All-solid-waste low-carbon concrete and preparation method thereof

By using materials such as fly ash, slag, silica fume, recycled aggregates and fibers, combined with alkali activator solution soaking and mixing and stirring technology, all solid waste low-carbon concrete is prepared, which solves the energy consumption and environmental damage in the traditional concrete production process. problem, achieving high-strength and low-carbon-emission concrete properties.

CN118754522APending Publication Date: 2024-10-11NORTHWEST ENGINEERING CORPORATION LIMITED

Patent Information

Application Number
CN202410862669.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

High-temperature calcination in the traditional concrete production process leads to increased energy consumption and carbon dioxide emissions, and the mining of natural aggregates leads to environmental damage and resource depletion. The application performance of industrial solid waste and recycled aggregates is difficult to stably control, which limits the use of all-solid waste concrete in the construction industry. Promote applications.

Method used

Using materials such as fly ash, slag, silica fume, recycled aggregates, fibers and alkali activators, all-solid waste low-carbon concrete is prepared by soaking and mixing in alkali activator solutions to improve the strength and durability of concrete and reduce resource consumption. and carbon emissions.

Benefits of technology

It realizes the full utilization of industrial solid waste and aggregates, reduces natural resource mining and carbon emissions, improves the compressive strength and durability of concrete, and meets the construction industry's demand for concrete strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, in particular to all-solid-waste low-carbon concrete and a preparation method thereof. The all-solid-waste low-carbon concrete is prepared from the following components in parts by mass: 150 to 300 parts of fly ash, 15 to 70 parts of silica fume, 150 to 420 parts of slag, 400 to 850 parts of coarse aggregate, 530 to 850 parts of fine aggregate, 7 to 15 parts of water reducing agent, 100 to 351 parts of alkali activator and 0 to 116 parts of fiber, according to the concrete, industrial solid waste and building waste are fully utilized, the full-solid-waste low-carbon concrete meeting the engineering use requirement is prepared, the problems of building waste accumulation and solid waste resource utilization can be solved, and the purpose of low-carbon emission in building material production is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of building materials, and in particular to an all-solid waste low-carbon concrete and a preparation method thereof. Background Art

[0002] With the acceleration of urbanization and the booming construction industry, the demand for concrete, as the most basic building material, is growing. One of the main components of traditional concrete is cement. In the production process of cement, high-temperature calcination is an indispensable step. This process not only consumes a lot of energy, such as coal or natural gas, but also produces a large amount of carbon dioxide emissions during the combustion process. This not only aggravates the global greenhouse effect, but also has a serious negative impact on the environment. Aggregates in traditional concrete mainly come from natural mining, such as river sand, mountain rocks, etc. However, large-scale mining of natural aggregates will not only cause damage to the environment, such as soil erosion, imbalance of the ecosystem, etc., but also with the increase in mining, natural resources are also facing the risk of depletion.

[0003] Currently, industrial solid waste materials and recycled aggregates are being used to replace cement and natural aggregates in traditional concrete. Industrial solid waste materials, such as abandoned slag and fly ash, are not only widely available and inexpensive, but their use can also effectively solve the problem of construction waste and solid waste stacking and reduce the impact on the environment. At the same time, by recycling and utilizing recycled aggregates made from construction waste, waste concrete, etc., it can also reduce the exploitation of natural resources and reduce the risk of resource depletion.

[0004] However, despite the many advantages of the application of industrial solid waste and recycled aggregates, there are still many challenges in the actual application process. Due to the wide range of sources of solid waste, complex composition and large differences, the performance of all-solid waste concrete is difficult to stably control. At the same time, due to the lack of refined and standardized design methods for concrete, the formulation of standards for all-solid waste concrete based on material properties and performance indicators has become particularly difficult. These problems not only limit the promotion and application of all-solid waste concrete in the construction industry, but also hinder the improvement and optimization of its performance. Therefore, how to fully utilize industrial solid waste and recycled aggregates and improve the performance of all-solid waste concrete has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a full-solid waste low-carbon concrete and a preparation method thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides an all-solid waste low-carbon concrete, which includes, by weight, 150 to 300 parts of fly ash, 15 to 70 parts of silica fume, 150 to 420 parts of slag, 400 to 850 parts of coarse aggregate, 530 to 850 parts of fine aggregate, 7 to 15 parts of water reducer, 100 to 351 parts of alkali activator and 0 to 116 parts of fiber.

[0008] Preferably, the coarse aggregate comprises recycled coarse aggregate and geopolymer unburned artificial aggregate.

[0009] Preferably, the recycled coarse aggregate is one or more of discarded concrete blocks, bricks and asphalt.

[0010] Preferably, the cylinder compressive strength of the coarse aggregate is 9MPa to 13Mpa.

[0011] Preferably, the fine aggregate is recycled fine aggregate.

[0012] Preferably, the water reducer is a polycarboxylic acid type high efficiency water reducer.

[0013] Preferably, the alkaline activator comprises sodium silicate, sodium hydroxide and water.

[0014] Preferably, the fibers include steel fibers and PVA fibers.

[0015] In a second aspect, the present invention provides a method for preparing all-solid waste low-carbon concrete, comprising the following steps:

[0016] S1: prepare an alkali activator solution, soak the aggregate in the solution for strengthening, and then take it out;

[0017] S2: After the alkali activator solution is cooled, the fly ash, slag, silica fume, fiber, fine aggregate and alkali activator solution are mixed and stirred evenly;

[0018] S3: Add coarse aggregate to the mixture to form all-solid waste low-carbon concrete.

[0019] Preferably, the method for preparing the alkaline activator solution comprises the following steps:

[0020] The sodium hydroxide solution and the sodium silicate solution are thoroughly mixed to form an alkaline activator solution.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention makes full use of industrial solid waste and aggregates, can save natural mineral resources to the greatest extent, reduce the environmental damage caused by resource exploitation and processing, and reduce carbon dioxide emissions, thereby realizing the resource utilization of bulk solid waste and construction waste; the fiber is used to toughen the all-solid waste concrete, thereby improving the significant brittleness of cementitious materials and recycled aggregates. The 28-day compressive strength of the prepared concrete can reach 40MPa, which can meet the construction industry's demand for concrete strength. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0024] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.

[0025] It should also be understood that the terms used in the present specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the present specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.

[0026] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0027] The first object of the present invention is to provide an all-solid waste low-carbon concrete, which includes, by weight, 150 to 300 parts of fly ash, 15 to 70 parts of silica fume, 150 to 420 parts of slag, 400 to 850 parts of coarse aggregate, 530 to 850 parts of fine aggregate, 7 to 15 parts of water reducer, 100 to 351 parts of alkali activator and 0 to 116 parts of fiber.

[0028] The fly ash is Class F low-calcium fly ash, which can fill the gaps between cement particles and improve the compactness and strength of concrete. The volcanic ash reaction of low-calcium fly ash is relatively slow, which helps to reduce the early hydration heat of concrete, reduce the risk of cracking, and increase the durability of concrete. The slag is S95 grade granulated blast furnace slag. The use of slag can reduce the heat release rate of concrete, reduce the occurrence of temperature cracks, and improve the concrete's resistance to sulfate erosion. The silica fume is S88 grade silica fume, which has extremely high activity and can significantly improve the strength and durability of concrete. The fine particles of silica fume can fill the micropores in concrete, reduce permeability, and improve impermeability and frost resistance. The coarse aggregate includes recycled coarse aggregate and geopolymer unburned artificial aggregate, wherein the recycled coarse aggregate is the recycled coarse aggregate obtained by crushing and screening after building demolition, with a particle size of 2.36 to 16 mm; the geopolymer unburned artificial aggregate is fly ash and slag granulated by disc The spherical aggregate is formed by the method; the fine aggregate is the recycled fine aggregate obtained by crushing and screening after the demolition of the building, and the particle size is 0.15-4.75mm; the coarse aggregate and the fine aggregate are the main skeleton of the concrete, supporting and constraining the cement paste, and affecting the strength and durability of the concrete; the water reducer is a polycarboxylic acid type high-efficiency water reducer, which can reduce the water-cement ratio of the concrete and improve the strength and durability of the concrete; the alkali activator includes sodium silicate, sodium hydroxide and water, and the alkali activator can stimulate the activity of admixtures such as fly ash and slag, promote their reaction with cement hydration products, and generate more cementitious substances; the fiber includes steel fiber and PVA fiber, the tensile strength is 1100MPa, the elastic modulus is 20Gpa, the fiber can enhance the tensile strength and toughness of the concrete, improve the crack resistance and durability of the concrete, and the use of steel fiber and PVA fiber can significantly improve the crack resistance and durability of the concrete, while enhancing the seismic resistance and impact resistance of the concrete.

[0029] The above-mentioned recycled coarse aggregates are one or more combinations of discarded concrete blocks, bricks, and asphalt; the cylinder compressive strength of the coarse aggregates is 9MPa to 13Mpa; the aggregates are strengthened by soaking in an alkaline activator solution or by carbonization. The use of recycled aggregates not only realizes the effective utilization of waste concrete, but also reduces the resource consumption and carbon emissions of concrete production. At the same time, after the strengthening treatment, the performance of the recycled aggregates has been further improved, ensuring the overall performance of the concrete.

[0030] The second object of the present invention is to provide a method for preparing all-solid waste low-carbon concrete, comprising the following steps:

[0031] S1: prepare an alkali activator solution, soak the aggregate in the solution for strengthening, and then take it out;

[0032] S2: After the alkali activator solution is cooled, the fly ash, slag, silica fume, fiber, fine aggregate and alkali activator solution are mixed and stirred evenly;

[0033] S3: Add coarse aggregate into the mixture and stir to form all-solid waste low-carbon concrete.

[0034] The preparation method of the alkaline activator comprises the following steps: mixing a sodium hydroxide solution and a sodium silicate solution to form an alkaline activator solution; the mass fraction of the sodium hydroxide solution and the sodium silicate solution are both 40%.

[0035] Specifically, the stirring condition in S2 is: slow stirring for 150 seconds; the stirring time in S3 is 90 seconds.

[0036] After the all-solid waste low-carbon concrete is formed, it is poured into a mold and fully vibrated. After one day of standard curing, the mold is removed and placed in a standard curing room of a specified age for performance testing.

[0037] Embodiment 1:

[0038] This embodiment includes the following raw materials: 210 parts of fly ash, 420 parts of slag, 70 parts of silica fume, 530 parts of fine aggregate, 675 parts of coarse aggregate, 77 parts of fiber, 54 parts of sodium hydroxide solution, 209 parts of sodium silicate solution, 88 parts of water, and 7 parts of water reducing agent.

[0039] The fly ash is Class F low-calcium fly ash; the slag is S95 grade granular blast furnace slag; the silica fume is S88 grade silica fume; the fine aggregate is the recycled fine aggregate obtained by crushing and screening after the building is demolished, and the particle size is 0.15-4.75 mm; the coarse aggregate is the recycled coarse aggregate obtained by crushing and screening after the building is demolished, and the particle size is 2.36-16 mm; the fiber is end-hook steel fiber, the tensile strength is 1100 MPa, and the elastic modulus is 20 GPa; the concentration of the sodium hydroxide solution and the sodium silicate solution is 40%, and the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0040] The preparation process of all-solid waste low-carbon concrete includes the following steps:

[0041] (1) A sodium hydroxide solution and a sodium silicate solution with a mass fraction of 40% were prepared one day in advance, fully mixed according to a preset modulus, and the aggregate was strengthened by soaking in an alkaline solution.

[0042] (2) After the alkaline activator solution has cooled, pour the prepared fly ash, slag, silica fume, fiber, fine aggregate and alkaline activator solution into a mixer and slowly stir for 150 seconds to mix them evenly.

[0043] (3) Add coarse aggregate to the mixture and stir for 90 seconds. Finally, pour the mixture into the mold and vibrate it thoroughly. After one day of standard curing, remove the mold and place the specimen in a standard curing room for the specified age.

[0044] (4) Test various indicators of concrete in accordance with GB / T 50080-2016 and GB / T 50081-2019.

[0045] Example 2

[0046] This embodiment includes the following raw materials: 210 parts of fly ash, 420 parts of slag, 70 parts of silica fume, 530 parts of fine aggregate, 675 parts of coarse aggregate, 39 parts of fiber, 54 parts of sodium hydroxide solution, 209 parts of sodium silicate solution, 88 parts of water, and 7 parts of water reducing agent.

[0047] The fly ash is Class F low-calcium fly ash; the slag is S95 grade granular blast furnace slag; the silica fume is S88 grade silica fume; the fine aggregate is the recycled fine aggregate obtained by crushing and screening after the building is demolished, and the particle size is 0.15-4.75 mm; the coarse aggregate is the recycled coarse aggregate obtained by crushing and screening after the building is demolished, and the particle size is 2.36-16 mm; the fiber is end-hook steel fiber, the tensile strength is 1100 MPa, and the elastic modulus is 20 GPa; the concentration of the sodium hydroxide solution and the sodium silicate solution is 40%, and the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0048] The preparation process of all-solid waste low-carbon concrete includes the following steps:

[0049] (1) A sodium hydroxide solution and a sodium silicate solution with a mass fraction of 40% were prepared one day in advance, fully mixed according to a preset modulus, and the aggregate was strengthened by soaking in an alkaline solution.

[0050] (2) After the alkaline activator solution has cooled, pour the prepared fly ash, slag, silica fume, fiber, fine aggregate and alkaline activator solution into a mixer and slowly stir for 150 seconds to mix them evenly.

[0051] (3) Add coarse aggregate to the mixture and stir for 90 seconds. Finally, pour the mixture into the mold and vibrate it thoroughly. After one day of standard curing, remove the mold and place the specimen in a standard curing room for the specified age.

[0052] (4) Test various indicators of concrete in accordance with GB / T 50080-2016 and GB / T 50081-2019.

[0053] Example 3

[0054] This embodiment includes the following raw materials: 210 parts of fly ash, 420 parts of slag, 70 parts of silica fume, 530 parts of fine aggregate, 675 parts of coarse aggregate, 77 parts of fiber, 54 parts of sodium hydroxide solution, 209 parts of sodium silicate solution, 88 parts of water, and 7 parts of water reducing agent.

[0055] The fly ash is Class F low-calcium fly ash; the slag is S95 grade granular blast furnace slag; the silica fume is S88 grade silica fume; the fine aggregate is the recycled fine aggregate obtained by crushing and screening after the building is demolished, and the particle size is 0.15-4.75 mm; the coarse aggregate is the recycled coarse aggregate obtained by crushing and screening after the building is demolished, and the particle size is 2.36-16 mm; the fiber is end-hook steel fiber, the tensile strength is 1100 MPa, and the elastic modulus is 20 GPa; the concentration of the sodium hydroxide solution and the sodium silicate solution is 40%, and the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0056] The preparation process of all-solid waste low-carbon concrete includes the following steps:

[0057] (1) A sodium hydroxide solution and a sodium silicate solution with a mass fraction of 40% were prepared one day in advance, fully mixed according to a preset modulus, and the aggregate was strengthened by soaking in an alkaline solution.

[0058] (2) After the alkaline activator solution has cooled, pour the prepared fly ash, slag, silica fume, fiber, fine aggregate and alkaline activator solution into a mixer and slowly stir for 150 seconds to mix them evenly.

[0059] (3) Add coarse aggregate to the mixture and stir for 90 seconds. Finally, pour the mixture into the mold and vibrate it thoroughly. After one day of standard curing, remove the mold and place the specimen in a standard curing room for the specified age.

[0060] (4) Test various indicators of concrete in accordance with GB / T 50080-2016 and GB / T 50081-2019.

[0061] Example 4

[0062] This embodiment includes the following raw materials: 210 parts of fly ash, 420 parts of slag, 70 parts of silica fume, 530 parts of fine aggregate, 675 parts of coarse aggregate, 116 parts of fiber, 54 parts of sodium hydroxide solution, 209 parts of sodium silicate solution, 88 parts of water, and 7 parts of water reducing agent.

[0063] The fly ash is Class F low-calcium fly ash; the slag is S95 grade granular blast furnace slag; the silica fume is S88 grade silica fume; the fine aggregate is the recycled fine aggregate obtained by crushing and screening after the building is demolished, and the particle size is 0.15-4.75 mm; the coarse aggregate is the recycled coarse aggregate obtained by crushing and screening after the building is demolished, and the particle size is 2.36-16 mm; the fiber is end-hook steel fiber, the tensile strength is 1100 MPa, and the elastic modulus is 20 GPa; the concentration of the sodium hydroxide solution and the sodium silicate solution is 40%, and the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0064] The preparation process of all-solid waste low-carbon concrete includes the following steps:

[0065] (1) A sodium hydroxide solution and a sodium silicate solution with a mass fraction of 40% were prepared one day in advance, fully mixed according to a preset modulus, and the aggregate was strengthened by soaking in an alkaline solution.

[0066] (2) After the alkaline activator solution has cooled, pour the prepared fly ash, slag, silica fume, fiber, fine aggregate and alkaline activator solution into a mixer and slowly stir for 150 seconds to mix them evenly.

[0067] (3) Add coarse aggregate to the mixture and stir for 90 seconds. Finally, pour the mixture into the mold and vibrate it thoroughly. After one day of standard curing, remove the mold and place the specimen in a standard curing room for the specified age.

[0068] (4) Test various indicators of concrete in accordance with GB / T 50080-2016 and GB / T 50081-2019.

[0069] Example 5

[0070] This embodiment includes the following raw materials: 219 parts of fly ash, 197 parts of slag, 21.9 parts of silica fume, 625 parts of fine aggregate, 764 parts of coarse aggregate, 0 parts of fiber, 34 parts of sodium hydroxide solution, 130 parts of sodium silicate solution, 55 parts of water, and 11.4 parts of water reducing agent.

[0071] The fly ash is F-type low-calcium fly ash; the slag is S95-grade granular blast furnace slag; the silica fume is S88-grade silica fume; the fine aggregate is recycled fine aggregate obtained by crushing and screening after building demolition, with a particle size of 0.15-4.75 mm; the coarse aggregate is artificial aggregate prepared from fly ash and slag, with a particle size of 4.75-16 mm; the fiber is PVA fiber, with a tensile strength of 1600 MPa and an elastic modulus of 40 GPa; the concentration of the sodium hydroxide solution and the sodium silicate solution is 40%, and the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0072] The preparation process of all-solid waste low-carbon concrete includes the following steps:

[0073] (1) A sodium hydroxide solution and a sodium silicate solution with a mass fraction of 40% were prepared one day in advance, fully mixed according to a preset modulus, and the aggregate was strengthened by soaking in an alkaline solution.

[0074] (2) After the alkaline activator solution has cooled, pour the prepared fly ash, slag, silica fume, fiber, fine aggregate and alkaline activator solution into a mixer and slowly stir for 150 seconds to mix them evenly.

[0075] (3) Add coarse aggregate to the mixture and stir for 90 seconds. Finally, pour the mixture into the mold and vibrate it thoroughly. After one day of standard curing, remove the mold and place the specimen in a standard curing room for the specified age.

[0076] (4) Test various indicators of concrete in accordance with GB / T 50080-2016 and GB / T 50081-2019.

[0077] Example 6

[0078] This embodiment includes the following raw materials: 219 parts of fly ash, 197 parts of slag, 21.9 parts of silica fume, 625 parts of fine aggregate, 764 parts of coarse aggregate, 6.5 parts of fiber, 34 parts of sodium hydroxide solution, 130 parts of sodium silicate solution, 55 parts of water, and 11.4 parts of water reducing agent.

[0079] The fly ash is F-type low-calcium fly ash; the slag is S95-grade granular blast furnace slag; the silica fume is S88-grade silica fume; the fine aggregate is recycled fine aggregate obtained by crushing and screening after building demolition, with a particle size of 0.15-4.75 mm; the coarse aggregate is artificial aggregate prepared from fly ash and slag, with a particle size of 4.75-16 mm; the fiber is PVA fiber, with a tensile strength of 1600 MPa and an elastic modulus of 40 GPa; the concentration of the sodium hydroxide solution and the sodium silicate solution is 40%, and the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0080] The preparation process of all-solid waste low-carbon concrete includes the following steps:

[0081] (1) A sodium hydroxide solution and a sodium silicate solution with a mass fraction of 40% were prepared one day in advance, fully mixed according to a preset modulus, and the aggregate was strengthened by soaking in an alkaline solution.

[0082] (2) After the alkaline activator solution has cooled, pour the prepared fly ash, slag, silica fume, fiber, fine aggregate and alkaline activator solution into a mixer and slowly stir for 150 seconds to mix them evenly.

[0083] (3) Add coarse aggregate to the mixture and stir for 90 seconds. Finally, pour the mixture into the mold and vibrate it thoroughly. After one day of standard curing, remove the mold and place the specimen in a standard curing room for the specified age.

[0084] (4) Test various indicators of concrete in accordance with GB / T 50080-2016 and GB / T 50081-2019.

[0085] Example 7

[0086] This embodiment includes the following raw materials: 219 parts of fly ash, 197 parts of slag, 21.9 parts of silica fume, 625 parts of fine aggregate, 764 parts of coarse aggregate, 13 parts of fiber, 34 parts of sodium hydroxide solution, 130 parts of sodium silicate solution, 55 parts of water, and 11.4 parts of water reducing agent.

[0087] The fly ash is F-type low-calcium fly ash; the slag is S95-grade granular blast furnace slag; the silica fume is S88-grade silica fume; the fine aggregate is recycled fine aggregate obtained by crushing and screening after building demolition, with a particle size of 0.15-4.75 mm; the coarse aggregate is artificial aggregate prepared from fly ash and slag, with a particle size of 4.75-16 mm; the fiber is PVA fiber, with a tensile strength of 1600 MPa and an elastic modulus of 40 GPa; the concentration of the sodium hydroxide solution and the sodium silicate solution is 40%, and the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0088] The preparation process of all-solid waste low-carbon concrete includes the following steps:

[0089] (1) A sodium hydroxide solution and a sodium silicate solution with a mass fraction of 40% were prepared one day in advance, fully mixed according to a preset modulus, and the aggregate was strengthened by soaking in an alkaline solution.

[0090] (2) After the alkaline activator solution has cooled, pour the prepared fly ash, slag, silica fume, fiber, fine aggregate and alkaline activator solution into a mixer and slowly stir for 150 seconds to mix them evenly.

[0091] (3) Add coarse aggregate to the mixture and stir for 90 seconds. Finally, pour the mixture into the mold and vibrate it thoroughly. After one day of standard curing, remove the mold and place the specimen in a standard curing room for the specified age.

[0092] (4) Test various indicators of concrete in accordance with GB / T 50080-2016 and GB / T 50081-2019.

[0093] Embodiment 8:

[0094] This embodiment includes the following raw materials: 150 parts of fly ash, 200 parts of slag, 15 parts of silica fume, 530 parts of fine aggregate, 850 parts of coarse aggregate, 77 parts of fiber, 20 parts of sodium hydroxide solution, 20 parts of sodium silicate solution, 60 parts of water, and 15 parts of water reducing agent.

[0095] The fly ash is Class F low-calcium fly ash; the slag is S95 grade granular blast furnace slag; the silica fume is S88 grade silica fume; the fine aggregate is the recycled fine aggregate obtained by crushing and screening after the building is demolished, and the particle size is 0.15-4.75 mm; the coarse aggregate is the recycled coarse aggregate obtained by crushing and screening after the building is demolished, and the particle size is 2.36-16 mm; the fiber is end-hook steel fiber, the tensile strength is 1100 MPa, and the elastic modulus is 20 GPa; the concentration of the sodium hydroxide solution and the sodium silicate solution is 40%, and the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0096] The preparation process of all-solid waste low-carbon concrete includes the following steps:

[0097] (1) A sodium hydroxide solution and a sodium silicate solution with a mass fraction of 40% were prepared one day in advance, fully mixed according to a preset modulus, and the aggregate was strengthened by soaking in an alkaline solution.

[0098] (2) After the alkaline activator solution has cooled, pour the prepared fly ash, slag, silica fume, fiber, fine aggregate and alkaline activator solution into a mixer and slowly stir for 150 seconds to mix them evenly.

[0099] (3) Add coarse aggregate to the mixture and stir for 90 seconds. Finally, pour the mixture into the mold and vibrate it thoroughly. After one day of standard curing, remove the mold and place the specimen in a standard curing room for the specified age.

[0100] (4) Test various indicators of concrete in accordance with GB / T 50080-2016 and GB / T 50081-2019.

[0101] Embodiment 9:

[0102] This embodiment includes the following raw materials: 300 parts of fly ash, 150 parts of slag, 50 parts of silica fume, 850 parts of fine aggregate, 400 parts of coarse aggregate, 77 parts of fiber, 54 parts of sodium hydroxide solution, 209 parts of sodium silicate solution, 88 parts of water, and 7 parts of water reducing agent.

[0103] The fly ash is Class F low-calcium fly ash; the slag is S95 grade granular blast furnace slag; the silica fume is S88 grade silica fume; the fine aggregate is the recycled fine aggregate obtained by crushing and screening after the building is demolished, and the particle size is 0.15-4.75 mm; the coarse aggregate is the recycled coarse aggregate obtained by crushing and screening after the building is demolished, and the particle size is 2.36-16 mm; the fiber is end-hook steel fiber, the tensile strength is 1100 MPa, and the elastic modulus is 20 GPa; the concentration of the sodium hydroxide solution and the sodium silicate solution is 40%, and the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0104] The preparation process of all-solid waste low-carbon concrete includes the following steps:

[0105] (1) A sodium hydroxide solution and a sodium silicate solution with a mass fraction of 40% were prepared one day in advance, fully mixed according to a preset modulus, and the aggregate was strengthened by soaking in an alkaline solution.

[0106] (2) After the alkaline activator solution has cooled, pour the prepared fly ash, slag, silica fume, fiber, fine aggregate and alkaline activator solution into a mixer and slowly stir for 150 seconds to mix them evenly.

[0107] (3) Add coarse aggregate to the mixture and stir for 90 seconds. Finally, pour the mixture into the mold and vibrate it thoroughly. After one day of standard curing, remove the mold and place the specimen in a standard curing room for the specified age.

[0108] (4) Test various indicators of concrete in accordance with GB / T 50080-2016 and GB / T 50081-2019.

[0109] The all-solid waste low-carbon concrete prepared in Examples 1-7 was tested, and Table 1 shows the aggregate performance test results.

[0110] Table 1 Performance of all-solid waste low-carbon concrete prepared in Examples 1-7

[0111]

[0112] From the test results of the all-solid waste low-carbon concrete prepared in the above Examples 1-7, it can be seen that the concrete prepared by the present invention has the characteristics of low carbon emissions and high early strength, and the final strength meets the requirements of construction use.

[0113] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A full solid waste low-carbon concrete, characterized in that: Calculated by mass, it includes 150 to 300 parts of fly ash, 15 to 70 parts of silica fume, 150 to 420 parts of slag, 400 to 850 parts of coarse aggregate, 530 to 850 parts of fine aggregate, 7 to 15 parts of water reducer, 100 to 351 parts of alkali activator and 0 to 116 parts of fiber.

2. The all-solid waste low-carbon concrete according to claim 1, characterized in that: The coarse aggregate includes recycled coarse aggregate and geopolymer unburned artificial aggregate.

3. The all-solid waste low-carbon concrete according to claim 1, characterized in that: The recycled aggregate is one or more of discarded concrete blocks, bricks and asphalt.

4. The all-solid waste low-carbon concrete according to claim 1, characterized in that: The cylinder compressive strength of the coarse aggregate is 9MPa-13Mpa.

5. The all-solid waste low-carbon concrete according to claim 1, characterized in that: The fine aggregate is recycled fine aggregate.

6. The all-solid waste low-carbon concrete according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid type high efficiency water reducing agent.

7. The all-solid waste low-carbon concrete according to claim 1, characterized in that: The alkaline activator includes sodium silicate, sodium hydroxide and water.

8. The all-solid waste low-carbon concrete according to claim 1, characterized in that: The fibers include steel fibers and PVA fibers.

9. A method for preparing all-solid waste low-carbon concrete according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: prepare an alkali activator solution, soak the aggregate in the solution for strengthening, and then take it out; S2: After the alkali activator solution is cooled, the fly ash, slag, silica fume, fiber, fine aggregate and alkali activator solution are mixed and stirred evenly; S3: Add coarse aggregate to the mixture to form all-solid waste low-carbon concrete.

10. The preparation method according to claim 9, characterized in that: The preparation method of the alkaline activator solution comprises the following steps: The sodium hydroxide solution and the sodium silicate solution are thoroughly mixed to form an alkaline activator solution.

Citation Information

Patent Citations

  • PVA fiber and steel fiber reinforced concrete

    CN110272237A

  • Method for preparing PVA (Polyvinyl Alcohol) fiber and steel fiber reinforced concrete

    CN110330279A

  • High-temperature cured low-carbon high-strength geopolymer concrete material and preparation method thereof

    CN114956681A

  • Anti-cracking recycled concrete and preparation method thereof

    CN116477897A

  • Permeable concrete block manufacture method to use eco-friendly recycled aggregate coated

    KR101173442B1

Cited By

  • All-solid waste alkali-activated recycled concrete and preparation method thereof

    CN120965251A

  • High-toughness impact-resistant geopolymer concrete membrane shell and preparation method thereof

    CN122325163A

  • Multi-solid-waste synergistic geopolymer composite material and preparation method thereof

    CN122685369A