the high-purity niobium hydroxide filter cake in Comparative Example 1 was performed using a laser particle size analyzer, and the results showed that D10 = 3.77 μm, D25 = 6.85 μm, D50 = 15.83 μm, D75 = 23.25 μm, and D90 = 29.37 μm.
[0103] The amount of high-purity water used in Comparative Example 1 is 4×13+2×10+6=78m 3 The amount of niobium oxide in the high-purity fluoroniobate solution is 1.5 tons, and the amount of water used for defluorination per ton of high-purity niobium oxide is 78 / 1.5=52m 3 .
[0104] Comparative Example 2, a method for removing fluorine from high-purity niobium hydroxide, comprising the following steps:
[0105] S1, the first stage of neutralization precipitation, pump 4918 liters of high-purity fluoroniobic acid solution with a niobium oxide concentration of 152.5 g / L and an acidity of 5.1N into the two neutralization precipitation tanks respectively, start the first agitator of the neutralization precipitation tank to stir at a frequency of 35HZ, set the feed liquid temperature of each of the two neutralization precipitation tanks to be lower than 102°C, intermittently pass normal temperature cooling water into the cooling water rings of the two neutralization precipitation tanks, and pass 120Nm3 of cooling water into the two neutralization precipitation tanks respectively. 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 6, and then the ammonia gas is stopped;
[0106] S2, the first cooling, the first agitator of the neutralization sedimentation tank continues to stir at a frequency of 35HZ, and the normal temperature cooling water with a flow rate of 10L / min is respectively introduced into the cooling water rings of the two neutralization sedimentation tanks until the temperature of the feed liquid in each of the two neutralization sedimentation tanks drops to 83°C, and the normal temperature cooling water is stopped;
[0107] S3, the second stage of neutralization precipitation, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, the temperature of the feed liquid in each of the two neutralization precipitation tanks is set to be lower than 95°C, and the cooling water rings of the two neutralization precipitation tanks are intermittently introduced into the cooling water rings of the two neutralization precipitation tanks, and the flow rate of 110Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 10, and then the ammonia gas is stopped;
[0108] S4, the second cooling, the first agitator of the neutralization precipitation tank continues to stir at a frequency of 35HZ, and the room temperature cooling water with a flow rate of 10L / min is respectively passed into the cooling water rings of the two neutralization precipitation tanks until the temperature of the feed liquid in each of the two neutralization precipitation tanks drops to 70°C and the room temperature cooling water is stopped;
[0109] S5, the first pressing and the first air blowing, the liquid in the two neutralization and sedimentation tanks is pumped into a chamber diaphragm filter press by a pump, the chamber diaphragm filter press is controlled to perform the first pressing, and then the chamber diaphragm filter press is controlled to perform the first air blowing, the pressure of the first pressing is 0.5Mpa, the pressure of the first air blowing is 0.45Mpa, the time of the first pressing is 10 minutes, and the time of the first air blowing is 10 minutes;
[0110] S6. First slurrying: 5000 liters of dilute ammonia water A at room temperature are prepared in two slurrying tanks respectively, and the high-purity niobium hydroxide filter cake in the chamber diaphragm filter press after the first air blowing is placed in the two slurrying tanks respectively, and the second agitator of the slurrying tank is turned on to stir the high-purity niobium hydroxide filter cake and dilute ammonia water A at room temperature in the slurrying tank at a frequency of 35 Hz to obtain high-purity niobium hydroxide slurry. The stirring time for the first slurrying is 40 minutes;
[0111] S7, first washing, pump the high-purity niobium hydroxide slurry prepared in the two slurry making tanks into the chamber diaphragm filter press by pumping, prepare 13,000 liters of dilute ammonia water B at room temperature in each of the two washing tanks, and use the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the first washing each time, and the first washing time is 60 minutes;
[0112] S8, second pressing and second air blowing, controlling the chamber diaphragm filter press to perform the second pressing at a pressure of 0.4 MPa, and then controlling the chamber diaphragm filter press to perform the second air blowing, the pressure of the second pressing is 0.4 MPa, the pressure of the second air blowing is 0.35 MPa, the second pressing time is 10 minutes, and the second air blowing time is 10 minutes;
[0113] S9, second pulping, prepare 5000 liters of room temperature dilute ammonia water A in each of the two pulping tanks, put the high purity niobium hydroxide filter cake in the chamber diaphragm filter press after the second air blowing into the two pulping tanks respectively, start the second agitator of the pulping tank to stir the high purity niobium hydroxide filter cake and room temperature dilute ammonia water A in the pulping tank at a frequency of 35HZ to obtain high purity niobium hydroxide slurry, and the stirring time during the second pulping is 40 minutes;
[0114] S10, second washing, pumping the high-purity niobium hydroxide slurry obtained in the two slurry making tanks into the chamber diaphragm filter press by pumping, respectively preparing 13,000 liters of dilute ammonia water B at room temperature in the two washing tanks, and each time using the dilute ammonia water B at room temperature in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the second washing, the second washing time is 60 minutes;
[0115] S11, the third pressing, controlling the chamber type diaphragm filter press to perform the third pressing, the pressure of the third pressing is 0.6Mpa, and the third pressing time is 10 minutes;
[0116] S12, third washing, using 6000 liters of high-purity water at room temperature to circulate and wash the high-purity niobium hydroxide cake formed by the third squeezing in the chamber diaphragm filter press for a third time, and the third washing time is 40 minutes;
[0117] S13, the fourth pressing, controlling the chamber-type diaphragm filter press to perform the fourth pressing, the pressure of the fourth pressing is 0.8 MPa, and the fourth pressing time is 25 minutes.
[0118] After the fourth pressing, the high-purity niobium hydroxide filter cake was unloaded from the chamber diaphragm filter press. Sampling and analysis showed that the high-purity niobium hydroxide filter cake in Comparative Example 2 contained 58.5% niobium oxide and 0.55% fluorine.
[0119] The physical particle abundance analysis of the high-purity niobium hydroxide filter cake in Comparative Example 2 was performed using a laser particle size analyzer, and the results showed that D10 = 3.27 μm, D25 = 6.25 μm, D50 = 15.13 μm, D75 = 22.25 μm, and D90 = 28.37 μm.
[0120] The amount of high-purity water used in Comparative Example 2 is 4×13+2×10+6=78m 3 The amount of niobium oxide in the high-purity fluoroniobate solution is 1.5 tons, and the amount of water used for defluorination per ton of high-purity niobium oxide is 78 / 1.5=52m 3 .
[0121] The ammonia flow rate of the neutralization precipitation in the second stage of Comparative Example 1 and the initial precipitation temperature of the feed liquid of the neutralization precipitation in the second stage of Comparative Example 2 are changed. After the pulping and washing described in Examples 1 to 3, the high-purity niobium hydroxide filter cake obtained has a relatively high fluorine content. Therefore, the washing effect of Comparative Examples 1 and Comparative Examples 2 is not as good as that of Examples 1 to 3. The reason may be closely related to the ammonia flow rate of the neutralization precipitation in the second stage and the initial feed liquid temperature of the neutralization precipitation in the second stage. The neutralization precipitation process in the second stage is the main process for the formation of high-purity niobium hydroxide particles. In this process, the changes in the ammonia flow rate and the feed liquid temperature have a great influence on the size of the particles, and the size of the high-purity niobium hydroxide particles will directly affect the effect of the fluorine reduction process, which is fed back to the amount of high-purity water used.
[0122] In the above three embodiments and two comparative examples, the temperature of the room temperature cooling water is 20-30°C. Room temperature dilute ammonia water A is prepared by mixing room temperature ammonia water with a mass fraction of 25% and room temperature high purity water in a ratio of 1:19. Room temperature dilute ammonia water B is prepared by adding ammonia gas from a purification tank to room temperature high purity water, and the concentration of room temperature dilute ammonia water B is 1 mol / L.
[0123] In the above three embodiments and two comparative examples, the model of the chamber-type membrane filter press is XAYZGM150 / 1250-UK.
[0124] The use of high-purity niobium hydroxide defluorination method can reduce the water consumption per ton of niobium oxide product to 45-55m3. 3 , which is about 30% lower than before.
[0125] In the above three embodiments, the defluorination time for 1.5 tons of niobium oxide is reduced from 3 days to 2 days, which is 33% shorter than the original time.
[0126] like Figure 2 As shown, the neutralization sedimentation tank 1 includes a conical steel-lined plastic tank with a diameter of 1.8 meters and a height of 3 meters. The conical steel-lined plastic tank is equipped with a first agitator 2, a radar level meter 3, a thermometer 4 and a PH test probe 5. The first agitator 2 adopts a first double-layer blade stirring paddle. The outer wall of the neutralization sedimentation tank is provided with a cooling water ring 6 that is close to the outer wall of the neutralization sedimentation tank. The cooling water ring 6 is welded with PVC plastic with a thickness of 0.5 cm. The ring distance of the cooling water ring is 5 cm and the height is 2 meters.
[0127] A spiral sawtooth crushing device is installed at the entrance of the high-purity niobium hydroxide filter cake of the pulping tank. The spiral sawtooth crushing device includes a driving motor, a rotating shaft, and two parallel seat bearings. The two ends of the rotating shaft are respectively interference-mounted in the inner rings of the seat bearings. One end of the rotating shaft is connected to the motor shaft of the driving motor through a coupling. A number of saw teeth arranged in a spiral shape are fixed to the middle of the rotating shaft.
[0128] Three vertical baffles are installed in the pulping tank. The second agitator of the pulping tank adopts a second double-layer blade stirring paddle. The blade inclination angle of the second double-layer blade stirring paddle is 5-10°. The volume of the pulping tank is 16m 3 .
[0129] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A method for removing fluorine from high-purity niobium hydroxide, characterized in that: The following steps are involved: S1, the first stage of neutralization precipitation, pumping X liters of high-purity fluoroniobic acid solution with a niobium oxide concentration of 150-155 g / L and an acidity of 5-5.5 N into the two neutralization precipitation tanks, respectively, turning on the first agitator of the neutralization precipitation tank for stirring, setting the feed liquid temperature of each of the two neutralization precipitation tanks to be lower than 102-104 ° C, intermittently passing normal temperature cooling water into the cooling water rings of the two neutralization precipitation tanks, and passing a flow rate of 115-125 Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 6, and then the ammonia gas is stopped; S2, the first cooling, the first agitator of the neutralization sedimentation tank continues to stir, and the room temperature cooling water with a flow rate of 5-20L / min is respectively passed into the cooling water rings of the two neutralization sedimentation tanks until the temperature of the feed liquid in each of the two neutralization sedimentation tanks drops to 50-60°C, and the room temperature cooling water is stopped; S3, the second stage of neutralization and precipitation, the first agitator of the neutralization precipitation tank continues to stir, the temperature of the feed liquid in each of the two neutralization precipitation tanks is set to be lower than 90-95°C, and the cooling water rings of the two neutralization precipitation tanks are intermittently introduced into the cooling water rings of the two neutralization precipitation tanks, and the flow rate of the two neutralization precipitation tanks is 80-110Nm 3 / h of ammonia gas until the pH of the feed liquid in the two neutralization and precipitation tanks reaches 10, and then the ammonia gas is stopped; S4, the second cooling, the first agitator of the neutralization precipitation tank continues to stir, and the room temperature cooling water with a flow rate of 5-20L / min is respectively passed into the cooling water rings of the two neutralization precipitation tanks until the temperature of the feed liquid in each of the two neutralization precipitation tanks drops to 70-75°C, and the room temperature cooling water is stopped; S5, the first squeezing and the first air blowing, using a pump to pump the liquid in the two neutralization and sedimentation tanks into a chamber type diaphragm filter press, controlling the chamber type diaphragm filter press to perform the first squeezing, and then controlling the chamber type diaphragm filter press to perform the first air blowing; S6, first slurrying, preparing 1X to 1.034X liters of dilute ammonia water A at room temperature in two slurrying tanks respectively, placing the high-purity niobium hydroxide filter cake in the chamber diaphragm filter press after the first air blowing into the two slurrying tanks respectively, turning on the second agitator of the slurrying tank to stir the high-purity niobium hydroxide filter cake and dilute ammonia water A at room temperature in the slurrying tank to obtain high-purity niobium hydroxide slurry; S7, first washing, pumping the high-purity niobium hydroxide slurry prepared for the first time in the two slurry making tanks into the chamber diaphragm filter press with a pump, preparing 2.6X to 2.687X liters of normal temperature dilute ammonia water B in each of the two washing tanks, and each time using the normal temperature dilute ammonia water B in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the first washing; S8, second squeezing and second air blowing, controlling the chamber type diaphragm filter press to perform the second squeezing at a pressure of 0.4 MPa, and then controlling the chamber type diaphragm filter press to perform the second air blowing; S9, second slurrying, preparing 1X to 1.034X liters of dilute ammonia water A at room temperature in two slurrying tanks respectively, placing the high-purity niobium hydroxide filter cake in the chamber diaphragm filter press after the second air blowing into the two slurrying tanks respectively, turning on the second agitator of the slurrying tank to stir the high-purity niobium hydroxide filter cake and dilute ammonia water A at room temperature in the slurrying tank to obtain high-purity niobium hydroxide slurry; S10, second washing, pumping the high-purity niobium hydroxide slurry obtained in the two slurry making tanks into the chamber diaphragm filter press by pumping, respectively preparing 2.6X to 2.687X liters of normal temperature dilute ammonia water B in two washing tanks, and each time using the normal temperature dilute ammonia water B in one washing tank to circulate the high-purity niobium hydroxide slurry in the chamber diaphragm filter press for the second washing; S11, the third pressing, controlling the chamber type diaphragm filter press to perform the third pressing; S12, washing for the third time, using 1.15X to 1.25X liters of high-purity water at room temperature to circulate and wash the high-purity niobium hydroxide cake formed by the third squeezing in the chamber-type diaphragm filter press for the third time; S13, the fourth pressing, controlling the chamber type diaphragm filter press to perform the fourth pressing.
2. The method for defluorination of high-purity niobium hydroxide according to claim 1, characterized in that: The temperature of the normal temperature cooling water is 20-30°C.
3. The method for defluorination of high-purity niobium hydroxide according to claim 1, characterized in that: The room temperature dilute ammonia water A is prepared by mixing room temperature ammonia water with a mass fraction of 25% and room temperature high purity water in a ratio of 1:
19.
4. The method for defluorination of high-purity niobium hydroxide according to claim 1, characterized in that: The room temperature dilute ammonia water B is prepared by adding ammonia gas from a purification tank into room temperature high purity water and mixing them together. The concentration of the room temperature dilute ammonia water B is 1 mol / L.
5. The method for defluorination of high-purity niobium hydroxide according to claim 1, characterized in that: The first pressing time is 10 minutes, the first air blowing time is 10 minutes, the second pressing time is 10 minutes, the second air blowing time is 10 minutes, the third pressing time is 10 minutes, the fourth pressing time is 25 minutes, the first washing time is 60 minutes, the second washing time is 60 minutes, the third washing time is 40 minutes, the stirring time during the first pulping is 40 minutes, and the stirring time during the second pulping is 40 minutes.
6. The method for defluorination of high-purity niobium hydroxide according to claim 1, characterized in that: The pressure of the first pressing is 0.5Mpa, the pressure of the first air blowing is 0.45Mpa, the pressure of the second pressing is 0.4Mpa, the pressure of the second air blowing is 0.35Mpa, the pressure of the third pressing is 0.6Mpa, and the pressure of the fourth pressing is 0.8Mpa.
7. The method for defluorination of high-purity niobium hydroxide according to claim 1, characterized in that: The first agitator of the neutralization sedimentation tank is stirred at a frequency of 35 Hz, and the second agitator of the pulping tank is stirred at a frequency of 35 Hz.
8. The method for defluorination of high-purity niobium hydroxide according to claim 1, characterized in that: The neutralization sedimentation tank comprises a conical steel-lined plastic tank with a diameter of 1.8 meters and a height of 3 meters. A first agitator, a radar level meter, a thermometer and a PH test probe are installed on the conical steel-lined plastic tank. The first agitator adopts a first double-blade stirring paddle. The outer wall of the neutralization sedimentation tank is provided with a cooling water ring sleeve that is close to the outer wall of the neutralization sedimentation tank. The cooling water ring sleeve is welded with PVC plastic with a thickness of 0.5 cm. The ring distance of the cooling water ring sleeve is 5 cm and the height is 2 meters.
9. The method for defluorination of high-purity niobium hydroxide according to claim 1, characterized in that: A spiral sawtooth crushing device is installed at the entrance of the high-purity niobium hydroxide filter cake of the slurry tank. The spiral sawtooth crushing device includes a driving motor, a rotating shaft, and two parallel seat bearings. The two ends of the rotating shaft are respectively interference-mounted in the inner rings of the seat bearings. One end of the rotating shaft is connected to the motor shaft of the driving motor through a coupling. A plurality of saw teeth arranged in a spiral shape are fixedly connected to the middle of the rotating shaft.
10. The method for defluorination of high-purity niobium hydroxide according to claim 1, characterized in that: The pulping tank is equipped with three vertical baffles. The second agitator of the pulping tank adopts a second double-blade stirring paddle. The blade inclination angle of the second double-blade stirring paddle is 5-10°. The volume of the pulping tank is 16m 3 .