Novel high-strength and high-toughness SiC ceramic material and preparation method thereof
By adding ZrO2 and Y2O3 powder and SiC whiskers to SiC ceramics for hot-pressing sintering, Y2SiO5, Zr3Y4O12 and ZrC are generated, which solves the bottleneck problem of improving the density and mechanical properties of SiC ceramic materials and achieves efficient and low-cost density. , improvement in flexural strength and fracture toughness, suitable for industrial applications.
Patent Information
- Application Number
- CN202410929896.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-11
AI Technical Summary
Existing SiC ceramic materials have bottlenecks in terms of density, flexural strength and fracture toughness, and the existing processes are complex, costly and inefficient, making it difficult to meet the requirements of industrial applications.
By adding specific contents of ZrO2 powder and Y2O3 powder to SiC whiskers for hot-pressing sintering, Y2SiO5, Zr3Y4O12 and ZrC are generated as the second phase to improve the density and mechanical properties of the ceramic.
The density of SiC ceramics exceeds 99%, the hardness exceeds 20GPa, the flexural strength exceeds 800MPa, and the fracture toughness exceeds 8MPa·m0.5. It simplifies the process, reduces costs, and is suitable for industrial production.
Smart Images

Figure CN118754672A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of structural ceramics, and in particular to a novel high-strength and high-toughness SiC ceramic material and a preparation method thereof. Background Art
[0002] SiC ceramics have the characteristics of high thermal conductivity, high temperature stability, and chemical inertness. SiC-based composite materials prepared from them can be widely used in industries such as aerospace and energy. However, SiC ceramics have difficulties in sintering densification (pure SiC can only be densified by hot pressing at 2300℃ and 50MPa) and low fracture toughness (about 3MPa·m 0.5 ) These two drawbacks cannot meet the requirements for structural components in some industrial fields, thus seriously limiting the industrial application of this material.
[0003] Therefore, it is necessary to solve the two problems of difficult sintering densification and low fracture toughness of SiC ceramics. The existing technology has tried various toughening methods to improve the fracture toughness of SiC ceramics, mainly including particle toughening and whisker toughening; however, the reported particle toughening SiC ceramics do not improve the fracture toughness much; and the preparation idea of using SiC whiskers to toughen SiC ceramics is to simply mix the whiskers with the powder evenly, and after sintering, use the pull-out and debonding mechanisms of SiC whiskers to increase the fracture toughness.
[0004] For example, Chinese patent CN104140265A discloses a method for preparing silicon carbide ceramics with zirconium oxide as a toughening phase by liquid phase sintering. This method belongs to the particle toughening method mentioned above. However, the maximum improvement of the fracture toughness of SiC ceramics can only reach 5.97MPa·m 0.5 Obviously, the improvement is not high; and the maximum bending strength can only reach 586MPa, which does not exceed 800MPa.
[0005] Chinese patent CN114516756A discloses a silicon carbide composite ceramic material and its preparation method and application. The method belongs to the synergistic toughening of particle toughening and whisker toughening. The sintering is divided into two steps, the process is long, the amount of acid solution consumed is large, the pressure of pressurization is high, and the cost is high. Moreover, the mechanical properties of SiC ceramics obtained by this toughening method have almost reached a bottleneck, and the maximum fracture toughness can only reach about 7.5MPa·m 0.5 Although the invention has a complicated process flow, the fracture toughness obtained still cannot meet some extreme service conditions, such as the cladding material in China's new generation of nuclear reactors.
[0006] Chinese patent CN106977217A discloses a method for preparing a high-strength and high-toughness silicon carbide fiber reinforced silicon carbide ceramic-based composite material, which requires the silicon carbide fiber to be woven into a three-dimensional silicon carbide fiber reinforcement, and then the silicon carbide is deposited to obtain the initial silicon carbide matrix, and the impregnation slurry is vacuum impregnated and cracked to obtain the silicon carbide matrix, and finally the silicon carbide coating is deposited to obtain; Obviously, this method improves the structure of the silicon carbide fiber and the overall internal and external structure of the composite material. Although it can improve the fracture toughness of the material, the process is extremely long, the operation is difficult, the cost is high, and the efficiency is low. In addition, the SiC fiber used in the process is a soft long fiber, so the fracture toughness is greatly improved at the expense of the hardness and flexural strength of the material, ensuring that the material is not easy to break. However, the material cannot meet the hardness requirements for structural components in the industrial field. The lower hardness will cause the material to be unable to withstand greater stress, resulting in destructive behavior.
[0007] Chinese patent CN116573940A discloses a high-toughness silicon carbide ceramic material and a preparation method thereof, wherein the mixed powder of silicon carbide powder and sintering aid is ball-milled to obtain silicon carbide slurry, which is then dried, mechanically ground and pressed into a silicon carbide blank, then sintered at high temperature in vacuum to obtain a silicon carbide ceramic body, and sintered at low temperature to obtain a high-toughness silicon carbide ceramic material; it is obvious that the fracture toughness of the prepared ceramic material does not exceed 8MPa·m 0.5 The two sintering processes consume a lot of energy. Summary of the invention
[0008] The technical problem to be solved by the present invention is that the current silicon carbide ceramic materials cannot achieve low-cost and high-efficiency synergistic improvement in density, flexural strength and fracture toughness. The existing technologies do not have a significant effect on improving mechanical properties. There are few processes that can sinter SiC ceramics to a density of more than 99%, and the flexural strength and fracture toughness cannot simultaneously meet the requirements of more than 800MPa and 8MPa·m 0.5 Most of the current process methods are particle toughening, whisker toughening, and synergistic toughening. A small number of them are based on synergistic toughening and use three-dimensional silicon carbide fiber reinforcement, sintering aids and ceramic materials for internal and external results to strengthen, which brings technical defects such as complex operation, high cost and low efficiency.
[0009] In order to solve the above technical problems, the technical solutions provided by the present invention are as follows:
[0010] A new type of high-strength and high-toughness SiC ceramic material, the new type of high-strength and high-toughness SiC ceramic material comprises 75-82wt.% SiC, 10-12wt.% Y2SiO5, 6-7wt.% Zr3Y4O 12 and 1-2wt.% ZrC, and different sizes of materials can be prepared using different molds, and the size is adjustable.
[0011] Optionally, the SiC is in the form of equiaxed grains with a size of 1-1.5 μm; the remaining second phases Y2SiO5, Zr3Y4O 12 and ZrC are dispersed and evenly wrapped around the matrix SiC grains with a size of 0.5-2μm.
[0012] Optionally, the density of the new high-strength and high-toughness SiC ceramic material exceeds 99%, and the density is 3.45-3.51 g / cm 3 , hardness exceeds 20GPa, bending strength exceeds 800MPa, fracture toughness exceeds 8MPa·m 0.5 .
[0013] A method for preparing the novel high-strength and high-toughness SiC ceramic material based on the above-mentioned method comprises the following steps:
[0014] S1. Raw material weighing:
[0015] Select α-SiC powder, ZrO2 powder, Y2O3 powder and SiC whisker as raw material powders, weigh them according to the proportion of the components of the novel high-strength and high-toughness SiC ceramic material, and obtain raw material mixed powder;
[0016] S2, ball milling:
[0017] The raw material mixed powder of S1 is wet ball-milled to obtain a mixed slurry;
[0018] S3, Drying and Sieving:
[0019] The mixed slurry of S2 is dried and sieved to obtain a fine particle mixed powder;
[0020] S4. Graphite mold preparation:
[0021] According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined, and a graphite mold that meets the product requirements is prepared. Then, the fine particle mixed powder of S3 is placed in the graphite mold and vibrated. A layer of graphite paper needs to be placed between the graphite mold and the powder to prevent the sintered sample from sticking to the mold;
[0022] S5, hot pressing sintering:
[0023] The fine-particle mixed powder in the graphite mold filled with the S4 fine-particle mixed powder is hot-pressed and sintered at a high temperature below 1900°C. After the sintering is completed, the pressure is directly released to obtain a new type of high-strength and high-toughness SiC ceramic material product.
[0024] Optionally, the purity of α-SiC powder in S1 is 98.5-99.9%, and the average particle size is 0.05-0.2μm; the purity of ZrO2 powder is 98-99.9%, and the average particle size is 0.01-0.06μm; the purity of Y2O3 powder is 98-99.9%, and the average particle size is 0.01-0.03μm; the purity of SiC whiskers is 99%, the length is 4-35μm, and the diameter is 0.3-0.7μm.
[0025] Optionally, the volume percentage of ZrO2 powder and Y2O3 powder in S1 in the raw material mixed powder is 13-17 vol%, wherein the molar ratio of ZrO2 powder to Y2O3 powder is 1:1; the volume percentage of the added SiC whisker in the raw material mixed powder is between 40-50 vol.%.
[0026] Optionally, the wet ball milling in S2 requires mixing the raw material mixed powder with anhydrous ethanol and zirconium oxide ball milling beads (or silicon carbide ball milling beads, agate ball milling beads) in a mass ratio of 1:1:1, placing it in a nylon ball mill jar, and mixing it at a speed of 250-350 r / min for 4-8 hours.
[0027] Optionally, the drying temperature in S3 is 60-100° C., the drying time is 10-12 h, and the mesh size of the sieve after drying is 80-100 mesh.
[0028] Optionally, the cavity size of the graphite mold in S4 is 0.4-0.5mm larger than the product appearance size.
[0029] Optionally, the heating rate of hot pressing sintering in S5 is 5-10°C / min, the sintering temperature is 1850-1900°C, the pressure is 40-60MPa, and the heat and pressure holding time is 2-2.5h.
[0030] Technical principle of the present invention:
[0031] The current preparation method of SiC whisker toughened SiC ceramics is improved. By changing the formula, a new toughening method is obtained to greatly improve the mechanical properties of SiC ceramics.
[0032] Different from the SiCw toughened SiC ceramics reported so far, this scheme adds a specific type and content of powder to react with the added SiCw, thereby greatly improving the relative density and mechanical properties (including flexural strength and fracture toughness) of SiC ceramics.
[0033] The key points of the technology are: ① The type and content of the added powder are indispensable. A large change in the content will affect the process of the secondary reaction and ultimately have an adverse effect on the performance of the material. ② The sintering system of hot pressing sintering, temperature, time and pressure are indispensable. Changing a certain parameter may also affect the secondary reaction and thus affect the performance of the final material.
[0034] This scheme chooses to add ZrO2 powder, Y2O3 powder and SiC whiskers to α-SiC powder to react, and use the reaction products to promote the densification of SiC ceramics and improve the mechanical properties of the material. During the sintering process, SiC whiskers will react with the added ZrO2 and Y2O3 as follows:
[0035] SiC+ZrO2→ZrC+SiO↑+CO↑(1)
[0036] SiO↑+CO↑+Y2O3→Y2SiO5(2)
[0037] ZrO2+Y2O3→Zr3Y4O 12 (3)
[0038] Note: SiC in reaction (1) represents SiC whiskers. This reaction will only occur when SiC whiskers are added, and the subsequent reaction (2) will also occur.
[0039] The generated product can fill the gaps between SiC grains during sintering, thereby increasing the density of SiC ceramics. In addition, the product generated after the whiskers react with the added powder can refine the grains, thereby increasing the bending strength of the ceramics. And the product generated after the whiskers react with the added powder has appropriate bonding strength with the SiC matrix grains, thus improving the fracture toughness.
[0040] Compared with the prior art, the above technical solution has at least the following beneficial effects:
[0041] The above scheme, the present invention provides a new type of high-strength and high-toughness SiC ceramic material and preparation method, which overcomes the technical defect that the current SiC ceramic material cannot synergistically improve the density, flexural strength and fracture toughness at low cost and high efficiency, expands the application scope of SiC ceramic materials, and is conducive to large-scale industrial production and promotion.
[0042] The invention adds ZrO2 powder, Y2O3 powder and SiC whisker to α-SiC powder to react during hot pressing sintering to obtain 75-82wt.% SiC, 10-12wt.% Y2SiO5, 6-7wt.% Zr3Y4O 12and 1-2wt.% ZrC; among them, Y2SiO5 plays the role of filling the gaps between SiC grains to ensure the density of the material. 12 The role is to provide the right interface bonding strength with the matrix SiC grains, thereby improving the fracture toughness. ZrC can pin the grain boundaries to refine the grains and improve the bending strength of the material.
[0043] The present invention can fully mix various powders through wet ball milling. In particular, SiC whiskers are very easy to agglomerate due to their large specific surface area, thereby hindering mass transfer during the sintering process and resulting in poor density of SiC ceramics. Wet ball milling can ensure that the whiskers are evenly dispersed and will not agglomerate during the sintering process.
[0044] The hot pressing sintering temperature of the invention is lower than 1900° C., and SiC ceramics with excellent performance are obtained on the basis of reducing production costs.
[0045] The density of the new high-strength and high-toughness SiC ceramic material prepared by the present invention exceeds 99%, and the density is more than 3.45-3.51g / cm 3 , hardness exceeds 20GPa, bending strength exceeds 800MPa, fracture toughness exceeds 8MPa·m 0.5 .
[0046] In summary, compared with other traditional methods, the method of the present invention can obtain a composite material composed of Y2SiO5, Zr3Y4O3, and SiC whiskers by adding ZrO2 powder, Y2O3 powder, and SiC whiskers to α-SiC powder in the subsequent hot pressing sintering process. 12 SiC ceramic materials with ZrC as the second phase for strengthening and toughening have a hardness of more than 20GPa, a bending strength of more than 800MPa, and a fracture toughness of more than 8MPa·m on the basis of a density of more than 99%. 0.5 The process has simple steps, convenient operation, short process cycle, low cost, high efficiency, and easy control, which is conducive to industrial production and can produce SiC ceramics with the best comprehensive properties (especially flexural strength and fracture toughness) reported so far. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0048] Figure 1 This is a morphology diagram of the initial sintered powder in the method for preparing a novel high-strength and high-toughness SiC ceramic material according to Example 1 of the present invention;
[0049] Figure 2 This is an XRD diagram of a product prepared by a method for preparing a novel high-strength and high-toughness SiC ceramic material according to Example 1 of the present invention;
[0050] Figure 3 This is a fracture morphology of a product prepared by a method for preparing a novel high-strength and high-toughness SiC ceramic material according to Example 1 of the present invention;
[0051] Figure 4 This is the XRD pattern of the SiC ceramic prepared without adding SiC whiskers in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] A new type of high-strength and high-toughness SiC ceramic material, the new type of high-strength and high-toughness SiC ceramic material comprises 75-82wt.% SiC, 10-12wt.% Y2SiO5, 6-7wt.% Zr3Y4O 12 and 1-2wt.% ZrC, and different sizes of materials can be prepared using different molds, and the size is adjustable.
[0054] In particular, the shape of SiC is equiaxed grains with a size of 1-1.5 μm; the remaining second phases Y2SiO5, Zr3Y4O 12 and ZrC are dispersed and evenly wrapped around the matrix SiC grains with a size of 0.5-2μm.
[0055] In particular, the new high-strength and high-toughness SiC ceramic material has a density of more than 99% and a density of 3.45-3.51 g / cm 3 , hardness exceeds 20GPa, bending strength exceeds 800MPa, fracture toughness exceeds 8MPa·m 0.5 .
[0056] A method for preparing the novel high-strength and high-toughness SiC ceramic material based on the above-mentioned method comprises the following steps:
[0057] S1. Raw material weighing:
[0058] Select α-SiC powder, ZrO2 powder, Y2O3 powder and SiC whisker as raw material powders, weigh them according to the proportion of the components of the novel high-strength and high-toughness SiC ceramic material, and obtain raw material mixed powder;
[0059] S2, ball milling:
[0060] The raw material mixed powder of S1 is wet ball-milled to obtain a mixed slurry;
[0061] S3, Drying and Sieving:
[0062] The mixed slurry of S2 is dried and sieved to obtain a fine particle mixed powder;
[0063] S4. Graphite mold preparation:
[0064] According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined, and a graphite mold that meets the product requirements is prepared. Then, the fine particle mixed powder of S3 is placed in the graphite mold and vibrated. A layer of graphite paper needs to be placed between the graphite mold and the powder to prevent the sintered sample from sticking to the mold;
[0065] S5, hot pressing sintering:
[0066] The fine-particle mixed powder in the graphite mold filled with the S4 fine-particle mixed powder is hot-pressed and sintered at a high temperature below 1900°C. After the sintering is completed, the pressure is directly released to obtain a new type of high-strength and high-toughness SiC ceramic material product.
[0067] In particular, the purity of α-SiC powder in S1 is 98.5-99.9%, and the average particle size is 0.05-0.2μm; the purity of ZrO2 powder is 98-99.9%, and the average particle size is 0.01-0.06μm; the purity of Y2O3 powder is 98-99.9%, and the average particle size is 0.01-0.03μm; the purity of SiC whiskers is 99%, the length is 4-35μm, and the diameter is 0.3-0.7μm.
[0068] In particular, the volume percentage of ZrO2 powder and Y2O3 powder in S1 in the raw material mixed powder is 13-17 vol.%, wherein the molar ratio of ZrO2 powder to Y2O3 powder is 1:1; the volume percentage of the added SiC whisker in the raw material mixed powder is between 40-50 vol.%.
[0069] In particular, the wet ball milling in S2 requires mixing the raw material mixed powder with anhydrous ethanol and zirconium oxide ball milling beads (or silicon carbide ball milling beads, agate ball milling beads) in a mass ratio of 1:1:1, placing it in a nylon ball mill jar, and mixing it at a speed of 250-350r / min for 4-8h.
[0070] In particular, the drying temperature in S3 is 60-100° C., the drying time is 10-12 h, and the mesh size of the sieve after drying is 80-100 meshes.
[0071] In particular, the cavity size of the graphite mold in S4 is 0.4-0.5mm larger than the product appearance size.
[0072] In particular, the heating rate of hot pressing sintering in S5 is 5-10°C / min, the sintering temperature is 1850-1900°C, the pressure is 40-60MPa, and the heat and pressure holding time is 2-2.5h.
[0073] Example 1
[0074] A new type of high-strength and high-toughness SiC ceramic material, the new type of high-strength and high-toughness SiC ceramic material comprises 78wt.% SiC, 10wt.% Y2SiO5, 6wt.% Zr3Y4O 12 and 1wt.% ZrC.
[0075] A method for preparing the novel high-strength and high-toughness SiC ceramic material based on the above-mentioned method comprises the following steps:
[0076] S1. Raw material weighing:
[0077] According to the total content of ZrO2 powder and Y2O3 powder of 15 vol.% (the ratio of ZrO2 powder to Y2O3 powder is 1:1 in molar ratio), 40 vol.% SiC whisker and the rest of α-SiC powder are weighed to obtain 50 g of raw material mixed powder; wherein the purity of α-SiC powder is 98.9%, and the average particle size is 0.09 μm; the purity of ZrO2 powder is 98.7%, and the average particle size is 0.03 μm; the purity of Y2O3 powder is 98.3%, and the average particle size is 0.012 μm; the purity of SiC whisker is 99%, the length is 4-35 μm, and the diameter is 0.3-0.7 μm;
[0078] S2, ball milling:
[0079] The raw material mixed powder of S1 is wet-milled. The wet-milling method requires mixing the raw material mixed powder with 50 g of anhydrous ethanol and 50 g of zirconium oxide ball milling beads in a mass ratio of 1:1:1, placing the mixture in a nylon ball milling jar, and mixing the mixture at a speed of 300 r / min for 4 h to obtain a mixed slurry;
[0080] S3, Drying and Sieving:
[0081] The mixed slurry of S2 was dried and sieved at a drying temperature of 80°C for 11 hours. After drying, the mesh size of the sieve was 80 meshes to obtain a fine particle mixed powder;
[0082] S4. Graphite mold preparation:
[0083] According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined. The cavity size of the graphite mold is 0.4 mm larger than the product appearance size. A graphite mold that meets the product requirements is prepared. Then, the fine particle mixed powder of S3 is placed in the graphite mold and vibrated to obtain a graphite mold filled with fine particle mixed powder.
[0084] S5, hot pressing sintering:
[0085] The fine-particle mixed powder in the graphite mold filled with fine-particle mixed powder of S4 was hot-pressed and sintered at a high temperature below 1900℃. After 30 minutes, the temperature was raised to 200℃, and then to 1700℃ at a heating rate of 10℃ / min, and then to 1880℃ at a heating rate of 5℃ / min. After being kept at this temperature for 2 hours, it was naturally cooled to room temperature with the furnace. During the entire heating process, the pressure was gradually applied to 50MPa. When the sintering temperature reached 1880℃, the pressure applied was just 50MPa. The pressure was maintained for 2 hours, and the pressure was directly released after the sintering was completed to obtain a new type of high-strength and high-toughness SiC ceramic material product.
[0086] like Figure 1 As shown, it can be seen that SiC whiskers with obvious short rod-like morphology are added to the mixed powder and are evenly mixed with other powders.
[0087] like Figure 2 As shown in the figure, it can be clearly seen from the spectrum that the prepared SiC ceramic material contains SiC, Y2SiO5, Zr3Y4O 12 The new high-strength and high-toughness SiC ceramic material products prepared in this embodiment include SiC, Y2SiO5, Zr3Y4O 12 and ZrC, which are completely consistent with the several reaction products mentioned above.
[0088] like Figure 3 As shown in the figure, the dark grains are the matrix SiC grains, and the other bright white grains wrapped around the matrix grains are the generated Y2SiO5, Zr3Y4O 12 and ZrC. Their sizes can be counted by the ruler to be 0.5-2 μm. In addition, it can be seen that the rod-shaped SiC whiskers in the starting powder no longer exist, indicating that the whiskers have been completely reacted.
[0089] The density of the new high-strength and high-toughness SiC ceramic material prepared in this embodiment is 99.2±0.01%, and the density is 3.48±0.02g / cm 3, hardness is 21±0.2GPa, flexural strength is 885±55MPa, fracture toughness is 8.94±0.26MPa·m 0.5 .
[0090] Example 2
[0091] A new type of high-strength and high-toughness SiC ceramic material, the new type of high-strength and high-toughness SiC ceramic material comprises 75wt.% SiC, 12wt.% Y2SiO5, 7wt.% Zr3Y4O 12 and 1.5wt.% ZrC.
[0092] A method for preparing the novel high-strength and high-toughness SiC ceramic material based on the above-mentioned method comprises the following steps:
[0093] S1. Raw material weighing:
[0094] According to the total content of ZrO2 powder and Y2O3 powder of 17 vol.% (the ratio of ZrO2 powder to Y2O3 powder is 1:1 in molar ratio), 40 vol.% SiC whisker and the rest of α-SiC powder are weighed to obtain 50 g of raw material mixed powder; wherein the purity of α-SiC powder is 99.2%, and the average particle size is 0.15 μm; the purity of ZrO2 powder is 98.6%, and the average particle size is 0.05 μm; the purity of Y2O3 powder is 98.3%, and the average particle size is 0.01 μm; the purity of SiC whisker is 99%, the length is 4-35 μm, and the diameter is 0.3-0.7 μm;
[0095] S2, ball milling:
[0096] The raw material mixed powder of S1 is wet-milled. The wet-milling method requires mixing the raw material mixed powder with 50 g of anhydrous ethanol and 50 g of zirconium oxide ball milling beads in a mass ratio of 1:1:1, placing the mixture in a nylon ball milling jar, and mixing the mixture at a speed of 330 r / min for 6 h to obtain a mixed slurry;
[0097] S3, Drying and Sieving:
[0098] The mixed slurry of S2 was dried and sieved at a drying temperature of 70°C for 10 hours. After drying, the mesh size of the sieve was 80 meshes to obtain a fine particle mixed powder;
[0099] S4. Graphite mold preparation:
[0100] According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined. The cavity size of the graphite mold is 0.43 mm larger than the product appearance size. A graphite mold that meets the product requirements is prepared. Then, the fine particle mixed powder of S3 is placed in the graphite mold and vibrated to obtain a graphite mold filled with fine particle mixed powder.
[0101] S5, hot pressing sintering:
[0102] The fine-particle mixed powder in the graphite mold filled with fine-particle mixed powder of S4 was hot-pressed and sintered at a high temperature below 1900℃. After 30 minutes, the temperature was raised to 220℃, and then to 1650℃ at a heating rate of 10℃ / min, and then to 1860℃ at a heating rate of 5℃ / min. After keeping at this temperature for 2.2 hours, it was naturally cooled to room temperature with the furnace. During the entire heating process, the pressure was gradually applied to 52MPa. When the sintering temperature reached 1860℃, the pressure applied was just 52MPa. The pressure was maintained for 2.2 hours. After the sintering was completed, the pressure was directly released to obtain a new type of high-strength and high-toughness SiC ceramic material product.
[0103] There are no obvious rod-shaped whiskers inside the ceramic prepared in this example, indicating that the added whiskers have reacted to generate the reaction products mentioned in the article. In the new high-strength and high-toughness SiC ceramic material product prepared in this example, the shape of SiC is equiaxed grains with a size of 1.2μm; the remaining second phases Y2SiO5, Zr3Y4O 12 and ZrC are dispersed and evenly wrapped around the matrix SiC grains with a size of 1.35μm.
[0104] The new high-strength and high-toughness SiC ceramic material products prepared in this embodiment include SiC, Y2SiO5, Zr3Y4O 12 and ZrC, which are completely consistent with the several reaction products mentioned above.
[0105] The density of the new high-strength and high-toughness SiC ceramic material prepared in this embodiment is 99.3±0.02%, and the density is 3.49±0.02g / cm 3 , hardness is 22.3±0.2GPa, flexural strength is 890±47MPa, fracture toughness is 8.81±0.13MPa·m 0.5 .
[0106] Example 3
[0107] A new type of high-strength and high-toughness SiC ceramic material, the new type of high-strength and high-toughness SiC ceramic material comprises 77wt.% SiC, 11.5wt.% Y2SiO5, 6.8wt.% Zr3Y4O 12 and 1.7wt.% ZrC.
[0108] A method for preparing the novel high-strength and high-toughness SiC ceramic material based on the above-mentioned method comprises the following steps:
[0109] S1. Raw material weighing:
[0110] According to the total content of ZrO2 powder and Y2O3 powder of 16 vol.% (the ratio of ZrO2 powder to Y2O3 powder is 1:1 in molar ratio), 45 vol.% SiC whisker and the rest of α-SiC powder are weighed to obtain 50 g of raw material mixed powder; wherein, the purity of α-SiC powder is 99.5%, and the average particle size is 0.17 μm; the purity of ZrO2 powder is 98.8%, and the average particle size is 0.03 μm; the purity of Y2O3 powder is 99.3%, and the average particle size is 0.0025 μm; the purity of SiC whisker is 99%, the length is 4-35 μm, and the diameter is 0.3-0.7 μm;
[0111] S2, ball milling:
[0112] The raw material mixed powder of S1 is wet-milled. The wet-milling method requires mixing the raw material mixed powder with 50 g of anhydrous ethanol and 50 g of zirconia ball milling beads in a mass ratio of 1:1:1, placing the mixture in a nylon ball milling jar, and mixing the mixture at a speed of 280 r / min for 5 h to obtain a mixed slurry;
[0113] S3, Drying and Sieving:
[0114] The mixed slurry of S2 was dried and sieved at a drying temperature of 90°C for 10 hours. After drying, the mesh size of the sieve was 80 meshes to obtain a fine particle mixed powder;
[0115] S4. Graphite mold preparation:
[0116] According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined. The cavity size of the graphite mold is 0.46 mm larger than the product appearance size. A graphite mold that meets the product requirements is prepared. Then, the fine particle mixed powder of S3 is placed in the graphite mold and vibrated to obtain a graphite mold filled with fine particle mixed powder.
[0117] S5, hot pressing sintering:
[0118] The fine-particle mixed powder in the graphite mold filled with fine-particle mixed powder of S4 was hot-pressed and sintered at a high temperature below 1900℃. After 30 minutes, the temperature was raised to 250℃, and then to 1720℃ at a heating rate of 10℃ / min, and then to 1870℃ at a heating rate of 5℃ / min. After keeping at this temperature for 2.4 hours, it was naturally cooled to room temperature with the furnace. During the entire heating process, the pressure was gradually applied to 50MPa, and the pressure applied when the sintering temperature reached 1870℃ was just 48MPa. The pressure was maintained for 2.4 hours, and the pressure was directly released after the sintering was completed to obtain a new type of high-strength and high-toughness SiC ceramic material product.
[0119] There are no obvious rod-shaped whiskers inside the ceramic prepared in this example, indicating that the added whiskers have reacted to generate the reaction products mentioned in the article. In the new high-strength and high-toughness SiC ceramic material product prepared in this example, the shape of SiC is equiaxed grains with a size of 1.2μm; the remaining second phases Y2SiO5, Zr3Y4O 12 and ZrC are dispersed and evenly wrapped around the matrix SiC grains with a size of 1.5μm.
[0120] The new high-strength and high-toughness SiC ceramic material prepared in this embodiment is composed of SiC, Y2SiO5, Zr3Y4O 12 and ZrC, which is completely consistent with the several reaction products mentioned above.
[0121] The density of the new high-strength and high-toughness SiC ceramic material prepared in this embodiment is 99.7±0.15%, and the density is 3.48±0.01g / cm 3 , hardness is 20.8±0.3GPa, flexural strength is 870±38MPa, fracture toughness is 8.6±0.24MPa·m 0.5 .
[0122] Example 4
[0123] A new type of high-strength and high-toughness SiC ceramic material, the new type of high-strength and high-toughness SiC ceramic material wave expansion 76wt.% SiC, 10.5wt.% Y2SiO5, 6.73wt.% Zr3Y4O 12 and 1.86wt.% ZrC.
[0124] A method for preparing the novel high-strength and high-toughness SiC ceramic material based on the above-mentioned method comprises the following steps:
[0125] S1. Raw material weighing:
[0126] According to the total content of ZrO2 powder and Y2O3 powder of 14 vol.% (the ratio of ZrO2 powder to Y2O3 powder is 1:1 in molar ratio), 40 vol.% SiC whisker and the rest of α-SiC powder are weighed to obtain 50 g of raw material mixed powder; wherein the purity of α-SiC powder is 99.6%, and the average particle size is 0.093 μm; the purity of ZrO2 powder is 99.5%, and the average particle size is 0.05 μm; the purity of Y2O3 powder is 99.3%, and the average particle size is 0.025 μm; the purity of SiC whisker is 99%, the length is 4-35 μm, and the diameter is 0.3-0.7 μm;
[0127] S2, ball milling:
[0128] The raw material mixed powder of S1 was wet-milled. The wet-milling method required mixing the raw material mixed powder with 50 g of anhydrous ethanol and 50 g of zirconia ball milling beads in a mass ratio of 1:1:1, placing the mixture in a nylon ball milling jar, and mixing at a speed of 320 r / min for 4.5 h to obtain a mixed slurry;
[0129] S3, Drying and Sieving:
[0130] The mixed slurry of S2 was dried and sieved at a drying temperature of 70°C and a drying time of 11.5 h. After drying, the mesh size of the sieve was 80 meshes to obtain a fine particle mixed powder;
[0131] S4. Graphite mold preparation:
[0132] According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined. The mold cavity size of the graphite mold is 0.45 mm larger than the product appearance size. A graphite mold that meets the product requirements is prepared, and then the fine particle mixed powder of S3 is placed in the graphite mold and vibrated to obtain a graphite mold filled with fine particle mixed powder;
[0133] S5, hot pressing sintering:
[0134] The fine-particle mixed powder in the graphite mold filled with fine-particle mixed powder of S4 was hot-pressed and sintered at a high temperature below 1900℃. After 30 minutes, the temperature was raised to 300℃, and then to 1780℃ at a heating rate of 10℃ / min, and then to 1895℃ at a heating rate of 5℃ / min. After keeping at this temperature for 2.3 hours, it was naturally cooled to room temperature with the furnace. During the entire heating process, the pressure was gradually applied to 50MPa. When the sintering temperature reached 1895℃, the pressure applied was just 50MPa. The pressure was maintained for 2.3 hours. After the sintering was completed, the pressure was directly released to obtain a new type of high-strength and high-toughness SiC ceramic material product.
[0135] There are no obvious rod-shaped whiskers inside the ceramic prepared in this example, indicating that the added whiskers have reacted to generate the reaction products mentioned in the article. In the new high-strength and high-toughness SiC ceramic material product prepared in this example, the shape of SiC is equiaxed grains with a size of 1.32μm; the remaining second phases Y2SiO5, Zr3Y4O 12 and ZrC are dispersed and evenly wrapped around the matrix SiC grains with a size of 1.48μm.
[0136] The new high-strength and high-toughness SiC ceramic material prepared in this embodiment is composed of SiC, Y2SiO5, Zr3Y4O 12 and ZrC, which is completely consistent with the several reaction products mentioned above.
[0137] The density of the new high-strength and high-toughness SiC ceramic material prepared in this embodiment is 99.8±0.25%, and the density is 3.48±0.013g / cm 3 , hardness is 20.8±0.4GPa, flexural strength is 850±25MPa, fracture toughness is 8.4±0.30MPa·m 0.5 .
[0138] Example 5
[0139] A new type of high-strength and high-toughness SiC ceramic material, the new type of high-strength and high-toughness SiC ceramic material comprises 77.5wt.% SiC, 11.5wt.% Y2SiO5, 6.88wt.% Zr3Y4O 12 and 1.73wt.% ZrC.
[0140] A method for preparing the novel high-strength and high-toughness SiC ceramic material based on the above-mentioned method comprises the following steps:
[0141] S1. Raw material weighing:
[0142] According to the total content of ZrO2 powder and Y2O3 powder of 14.5 vol.% (the ratio of ZrO2 powder to Y2O3 powder is 1:1 in molar ratio), 45 vol.% SiC whisker and the rest of α-SiC powder are weighed to obtain 50 g of raw material mixed powder; wherein the purity of α-SiC powder is 99.3%, and the average particle size is 0.125 μm; the purity of ZrO2 powder is 99.6%, and the average particle size is 0.04 μm; the purity of Y2O3 powder is 99.4%, and the average particle size is 0.025 μm; the purity of SiC whisker is 99%, the length is 4-35 μm, and the diameter is 0.3-0.7 μm;
[0143] S2, ball milling:
[0144] The raw material mixed powder of S1 is wet-milled. The wet-milling method requires mixing the raw material mixed powder with 50 g of anhydrous ethanol and 50 g of zirconium oxide ball milling beads in a mass ratio of 1:1:1, placing the mixture in a nylon ball mill, and mixing the mixture at a speed of 300 r / min for 5 h to obtain a mixed slurry;
[0145] S3, Drying and Sieving:
[0146] The mixed slurry of S2 was dried and sieved at a drying temperature of 70°C for 11 hours. After drying, the mesh size of the sieve was 80 meshes to obtain a fine particle mixed powder;
[0147] S4. Graphite mold preparation:
[0148] According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined. The cavity size of the graphite mold is 0.47 mm larger than the product appearance size. A graphite mold that meets the product requirements is prepared. Then, the fine particle mixed powder of S3 is placed in the graphite mold and vibrated to obtain a graphite mold filled with fine particle mixed powder.
[0149] S5, hot pressing sintering:
[0150] The fine-particle mixed powder in the graphite mold filled with fine-particle mixed powder of S4 was hot-pressed and sintered at a high temperature below 1900℃. After 30 minutes, the temperature was raised to 290℃, and then to 1740℃ at a heating rate of 10℃ / min, and then to 1880℃ at a heating rate of 5℃ / min. After keeping at this temperature for 2.1 hours, it was naturally cooled to room temperature with the furnace. During the entire heating process, the pressure was gradually applied to 50MPa. When the sintering temperature reached 1880℃, the pressure applied was just 50MPa. The pressure was maintained for 2.1 hours. After the sintering was completed, the pressure was directly released to obtain a new type of high-strength and high-toughness SiC ceramic material product.
[0151] There are no obvious rod-shaped whiskers inside the ceramic prepared in this example, indicating that the added whiskers have reacted to generate the reaction products mentioned in the article. In the new high-strength and high-toughness SiC ceramic material product prepared in this example, the shape of SiC is equiaxed grains with a size of 1.23μm; the remaining second phases Y2SiO5, Zr3Y4O 12 and ZrC are dispersed and evenly wrapped around the matrix SiC grains with a size of 1.57μm.
[0152] The new high-strength and high-toughness SiC ceramic material products prepared in this embodiment include SiC, Y2SiO5, Zr3Y4O 12 and ZrC, which are completely consistent with the several reaction products mentioned above.
[0153] The density of the new high-strength and high-toughness SiC ceramic material prepared in this embodiment is 99.4±0.35%, and the density is 3.47±0.015g / cm 3 , hardness is 20.7±0.2GPa, flexural strength is 865±33MPa, fracture toughness is 8.75±0.33MPa·m 0.5 .
[0154] Example 6
[0155] A new type of high-strength and high-toughness SiC ceramic material, the new type of high-strength and high-toughness SiC ceramic material comprises 78wt.% SiC, 10.8wt.% Y2SiO5, 7wt.% Zr3Y4O 12 and 1.93wt.% ZrC.
[0156] A method for preparing the novel high-strength and high-toughness SiC ceramic material based on the above-mentioned method comprises the following steps:
[0157] S1. Raw material weighing:
[0158] According to the total content of ZrO2 powder and Y2O3 powder of 13 vol.% (the ratio of ZrO2 powder to Y2O3 powder is 1:1 in molar ratio), 40 vol.% SiC whisker and the rest of α-SiC powder are weighed to obtain 50 g of raw material mixed powder; wherein the purity of α-SiC powder is 99.5%, and the average particle size is 0.13 μm; the purity of ZrO2 powder is 99.6%, and the average particle size is 0.05 μm; the purity of Y2O3 powder is 99.4%, and the average particle size is 0.015 μm; the purity of SiC whisker is 99%, the length is 4-35 μm, and the diameter is 0.3-0.7 μm;
[0159] S2, ball milling:
[0160] The raw material mixed powder of S1 is wet-milled. The wet-milling method requires mixing the raw material mixed powder with 50 g of anhydrous ethanol and 50 g of zirconia ball milling beads in a mass ratio of 1:1:1, placing the mixture in a nylon ball milling jar, and mixing the mixture at a speed of 280 r / min for 5 h to obtain a mixed slurry;
[0161] S3, Drying and Sieving:
[0162] The mixed slurry of S2 was dried and sieved at a drying temperature of 70°C for 11 hours. After drying, the mesh size of the sieve was 80 meshes to obtain a fine particle mixed powder;
[0163] S4. Graphite mold preparation:
[0164] According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined. The cavity size of the graphite mold is 0.43 mm larger than the product appearance size. A graphite mold that meets the product requirements is prepared. Then, the fine particle mixed powder of S3 is placed in the graphite mold and vibrated to obtain a graphite mold filled with fine particle mixed powder.
[0165] S5, hot pressing sintering:
[0166] The fine-particle mixed powder in the graphite mold filled with fine-particle mixed powder of S4 was hot-pressed and sintered at a high temperature below 1900℃. After 30 minutes, the temperature was raised to 300℃, and then to 1750℃ at a heating rate of 10℃ / min, and then to 1900℃ at a heating rate of 5℃ / min. After keeping at this temperature for 2.1 hours, it was naturally cooled to room temperature with the furnace. During the entire heating process, the pressure was gradually applied to 53MPa. When the sintering temperature reached 1900℃, the pressure applied was just 53MPa. The pressure was maintained for 2.1 hours. After the sintering was completed, the pressure was directly released to obtain a new type of high-strength and high-toughness SiC ceramic material product.
[0167] There are no obvious rod-shaped whiskers inside the ceramic prepared in this example, indicating that the added whiskers have reacted to generate the reaction products mentioned in the article. In the new high-strength and high-toughness SiC ceramic material product prepared in this example, the shape of SiC is equiaxed grains with a size of 1.11μm; the remaining second phases Y2SiO5, Zr3Y4O 12 and ZrC are dispersed and evenly wrapped around the matrix SiC grains with a size of 1.23μm.
[0168] The new high-strength and high-toughness SiC ceramic material products prepared in this embodiment include SiC, Y2SiO5, Zr3Y4O 12 and ZrC, which are completely consistent with the several reaction products mentioned above.
[0169] The density of the new high-strength and high-toughness SiC ceramic material prepared in this embodiment is 99.4±0.35%, and the density is 3.48±0.015g / cm 3 , hardness is 20.9±0.3GPa, flexural strength is 875±42MPa, fracture toughness is 8.63±0.36MPa·m 0.5 .
[0170] Comparative Example 1
[0171] A method for preparing a high-strength and high-toughness SiC ceramic material, wherein the high-strength and high-toughness SiC ceramic material does not contain SiC whiskers, and thus the generated SiC ceramic does not contain Y2SiO5 and ZrC. The addition amounts of α-SiC powder, ZrO2 powder and Y2O3 powder are the same as those in Example 6, and the method for preparing the high-strength and high-toughness SiC ceramic material comprises the following steps:
[0172] S1. Raw material weighing:
[0173] According to the total content of ZrO2 powder and Y2O3 powder of 13 vol.% (the ratio of ZrO2 powder to Y2O3 powder is 1:1 in molar ratio) and the rest of α-SiC powder, 50 g of raw material mixed powder is obtained; wherein, the purity of α-SiC powder is 99.5%, and the average particle size is 0.13 μm; the purity of ZrO2 powder is 99.6%, and the average particle size is 0.05 μm; the purity of Y2O3 powder is 99.4%, and the average particle size is 0.015 μm;
[0174] S2, ball milling:
[0175] The raw material mixed powder of S1 is wet-milled. The wet-milling method requires mixing the raw material mixed powder with 50 g of anhydrous ethanol and 50 g of zirconia ball milling beads in a mass ratio of 1:1:1, placing the mixture in a nylon ball milling jar, and mixing the mixture at a speed of 280 r / min for 5 h to obtain a mixed slurry;
[0176] S3, Drying and Sieving:
[0177] The mixed slurry of S2 was dried and sieved at a drying temperature of 70°C for 11 hours. After drying, the mesh size of the sieve was 80 meshes to obtain a fine particle mixed powder;
[0178] S4. Graphite mold preparation:
[0179] According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined. The cavity size of the graphite mold is 0.43 mm larger than the product appearance size. A graphite mold that meets the product requirements is prepared. Then, the fine particle mixed powder of S3 is placed in the graphite mold and vibrated to obtain a graphite mold filled with fine particle mixed powder.
[0180] S5, hot pressing sintering:
[0181] The fine-particle mixed powder in the graphite mold filled with fine-particle mixed powder of S4 was hot-pressed and sintered at a high temperature below 1900℃. After 30 minutes, the temperature was raised to 300℃, and then to 1750℃ at a heating rate of 10℃ / min, and then to 1900℃ at a heating rate of 5℃ / min. After keeping at this temperature for 2.1 hours, it was naturally cooled to room temperature with the furnace. During the entire heating process, the pressure was gradually applied to 53MPa. When the sintering temperature reached 1900℃, the pressure applied was just 53MPa. The pressure was maintained for 2.1 hours. After the sintering was completed, the pressure was directly released to obtain a high-strength and high-toughness SiC ceramic material product.
[0182] like Figure 4 As shown, the second phase Y2SiO5 and ZrC do not exist in the high-strength and high-toughness SiC ceramic material product prepared in this comparative example.
[0183] The high-strength and high-toughness SiC ceramic material prepared in this embodiment has a density of 99.0±0.35% and a density of 3.46±0.015 g / cm 3 , hardness is 20.4±0.3GPa, bending strength is only 656±32MPa, fracture toughness is 6.30±0.36MPa·m 0.5 .
[0184] The above scheme, the present invention provides a new type of high-strength and high-toughness SiC ceramic material and preparation method, which overcomes the technical defect that the current SiC ceramic material cannot synergistically improve the density, flexural strength and fracture toughness at low cost and high efficiency, expands the application scope of SiC ceramic materials, and is conducive to large-scale industrial production and promotion.
[0185] The invention adds ZrO2 powder, Y2O3 powder and SiC whisker to α-SiC powder to react during hot pressing sintering to obtain 75-82wt.% SiC, 10-12wt.% Y2SiO5, 6-7wt.% Zr3Y4O 12 and 1-2wt.% ZrC; among them, Y2SiO5 plays the role of filling the gaps between SiC grains to ensure the density of the material. 12 The role is to provide the right interface bonding strength with the matrix SiC grains, thereby improving the fracture toughness. ZrC can pin the grain boundaries to refine the grains and improve the bending strength of the material.
[0186] The present invention can fully mix various powders through wet ball milling. In particular, SiC whiskers are very easy to agglomerate due to their large specific surface area, thereby hindering mass transfer during the sintering process and resulting in poor density of SiC ceramics. Wet ball milling can ensure that the whiskers are evenly dispersed and will not agglomerate during the sintering process.
[0187] The hot pressing sintering temperature of the invention is lower than 1900° C., and SiC ceramics with excellent performance are obtained on the basis of reducing production costs.
[0188] The density of the new high-strength and high-toughness SiC ceramic material prepared by the present invention exceeds 99%, and the density is more than 3.45-3.51g / cm 3 , hardness exceeds 20GPa, bending strength exceeds 800MPa, fracture toughness exceeds 8MPa·m 0.5 .
[0189] In summary, compared with other traditional methods, the method of the present invention can obtain a composite material composed of Y2SiO5, Zr3Y4O3, and SiC whiskers by adding ZrO2 powder, Y2O3 powder, and SiC whiskers to α-SiC powder in the subsequent hot pressing sintering process. 12 SiC ceramic materials with ZrC as the second phase for strengthening and toughening have a hardness of more than 20GPa, a bending strength of more than 800MPa, and a fracture toughness of more than 8MPa·m on the basis of a density of more than 99%. 0.5 The process has simple steps, convenient operation, short process cycle, low cost, high efficiency, and easy control, which is conducive to industrial production and can produce SiC ceramics with the best comprehensive properties (especially flexural strength and fracture toughness) reported so far.
[0190] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A new type of high-strength and high-toughness SiC ceramic material, It is characterized in that The novel high-strength and high-toughness SiC ceramic material comprises 75-82wt.% SiC, 10-12wt.% Y 2 SiO 5 、6-7wt.% Zr 3 Y 4 O 12 and 1-2wt.% ZrC, and materials of different sizes can be prepared using different molds.
2. The novel high-strength and high-toughness SiC ceramic material according to claim 1, It is characterized in that The shape of SiC is equiaxed grains with a size of 1-1.5 μm; the rest of the second phase Y 2 SiO 5 、Zr 3 Y 4 O 12 and ZrC are dispersed and evenly wrapped around the matrix SiC grains with a size of 0.5-2μm.
3. The novel high-strength and high-toughness SiC ceramic material according to claim 1, It is characterized in that The new high-strength and high-toughness SiC ceramic material has a density of more than 99% and a density of 3.45-3.51 g / cm 3 , hardness exceeds 20GPa, bending strength exceeds 800MPa, fracture toughness exceeds 8MPa·m 0.5 .
4. A method for preparing a novel high-strength and high-toughness SiC ceramic material according to any one of claims 1 to 3, It is characterized in that The preparation method of the novel high-strength and high-toughness SiC ceramic material comprises the following steps: S1. Raw material weighing: Select α-SiC powder, ZrO 2 Pink, Y 2 O 3 Powder and SiC whisker are weighed as raw material powders to obtain raw material mixed powder; S2, ball milling: The raw material mixed powder of S1 is wet ball-milled to obtain a mixed slurry; S3, Drying and Sieving: The mixed slurry of S2 is dried and sieved to obtain a fine particle mixed powder; S4. Preparation of graphite mold: According to the product requirements of the prepared new high-strength and high-toughness SiC ceramic material, the shape and size of the graphite mold are determined, and a graphite mold that meets the product requirements is prepared. Then, the fine particle mixed powder of S3 is placed in the graphite mold and vibrated. A layer of graphite paper needs to be placed between the graphite mold and the powder to prevent the sintered sample from sticking to the mold; S5, hot pressing sintering: The fine-particle mixed powder in the graphite mold filled with fine-particle mixed powder of S4 is hot-pressed and sintered at a high temperature below 1900°C. After the sintering is completed, the pressure is directly released, and a new type of high-strength and high-toughness SiC ceramic material product is obtained after cooling.
5. The method for preparing the novel high-strength and high-toughness SiC ceramic material according to claim 4, It is characterized in that The purity of α-SiC powder in S1 is 98.5-99.9%, and the average particle size is 0.05-0.2μm; ZrO 2 The purity of the powder is 98-99.9%, and the average particle size is 0.01-0.06μm; 2 O 3 The purity of the powder is 98-99.9%, and the average particle size is 0.01-0.03μm; the purity of the SiC whisker is 99%, the length is 4-35μm, and the diameter is 0.3-0.7μm.
6. The method for preparing the novel high-strength and high-toughness SiC ceramic material according to claim 4, It is characterized in that ZrO in S1 2 Pink and Y 2 O 3 The volume percentage of ZrO in the raw material mixed powder is 13-17 vol%. 2 Pink and Y 2 O 3 The molar ratio of the powder is 1:1; the volume percentage of the added SiC whisker in the raw material mixed powder is between 40-50vol.%.
7. The method for preparing the novel high-strength and high-toughness SiC ceramic material according to claim 4, It is characterized in that The wet ball milling in S2 requires mixing the raw material mixed powder with anhydrous ethanol and zirconium oxide ball milling beads (or silicon carbide ball milling beads, agate ball milling beads) in a mass ratio of 1:1:1, placing it in a nylon ball mill jar, and mixing it at a speed of 250-350 r / min for 4-8 hours.
8. The method for preparing the novel high-strength and high-toughness SiC ceramic material according to claim 4, It is characterized in that The drying temperature in S3 is 60-100°C, the drying time is 10-12h, and the mesh size of the sieve after drying is 80-100 mesh.
9. The method for preparing the novel high-strength and high-toughness SiC ceramic material according to claim 4, It is characterized in that The cavity size of the graphite mold in S4 is 0.4-0.5mm larger than the product appearance size.
10. The method for preparing the novel high-strength and high-toughness SiC ceramic material according to claim 4, It is characterized in that The heating rate of hot pressing sintering in S5 is 5-10°C / min, the sintering temperature is 1850-1900°C, the pressure is 40-60MPa, and the heat preservation and pressure holding time is 2-2.5h.
Citation Information
Patent Citations
Method adopting liquid phase sintering for manufacturing silicon carbide ceramics with zirconium oxide as toughening phase
CN104140265A
Liquid-phase sintering slip casting SiC ceramic valve material and preparation method thereof
CN113024257A
Preparation method of multiphase composite reinforced silicon carbide ceramic
CN113683435A
Plasma resistant ceramics sprayed coating
JP2009068066A
Method of producing hot-pressed silicon carbide ceramics
RU2816616C1
Cited By
High-strength ceramic matrix composite bolt and processing technology