A tire and its vulcanization method and application
By using tread glue formulas such as styrene butadiene rubber, Eucommia rubber, and phenyl POSS-grafted polyethylene polyamine and other raw materials, combined with specific vulcanization methods, the wear resistance and crack resistance of the tread glue for bias agricultural tires is solved. The problem of insufficient results enables higher wear and crack resistance, extends service life and reduces rolling resistance.
Patent Information
- Application Number
- CN202411237042.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The wear resistance and crack resistance of existing oblique agricultural tire tread glue is insufficient, resulting in a short service life and it is difficult to effectively resist damage to sharp objects such as stones and root thorns in field operations.
The tread glue formula is used to graft the raw materials such as styrene butadiene rubber, Eucommia ulmoide, white carbon black, phenyl POSS, polyethylene polyamine, carbon nanotubes and chloride paraffin, and an optimized crosslinking network is formed through specific vulcanization methods. To improve wear resistance and crack resistance.
It significantly improves the wear resistance, crack resistance and service life of the tire, reduces rolling resistance, and enhances the reliability and durability of the tire in a variety of use environments.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of tires, and in particular to a tire and a vulcanization method and application thereof. Background Art
[0002] Bias-ply agricultural tires are crucial in the field of agricultural machinery. They are widely used on tractors, harvesters and other equipment because of their adaptability to diverse operating environments and sturdy structural design. Bias-ply tires are characterized by their multi-layered cord ply structure with cross-angle superposition. This structure not only enhances the strength and durability of the tire, but also improves its resistance to lateral impact, giving it excellent handling performance on uneven terrain in the field. However, as modern agriculture has increasingly higher requirements for efficiency and sustainable development, further optimizing the performance of these tires has become an important research direction.
[0003] Tread rubber is an important component of bias agricultural tires because it directly affects the tire's grip, wear resistance and service life. Traditional tread rubber is mainly made of a combination of natural rubber and synthetic rubber, and reinforced materials such as carbon black are added to improve its wear resistance and anti-aging properties. Although this combination effectively improves the basic performance of the tire, its durability and crack resistance under long-term heavy load and high wear conditions still need to be improved. In addition, tires may be damaged by sharp objects such as stones and root thorns during field operations, so improving the cut resistance of the tread rubber has also become an essential area of improvement.
[0004] In order to meet these technical challenges, current research and development efforts are focused on exploring the application of new materials and modified fillers. The invention patent with patent number CN109593242A discloses a bias heavy truck tire tread rubber. Although increasing the styrene content can improve the elastic modulus and tear resistance, too high styrene will lead to increased plasticity, which in turn affects the wear resistance and overall durability. Therefore, it is necessary to develop more durable and efficient bias agricultural tires, which will effectively improve the production efficiency and operational reliability of agricultural machinery and meet the demand for high-performance tires in modern agriculture. Summary of the invention
[0005] In view of this, the present invention proposes a tire and a vulcanization method and application thereof to solve the technical problem of poor wear resistance and crack resistance of the tread rubber of the existing bias agricultural tire and to improve the service life of the tire.
[0006] The technical solution of the present invention is achieved as follows: the present invention provides a tire, which includes a tire body and a tread. Calculated by weight, the tread rubber of the tread includes the following raw materials: 90-120 parts of styrene-butadiene rubber, 20-30 parts of eucommia rubber, 30-40 parts of white carbon black, 5-8 parts of vulcanizing agent, 1-3 parts of vulcanization accelerator, 1-2 parts of zinc oxide, 10-15 parts of phenyl POSS grafted polyethylene polyamine, 8-10 parts of carbon nanotubes and 5-8 parts of chlorinated paraffin.
[0007] Eucommia rubber has the characteristics of rubber and plastic duality, which can effectively improve the wear resistance of the tread and extend the service life of the tire. Styrene-butadiene rubber provides good elasticity and flexibility. When combined with Eucommia rubber, it can better adapt to the impact and vibration of the tire on uneven ground and improve driving stability.
[0008] The nanostructure of phenyl POSS forms an optimized network with polyethylene polyamine through cross-linking, which makes the whole material bear greater stress during friction and less prone to wear. In addition, the cross-linking between phenyl POSS and polyethylene polyamine enhances stress dispersion, and the flexibility of polyethylene polyamine allows the material to deform more under stress, thereby delaying the formation of cracks and inhibiting crack propagation. At the same time, the combination of phenyl POSS and polyethylene polyamine makes the molecular structure of the material more orderly, the deformation during rolling is smoother, and the friction that needs to be overcome in rolling is reduced.
[0009] The lubrication effect of chlorinated paraffin significantly reduces the internal friction and dynamic viscosity of the material, allowing the molecular chains to flow more smoothly under load and reducing energy loss caused by friction. In addition, chlorinated paraffin as a plasticizer improves the ductility of the material and reduces its brittleness.
[0010] Phenyl POSS grafted polyethylene polyamine and chlorinated paraffin complement each other, thus producing a significant synergistic effect in improving the wear resistance and crack resistance of the material and reducing rolling resistance. This synergistic mechanism not only improves the overall performance of the tire, but also enhances its reliability and durability in a variety of usage environments.
[0011] In addition, the organic-inorganic hybrid properties of POSS give it good interfacial compatibility with rubber, silica and carbon nanotubes, thereby promoting the uniform dispersion of the reinforcing material and improving the overall strength and wear resistance of the composite material.
[0012] Zinc oxide, as an important active agent in the vulcanization system, when used together with chlorinated paraffin, enhances the network cross-linking efficiency of the vulcanization process and improves the heat resistance and strength of the rubber.
[0013] On the basis of the above technical scheme, preferably, the preparation method of the phenyl POSS grafted polyethylene polyamine comprises the following steps:
[0014] S1, dissolving phenyl POSS in anhydrous dichloromethane to obtain a phenyl POSS solution, and dissolving polyethylene polyamine in anhydrous ethanol to obtain a polyethylene polyamine solution;
[0015] S2, mixing the phenyl POSS solution and the polyethylene polyamine solution, adding triethylamine, stirring and reacting at 20-30°C for 0.5-1h, then heating to 50-70°C, and continuing the reaction for 3-4h. After the reaction is completed, cooling, drying, and rotary evaporation to remove the solvent obtain phenyl POSS grafted polyethylene polyamine.
[0016] On the basis of the above technical scheme, preferably, in step S2, 1-butyl-3-methylimidazole chloride is added to the phenyl POSS solution, and the solution is stirred evenly and then mixed with the polyethylene polyamine solution.
[0017] Specifically, the ionic liquid enhances the interaction between POSS and polyethylene polyamine during the reaction, making the cross-linked network more uniform and stable. It also improves the dispersion and interaction of other components during the mixing process, especially the dispersion of inorganic reinforcing materials. This improvement can enhance the strength of the material. In addition, by improving the fluidity of the molecular chain, the ionic liquid can effectively disperse stress, reduce the formation of microcracks, and enhance crack resistance. By optimizing the motion state of the molecular chain, the ionic liquid reduces internal friction and enhances the dynamic responsiveness of the material, thereby effectively reducing rolling resistance.
[0018] On the basis of the above technical scheme, preferably, the mass ratio of phenyl POSS: polyethylene polyamine: triethylamine is 1:1.5-2.5:0.05-0.15, the mass ratio of phenyl POSS: anhydrous dichloromethane is 1:10-50, the mass ratio of polyethylene polyamine: anhydrous ethanol is 1:5-10, and the mass ratio of chloride (1-butyl-3-methylimidazole): phenyl POSS is 0.1-1:1.
[0019] On the basis of the above technical solution, preferably, the chlorinated paraffin is pretreated by: treating the chlorinated paraffin with arc plasma at a DC voltage of 30-50 kV for 5-10 min to obtain activated chlorinated paraffin.
[0020] Specifically, arc plasma pretreatment increases the surface activity of chlorinated paraffin, thereby enhancing its bonding with natural rubber and butyl rubber. After treatment, chlorinated paraffin can synergize with stearic acid to improve interface bonding and cross-linking stability, enhance the overall strength and toughness of the material, and thus reduce the propagation and expansion of cracks.
[0021] In addition, the pretreated chlorinated paraffin is more easily dispersed in the colloid, which enhances the lubricity of the material and can effectively reduce internal friction and energy loss, thereby reducing rolling resistance.
[0022] On the basis of the above technical scheme, preferably, the phenyl POSS is one or two of POSS-phenyl and octa-p-aminophenyl-POSS; the vulcanizing agent is sulfur or phenolic resin, and the vulcanization accelerator is one or more of N-cyclohexyl-2-benzothiazole sulfonamide, N,N'-diphenyl-thiourea and 2-mercaptobenzothiazole.
[0023] On the other hand, the present invention also provides a tire vulcanization method, characterized in that it comprises the following steps:
[0024] S1, mixing styrene-butadiene rubber, eucommia rubber, white carbon black, zinc oxide, and phenyl POSS grafted polyethylene polyamine for a first time, then adding carbon nanotubes and quercetin for a second time, and then adding chlorinated paraffin, a vulcanizing agent, and a vulcanization accelerator for a third time, and after the mixing is completed, pressing a sheet to obtain a mixed film;
[0025] S2, bonding the mixed rubber sheet to the outer side of the tire body, placing it in a mold, and vulcanizing it at 138°C to 148°C for 50 to 80 minutes to obtain a tire.
[0026] Specifically, quercetin in the compound can not only act as an antioxidant to delay the occurrence of adverse side reactions during the vulcanization process, but also cooperate with the vulcanizer and vulcanization accelerator to optimize the structure of the vulcanization network and promote more uniform cross-linking, thereby enhancing the fatigue resistance of the tread rubber. In addition, the microstructure formed by quercetin in the material helps to enhance the formation of crystals and improve the wear resistance of the tread rubber. The antioxidant properties of quercetin also reduce the heat caused by friction, thereby reducing the friction enhancement and increased rolling resistance caused by aging.
[0027] On the basis of the above technical solution, preferably, the mass ratio of quercetin to carbon nanotubes is 0.5-1:8-10.
[0028] On the basis of the above technical solution, preferably, the temperature of the first mixing is 60-80°C, and the time is 3-5 min; the temperature of the second mixing is 100-120°C, and the time is 6-8 min; the temperature of the third mixing is 130-150°C, and the time is 5-10 min.
[0029] In yet another aspect, the present invention further provides an application of a tire tread rubber in preparing a bias agricultural tire.
[0030] The tire and the vulcanization method and application thereof of the present invention have the following beneficial effects compared with the prior art:
[0031] (1) Phenyl POSS has good dispersibility and compatibility with organic polymers. By enhancing the interaction between molecular chains, phenyl POSS grafted with polyethylene polyamine can increase the wear resistance and crack resistance of tread rubber. In addition, chlorinated paraffin, as a plasticizer and protective agent, can improve the flexibility and weather resistance of the rubber, thereby increasing the resistance of the tread rubber to physical damage and its service life. Their combined effect makes the molecular structure of the rubber more compact, effectively reducing the development of wear and cracks, while slightly reducing the internal friction of the material, thereby reducing rolling resistance.
[0032] (2) The introduction of 1-butyl-3-methylimidazole chloride ionic liquid helps to improve the interfacial compatibility between phenyl POSS and polyethylene polyamine and promotes the reaction to form stable chemical bonds. This stability enhances the cross-linking density of the rubber material and increases the strength and wear resistance of the tread rubber.
[0033] (3) Activating chlorinated paraffin with arc plasma can introduce active groups and improve its adhesion to the rubber matrix. This activation treatment strengthens the cross-linking structure inside the material, improves the overall mechanical strength of the rubber, and improves wear resistance. A stronger cross-linking network also means greater resistance to crack extension, thereby enhancing the crack resistance of the tread rubber. At the same time, efficient chemical bonding makes the internal structure of the material more compact, reduces the energy loss caused by friction, and also helps to reduce rolling resistance.
[0034] (4) Quercetin is a natural antioxidant and free radical scavenger. Its introduction helps improve the anti-aging properties of rubber. This not only improves the durability of the tread rubber, but also inhibits the oxidative degradation process and reduces the formation of crack sources, thereby enhancing crack resistance. At the same time, its own biocompatibility and enhancement properties help to further optimize the physical properties of the tread and reduce rolling resistance. DETAILED DESCRIPTION
[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] The eucommia rubber (synthetic 1,4-trans polyisoprene rubber) used in the present invention is purchased from Wuhan Yuancheng Gongchuang Technology Co., Ltd.; the styrene-butadiene rubber, model NS612, is a product of ZEON Chemical Co., Ltd.; and the white carbon black, model 200MP, is a product of Solvay Chemical.
[0037] In the examples of the present invention and comparative examples, 1 part by weight is 100 g.
[0038] Example 1
[0039] The tread rubber of this embodiment includes the following raw materials, calculated by weight: 110 parts of styrene-butadiene rubber, 26 parts of eucommia rubber, 35 parts of white carbon black, 7 parts of sulfur, 2 parts of N-cyclohexyl-2-benzothiazole sulfonamide, 1.5 parts of zinc oxide, 13 parts of phenyl POSS grafted polyethylene polyamine, 9 parts of carbon nanotubes and 7 parts of chlorinated paraffin.
[0040] Wherein, the preparation method of phenyl POSS grafted polyethylene polyamine comprises the following steps:
[0041] S1, 10g of eight-p-aminophenyl-POSS is dissolved in 300g of anhydrous dichloromethane to obtain eight-p-aminophenyl-POSS solution, and 20g of polyethylene polyamine is dissolved in 120g of anhydrous ethanol to obtain a polyethylene polyamine solution;
[0042] S2, mixing the octa-aminophenyl-POSS solution prepared in step S1 with the polyethylene polyamine solution, adding 1 g of triethylamine, stirring and reacting at 30° C. for 1 h, then heating to 50° C. and continuing the reaction for 3 h. After the reaction is completed, cooling, drying, and rotary evaporation to remove the solvent obtain phenyl POSS grafted polyethylene polyamine.
[0043] The tread rubber mixing method is as follows: styrene-butadiene rubber, eucommia rubber, white carbon black, zinc oxide and phenyl POSS grafted polyethylene polyamine are mixed once, the mixing temperature is 75°C, and the time is 5 minutes; then carbon nanotubes are added for secondary mixing, the mixing temperature is 110°C, and the time is 8 minutes; chlorinated paraffin, sulfur and N-cyclohexyl-2-benzothiazole sulfonamide are continuously added for the third mixing, the mixing temperature is 135°C, and the time is 10 minutes. After the mixing is completed, the mixed rubber sheet is obtained by pressing.
[0044] Example 2
[0045] The difference between this embodiment and embodiment 1 is that 1-butyl-3-methylimidazole chloride ionic liquid is added during the preparation of phenyl POSS grafted polyethylene polyamine, and the rest of the contents are the same.
[0046] Specifically, the preparation method of phenyl POSS grafted polyethylene polyamine comprises the following steps:
[0047] S1, 10g of eight-p-aminophenyl-POSS is dissolved in 300g of anhydrous dichloromethane to obtain eight-p-aminophenyl-POSS solution, and 20g of polyethylene polyamine is dissolved in 120g of anhydrous ethanol to obtain a polyethylene polyamine solution;
[0048] S2, add 5g of (1-butyl-3-methylimidazole) chloride to the octa-p-aminophenyl-POSS solution prepared in step S1, stir evenly and mix with the polyethylene polyamine solution, then add 1g of triethylamine, stir and react at 30°C for 1h, then heat to 50°C and continue to react for 3h. After the reaction is completed, cool, dry and evaporate to remove the solvent to obtain phenyl POSS grafted polyethylene polyamine.
[0049] Example 3
[0050] The difference between this embodiment and embodiment 2 is that the chlorinated paraffin is mixed after being pretreated, and the rest of the contents are the same.
[0051] Specifically, the tread rubber mixing method is:
[0052] S1, chlorinated paraffin pretreatment: chlorinated paraffin was treated with arc plasma at a DC voltage of 40 kV for 8 min to obtain activated chlorinated paraffin.
[0053] S2, mixing styrene-butadiene rubber, eucommia rubber, white carbon black, zinc oxide and phenyl POSS grafted polyethylene polyamine once, the mixing temperature is 75°C, the time is 5 minutes; then adding carbon nanotubes for secondary mixing, the mixing temperature is 110°C, the time is 8 minutes; continuing to add activated chlorinated paraffin, sulfur and N-cyclohexyl-2-benzothiazole sulfonamide for third mixing, the mixing temperature is 135°C, the time is 10 minutes, and after the mixing is completed, the mixed film is pressed into a sheet.
[0054] Example 4
[0055] The difference between this embodiment and embodiment 3 is that quercetin is added during the secondary mixing, and the rest of the contents are the same.
[0056] Specifically, the tread rubber mixing method is:
[0057] S1, chlorinated paraffin pretreatment: chlorinated paraffin was treated with arc plasma at a DC voltage of 40 kV for 8 min to obtain activated chlorinated paraffin.
[0058] S2, mixing styrene-butadiene rubber, eucommia rubber, white carbon black, zinc oxide and phenyl POSS grafted polyethylene polyamine once, the mixing temperature is 75°C, the time is 5 minutes; then adding 0.8 parts of quercetin carbon nanotubes for a second mixing, the mixing temperature is 110°C, the time is 8 minutes; continuing to add activated chlorinated paraffin, sulfur and N-cyclohexyl-2-benzothiazole sulfonamide for a third mixing, the mixing temperature is 135°C, the time is 10 minutes, and after the mixing is completed, the mixed film is pressed into a sheet.
[0059] Example 5
[0060] The tread rubber of this embodiment includes the following raw materials, calculated by weight: 90 parts of styrene-butadiene rubber, 22 parts of eucommia rubber, 30 parts of white carbon black, 6 parts of phenolic resin, 1 part of N,N'-diphenyl-thiourea, 1.3 parts of zinc oxide, 10 parts of phenyl POSS grafted polyethylene polyamine, 8 parts of carbon nanotubes and 8 parts of chlorinated paraffin.
[0061] Wherein, the preparation method of phenyl POSS grafted polyethylene polyamine comprises the following steps:
[0062] S1, 10g of phenyl POSS is dissolved in 100g of anhydrous dichloromethane to obtain a phenyl POSS solution, and 25g of polyethylene polyamine is dissolved in 125g of anhydrous ethanol to obtain a polyethylene polyamine solution;
[0063] S2, add 8g of (1-butyl-3-methylimidazole) chloride to the phenyl POSS solution prepared in step S1, stir evenly and mix with the polyethylene polyamine solution, then add 0.5g of triethylamine, stir and react at 20°C for 0.5h, then heat to 70°C and continue to react for 4h. After the reaction is completed, cool, dry and evaporate to remove the solvent to obtain phenyl POSS grafted polyethylene polyamine.
[0064] The tread rubber mixing method comprises the following steps:
[0065] S1, chlorinated paraffin pretreatment: chlorinated paraffin was treated with arc plasma at a DC voltage of 30 kV for 8 min to obtain activated chlorinated paraffin.
[0066] S2, mixing styrene-butadiene rubber, eucommia rubber, white carbon black, zinc oxide and phenyl POSS grafted polyethylene polyamine once, the mixing temperature is 60℃, the time is 5min; then adding 1 part of carbon nanotubes and quercetin for a second mixing, the mixing temperature is 100℃, the time is 7min; continuing to add activated chlorinated paraffin, phenolic resin and N,N'-diphenyl-thiourea for a third mixing, the mixing temperature is 130℃, the time is 8min, and after mixing, pressing to obtain a mixed film.
[0067] Example 6
[0068] The tread rubber of this embodiment includes the following raw materials, calculated by weight: 100 parts of styrene-butadiene rubber, 30 parts of eucommia rubber, 33 parts of white carbon black, 5 parts of sulfur, 1.5 parts of 2-mercaptobenzothiazole, 1 part of zinc oxide, 11 parts of phenyl POSS grafted polyethylene polyamine, 10 parts of carbon nanotubes and 6 parts of chlorinated paraffin.
[0069] Wherein, the preparation method of phenyl POSS grafted polyethylene polyamine comprises the following steps:
[0070] S1, 10g of phenyl POSS is dissolved in 500g of anhydrous dichloromethane to obtain a phenyl POSS solution, and 18g of polyethylene polyamine is dissolved in 150g of anhydrous ethanol to obtain a polyethylene polyamine solution;
[0071] S2, add 1g of (1-butyl-3-methylimidazole) chloride to the phenyl POSS solution prepared in step S1, stir evenly and mix with the polyethylene polyamine solution, then add 1.5g of triethylamine, stir and react at 25°C for 1h, then heat to 55°C and continue to react for 3.5h. After the reaction is completed, cool, dry and evaporate to remove the solvent to obtain phenyl POSS grafted polyethylene polyamine.
[0072] The tread rubber mixing method comprises the following steps:
[0073] S1, chlorinated paraffin pretreatment: chlorinated paraffin was treated with arc plasma at a DC voltage of 50 kV for 8 minutes to obtain activated chlorinated paraffin.
[0074] S2, mixing styrene-butadiene rubber, eucommia rubber, white carbon black, zinc oxide and phenyl POSS grafted polyethylene polyamine once, the mixing temperature is 80°C, and the time is 3 minutes; then adding 0.7 parts of carbon nanotubes and quercetin for a second mixing, the mixing temperature is 120°C, and the time is 6 minutes; continuing to add activated chlorinated paraffin, sulfur and 2-mercaptobenzothiazole for a third mixing, the mixing temperature is 150°C, and the time is 5 minutes. After the mixing is completed, the mixed film is pressed into a sheet.
[0075] Example 7
[0076] The tread rubber of this embodiment includes the following raw materials, calculated by weight: 120 parts of styrene-butadiene rubber, 28 parts of eucommia rubber, 40 parts of white carbon black, 7 parts of sulfur, 3 parts of N-cyclohexyl-2-benzothiazole sulfonamide, 1.6 parts of zinc oxide, 15 parts of phenyl POSS grafted polyethylene polyamine, 9 parts of carbon nanotubes and 5 parts of chlorinated paraffin.
[0077] Wherein, the preparation method of phenyl POSS grafted polyethylene polyamine comprises the following steps:
[0078] S1, 10g of phenyl POSS is dissolved in 400g of anhydrous dichloromethane to obtain a phenyl POSS solution, and 25g of polyethylene polyamine is dissolved in 200g of anhydrous ethanol to obtain a polyethylene polyamine solution;
[0079] S2, add 10g of (1-butyl-3-methylimidazole) chloride to the phenyl POSS solution prepared in step S1, stir evenly and mix with the polyethylene polyamine solution, then add 1g of triethylamine, stir and react at 30°C for 0.5h, then heat to 65°C and continue to react for 4h. After the reaction is completed, cool, dry and evaporate to remove the solvent to obtain phenyl POSS grafted polyethylene polyamine.
[0080] The tread rubber mixing method comprises the following steps:
[0081] S1, chlorinated paraffin pretreatment: chlorinated paraffin was treated with arc plasma at a DC voltage of 35 kV for 8 min to obtain activated chlorinated paraffin.
[0082] S2, mixing styrene-butadiene rubber, eucommia rubber, white carbon black, zinc oxide and phenyl POSS grafted polyethylene polyamine once, the mixing temperature is 75°C, and the time is 5 minutes; then adding 0.9 parts of carbon nanotubes and quercetin for a second mixing, the mixing temperature is 120°C, and the time is 8 minutes; continuing to add activated chlorinated paraffin, sulfur and N-cyclohexyl-2-benzothiazole sulfonamide for a third mixing, the mixing temperature is 145°C, and the time is 10 minutes. After the mixing is completed, the mixed film is pressed into a sheet.
[0083] Example 8
[0084] The tread rubber of this embodiment includes the following raw materials, calculated by weight: 115 parts of styrene-butadiene rubber, 20 parts of eucommia rubber, 38 parts of white carbon black, 8 parts of phenolic resin, 2.5 parts of N,N'-diphenyl-thiourea, 2 parts of zinc oxide, 14 parts of phenyl POSS grafted polyethylene polyamine, 8.5 parts of carbon nanotubes and 7.5 parts of chlorinated paraffin.
[0085] Wherein, the preparation method of phenyl POSS grafted polyethylene polyamine comprises the following steps:
[0086] S1, 10g of phenyl POSS is dissolved in 200g of anhydrous dichloromethane to obtain a phenyl POSS solution, and 22g of polyethylene polyamine is dissolved in 150g of anhydrous ethanol to obtain a polyethylene polyamine solution;
[0087] S2, add 3g of (1-butyl-3-methylimidazole) chloride to the phenyl POSS solution prepared in step S1, stir evenly and mix with the polyethylene polyamine solution, then add 1g of triethylamine, stir and react at 30°C for 1h, then heat to 60°C and continue to react for 3h. After the reaction is completed, cool, dry and evaporate to remove the solvent to obtain phenyl POSS grafted polyethylene polyamine.
[0088] The tread rubber mixing method comprises the following steps:
[0089] S1, chlorinated paraffin pretreatment: chlorinated paraffin was treated with arc plasma at a DC voltage of 45 kV for 8 minutes to obtain activated chlorinated paraffin.
[0090] S2, mixing styrene-butadiene rubber, eucommia rubber, white carbon black, zinc oxide and phenyl POSS grafted polyethylene polyamine once, the mixing temperature is 65°C, the time is 5 minutes; then adding 0.5 parts of carbon nanotubes and quercetin for a second mixing, the mixing temperature is 115°C, the time is 8 minutes; continuing to add activated chlorinated paraffin, phenolic resin and N,N'-diphenyl-thiourea for a third mixing, the mixing temperature is 145°C, the time is 10 minutes, and after the mixing is completed, the mixed film is pressed into a sheet.
[0091] Comparative Example 1
[0092] Compared with Example 1, Comparative Example 1 lacks phenyl POSS grafted polyethylene polyamine, and the rest of the contents are the same.
[0093] Comparative Example 2
[0094] Compared with Example 1, Comparative Example 2 lacks chlorinated paraffin, and the rest of the contents are the same.
[0095] Comparative Example 3
[0096] Comparative Example 3 Compared with Example 1, the phenyl POSS grafted polyethylene polyamine exceeds the limited range, specifically 30 parts, and the rest of the contents are the same.
[0097] Comparative Example 4
[0098] Compared with Example 1, in Comparative Example 4, the amount of chlorinated paraffin exceeds the limit, specifically 15 parts, and the rest of the contents are the same.
[0099] Comparative Example 5
[0100] Compared with Example 1, in Comparative Example 5, the eucommia rubber exceeds the limit, specifically 40 parts, and the rest of the contents are the same.
[0101] The performance of the tread rubbers prepared in the above embodiments and comparative examples was tested, wherein the wear resistance test was based on GB / T 1689-2014, the rolling resistance was characterized by the 60°C Tanδ index, and the strength test results were shown in the table below.
[0102] Table 1 Tread rubber properties
[0103]
[0104] The cut resistance index indicates the cut resistance of the tread rubber. The higher the value, the better the cut resistance and puncture resistance. The DIN wear index indicates the wear resistance of the tread rubber. The higher the value, the better the wear resistance. The lower the rolling resistance 60℃ Tanδ value, the lower the rolling resistance of the surface tread rubber.
[0105] As shown in Table 1, compared with the comparative example, the tread rubber of the embodiment of the present invention has stronger wear resistance and strong resistance. From comparative examples 1-2 and embodiments 1-4, it can be concluded that: (1) After adding phenyl POSS grafted polyethylene polyamine and chlorinated paraffin, the interaction force of the colloid molecular chain is enhanced, making the intermolecular structure of the rubber more compact, effectively reducing the development of wear and cracks, and also reducing rolling resistance. (2) The ionic liquid enhances the interaction between phenyl POSS and polyethylene polyamine, making the cross-linked network more stable, thereby improving the overall performance of the colloid. (3) After the activation of chlorinated paraffin, more active groups are introduced, which enhances the cross-linking strength of each component, improves the overall strength and wear resistance, and also reduces the energy loss caused by friction and reduces rolling resistance. (4) The addition of quercetin promotes vulcanization, optimizes the vulcanization network structure, enhances the tear and cut resistance of the tread rubber, and the antioxidant properties of quercetin also play a role in the friction enhancement and rolling resistance increase caused by aging.
[0106] Comparative Examples 3-5 can be concluded that excessive use of phenyl POSS grafted polyethylene polyamine can increase the hardness and brittleness of the material, thereby causing the tear resistance to decrease. In addition, excessive phenyl POSS grafted polyethylene polyamine may cause excessive crosslinking, making the elasticity of rubber deteriorate, reducing wear resistance and anti-cutting ability. Chlorinated paraffin excessively softens rubber, reduces its mechanical strength and wear resistance, and increases abrasion. Too much consumption of eucommia rubber can affect the uniformity of the material, thereby causing the tear resistance, rolling resistance and anti-cutting performance to decrease.
[0107] In view of the strong cut resistance and wear resistance as well as the low rolling resistance of the tread rubber of the present invention, it can be used as the tread rubber of bias agricultural tires.
[0108] When preparing bias agricultural tires, the mixed rubber sheet is bonded to the outside of the tire body, placed in a mold, and vulcanized at 138° C. to 148° C. for 50 to 80 minutes to obtain a bias agricultural tire.
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A tire, Features: The invention comprises a carcass and a tread. The tread rubber of the tread comprises the following raw materials, calculated by weight: 90-120 parts of styrene-butadiene rubber, 20-30 parts of eucommia rubber, 30-40 parts of white carbon black, 5-8 parts of a vulcanizing agent, 1-3 parts of a vulcanization accelerator, 1-2 parts of zinc oxide, 10-15 parts of phenyl POSS grafted polyethylene polyamine, 8-10 parts of carbon nanotubes and 5-8 parts of chlorinated paraffin; The chlorinated paraffin is pretreated by subjecting the chlorinated paraffin to arc plasma treatment for 5-10 minutes at a DC voltage of 30-50 kV to obtain activated chlorinated paraffin.
2. A tire according to claim 1, Features: The preparation method of the phenyl POSS grafted polyethylene polyamine comprises the following steps: S1, dissolving phenyl POSS in anhydrous dichloromethane to obtain a phenyl POSS solution, and dissolving polyethylene polyamine in anhydrous ethanol to obtain a polyethylene polyamine solution; S2, mixing the phenyl POSS solution and the polyethylene polyamine solution, adding triethylamine, stirring and reacting at 20-30° C. for 0.5-1 h, then heating to 50-70° C., continuing the reaction for 3-4 h, cooling after the reaction, drying, and rotary evaporation to remove the solvent to obtain phenyl POSS grafted polyethylene polyamine; The phenyl POSS is one or two of POSS-phenyl and octa-p-aminophenyl-POSS; In step S2, 1-butyl-3-methylimidazole chloride is added to the phenyl POSS solution, stirred evenly, and then mixed with the polyethylene polyamine solution.
3. A tire as claimed in claim 2, Features: The mass ratio of phenyl POSS: polyethylene polyamine: triethylamine is 1:1.5-2.5:0.05-0.15, the mass ratio of phenyl POSS: anhydrous dichloromethane is 1:10-50, the mass ratio of polyethylene polyamine: anhydrous ethanol is 1:5-10, and the mass ratio of chloride (1-butyl-3-methylimidazole): phenyl POSS is 0.1-1:
1.
4. A tire as claimed in claim 1, Features: The vulcanizing agent is sulfur or phenolic resin, and the vulcanization accelerator is one or more of N-cyclohexyl-2-benzothiazole sulfenamide, N,N'-diphenyl-thiourea and 2-mercaptobenzothiazole.
5. A method for vulcanizing a tire according to any one of claims 1 to 4, Features: The following steps are involved: S1, mixing styrene-butadiene rubber, eucommia rubber, white carbon black, zinc oxide, and phenyl POSS grafted polyethylene polyamine for a first time, then adding carbon nanotubes and quercetin for a second time, and then adding chlorinated paraffin, a vulcanizing agent, and a vulcanization accelerator for a third time, and after the mixing is completed, pressing a sheet to obtain a mixed film; S2, bonding the mixed rubber sheet to the outer side of the tire body, placing it in a mold, and vulcanizing it at 138°C to 148°C for 50 to 80 minutes to obtain a tire.
6. A tire vulcanization method as claimed in claim 5, Features: The mass ratio of quercetin to carbon nanotubes is 0.5-1:8-10.
7. A tire vulcanization method as claimed in claim 5, Features: The temperature of the first mixing is 60-80°C, and the time is 3-5 minutes; the temperature of the second mixing is 100-120°C, and the time is 6-8 minutes; the temperature of the third mixing is 130-150°C, and the time is 5-10 minutes.
8. Use of the tread rubber of a tire as claimed in any one of claims 1 to 4 in preparing bias agricultural tires.