Nanofiber composite hydrogel capable of being sprayed for sterilization, resisting inflammation, inducing stem cell migration and promoting repair
Through the preparation of nanofiber composite hydrogel, combined with electrospinning and photothermal control technology, the deficiencies of existing dressings in sterilization, anti-inflammation and stem cell induction have been solved, and efficient wound repair effects have been achieved, with the wound healing rate reaching 90% %above.
Patent Information
- Application Number
- CN202410761992.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult for existing dressings to simultaneously kill bacteria, inhibit inflammation, and regenerate tissues. In particular, they are deficient in inducing endogenous stem cells to migrate to the wound and survive in the microenvironment, resulting in poor wound repair effects.
Using the preparation method of nanofiber composite hydrogel, PLGA fiber is prepared through electrospinning technology, and anti-inflammatory drugs and factors that induce stem cell migration are added to it, combined with photothermal sterilization and near-infrared light-controlled release technology to form a soluble fiber. Sprayed nanofiber composite hydrogel. The hydrogel achieves controlled drug release under near-infrared light irradiation and provides a suitable microenvironment to promote stem cell migration and repair.
It significantly improves the release efficiency of anti-inflammatory drugs, promotes the migration of stem cells and wound repair, and the wound healing rate reaches more than 90%. It solves the problems of inaccurate controlled release of drugs and insufficient migration of stem cells in the existing technology.
Smart Images

Figure CN118767202A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional hydrogels, and particularly relates to a nanofiber composite hydrogel which can be sprayed to kill bacteria, resist inflammation, induce stem cell migration and promote repair. Background Art
[0002] The treatment of infected wounds places increasing demands on modern dressings, which need to simultaneously meet the diverse functional requirements of killing bacteria, inhibiting inflammation, and tissue regeneration. Current dressings can achieve bactericidal or anti-inflammatory functions by loading drugs, antimicrobial peptides, etc., but there are problems such as bacterial resistance and complex microenvironment conditions that lead to inaccurate drug release. In terms of tissue regeneration, recruiting endogenous stem cells to repair wounds is an effective means, but inducing enough endogenous stem cells to migrate to the site of injury and survive in the wound microenvironment is a problem faced. Therefore, integrating multiple functions into one to form a good synergistic repair-promoting effect is a difficult problem that needs to be solved urgently for wound dressings. Summary of the invention
[0003] In view of the defects of the prior art, the technical problem to be solved by the present invention is to provide a nanofiber composite hydrogel that can be sprayed to kill bacteria, resist inflammation, induce stem cell migration and promote repair.
[0004] The present invention provides a method for preparing a nanofiber composite hydrogel, comprising:
[0005] (1) polylactic acid-co-glycolic acid (PLGA), a solvent, and gold nanorods are stirred and mixed, and then a small molecule drug is added and stirred to dissolve to obtain a spinning solution, and then electrospinning is performed to obtain an electrospun nanofiber membrane;
[0006] (2) mixing the electrospun nanofiber membrane after aminolysis and the polyvinyl alcohol (PVA) solution, homogenizing, and freeze-drying to obtain PLGA short fibers;
[0007] (3) dissolving methacryloyl gelatin (GelMA) in deionized water by stirring in a water bath to obtain a solution, and then mixing with an initiator, PLGA short fibers, and a macromolecular drug to obtain a precursor solution;
[0008] (4) reacting the precursor solution to obtain a nanofiber composite hydrogel.
[0009] Furthermore, the step (1) is specifically to mix PLGA and solvent, stir for 12-48 hours until completely dissolved, then add gold nanorods, stir for 3-12 hours until the solution is uniform, and then add small molecule drugs and stir for 4-12 hours until the drugs are completely dissolved.
[0010] Preferably, in step (1), the molar ratio of lactic acid to glycolic acid of PLGA monomers is 70:30 to 90:10; the solvent is one or more of hexafluoroisopropanol, chloroform, dichloromethane, and N,N-dimethylformamide;
[0011] Preferably, the small molecule drug is a small molecule anti-inflammatory drug; the small molecule anti-inflammatory drug includes one or more of aspirin, diclofenac sodium, and nimesulide.
[0012] Preferably, in step (1), the concentration of polylactic acid-glycolic acid copolymer PLGA in the solvent is 0.1-0.25 g / mL; the content of gold nanorods relative to PLGA is 0.05-0.35 wt %, and the content of small molecule drugs relative to PLGA is 5-25 wt %.
[0013] Preferably, the electrospinning process in step (1) comprises: placing the spinning solution in a micro-syringe, the injection speed is 0.1-2.5 mL / h, the spinning voltage is 6-15 kV, the receiving distance is 10-20 cm, the ambient temperature is 25±1° C., and the ambient relative humidity is 30-70%;
[0014] The electrospun nanofiber membrane is vacuum dried.
[0015] Preferably, the glass transition temperature of the electrospun nanofiber membrane in step (1) is 40-60°C.
[0016] The electrospun nanofiber membrane after aminolysis in step (2): the sheared electrospun fiber membrane block is immersed in a 0.5-5w / v% diamine solution for aminolysis for 5-60 minutes, and then washed; wherein the diamine is one or more of 1,6-hexanediamine and 1,2-ethylenediamine.
[0017] Preferably, the electrospun nanofiber membrane in step (2) is a sheared electrospun nanofiber membrane; the concentration of the PVA solution is 0.1-1 w / v%;
[0018] Preferably, in the step (2), the homogenization process is performed at 8000-16000 rpm for 5-20 min; the freeze-drying process is performed by placing the mixture at -20°C for 10-12 h and freeze-drying the mixture for more than 24 h after removal.
[0019] Further, in step (3), GelMA (5-15w / v%) is dissolved in deionized water, and stirred in a water bath at 37-60°C for 1-2h until the solution is uniform, thereby obtaining solution one; an initiator (0.1-1.5w / v%) is added to solution one, and stirred for 10-30min until the solution is uniform, thereby obtaining mixed solution two; PLGA short fibers (0.1-3w / v%) are then added to mixed solution two, and stirred at 37°C for 30-60min until the short fibers are uniformly dispersed, thereby obtaining mixed solution three; and macromolecular drugs (50-300ng / mL) are continuously added to mixed solution three, and stirred at 37°C for 5-10min until the solution is uniformly mixed, thereby obtaining a nanofiber composite hydrogel precursor solution.
[0020] The preparation of the methacryloyl gelatin (GelMA) comprises: dissolving gelatin in a PBS solution under water bath conditions, then adding methacrylic anhydride dropwise, and continuing to stir in the water bath; then using a PBS solution to terminate the reaction, continuing to stir, dialyzing, and freeze-drying to obtain GelMA.
[0021] Preferably, the initiator in step (3) is photoinitiator I2959; the macromolecular drug is at least one of human stromal cell-derived factor-1α (SDF-1α), interleukin-8 (IL-8), and monocyte chemoattractant protein-1 (MCP-1).
[0022] Preferably, the concentrations of methacryloyl gelatin, photoinitiator, PLGA short fibers, and macromolecular drugs in the precursor solution of step (3) are 5-15 w / v%, 0.1-1.5 w / v%, 0.1-3 w / v%, and 50-300 ng / mL, respectively.
[0023] Preferably, the reaction in step (4) is carried out under 365 nm ultraviolet light for 1-10 min.
[0024] Note: w / v% in the present invention, wherein w / v is g / mL.
[0025] The invention provides a nanofiber composite hydrogel prepared by the method.
[0026] The present invention provides an application of the nanofiber composite hydrogel in the field of bacterially infected skin repair dressings.
[0027] The present invention develops a nanofiber composite hydrogel that can be sprayed to kill bacteria, fight inflammation, and induce stem cell migration and promote repair. Under NIR irradiation, the hydrogel can not only achieve photothermal sterilization, but also control drug release, providing a good growth microenvironment for the subsequent recruitment of endogenous stem cells, and ultimately achieve early bactericidal and anti-inflammatory effects on wounds, coordinated chemokine release, induction of endogenous stem cell migration, and promotion of tissue repair, so as to overcome the shortcomings of the prior art in practical applications.
[0028] Beneficial Effects
[0029] (1) A nanofiber composite hydrogel, which introduces biodegradable PLGA with a specific monomer ratio to make the glass transition temperature of the prepared electrospun fiber around 46°C, thereby achieving light-controlled drug release under near-infrared light irradiation, and the cumulative release of anti-inflammatory drugs can be increased by more than 9 times under four near-infrared light on / off cycles;
[0030] (2) By adjusting the spinning humidity and spinning parameters, non-bonded electrospun fibers were prepared, and the fiber membrane was further broken up into short fibers using a homogenizer. Compared with the short fibers prepared from the bonded electrospun fiber membrane, the obtained short fibers not only had better uniformity, but also had a significantly increased yield (increased by more than 1 times).
[0031] (3) A drug-loaded nanofiber composite hydrogel, which loads small molecule anti-inflammatory drugs in short fibers and macromolecular drugs that can induce stem cell migration in hydrogels, thereby achieving near-infrared light-controlled anti-inflammatory drug release first to relieve early inflammation (providing a good microenvironment for stem cells), and then combined with the slow release of macromolecular drugs in the hydrogel to induce stem cells to migrate to the wound to participate in repair. The early release of anti-inflammatory drugs and the slow release of macromolecular drugs synergistically promote wound repair.
[0032] (4) The nanofiber composite hydrogel, when applied to a rat full-thickness skin defect infection model, can achieve a wound healing rate of more than 90%, with significant repair effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Schematic diagram of nanofiber composite hydrogel; 1-hydrogel, 2-short fiber, 3-macromolecule drug, 4-small molecule anti-inflammatory drug, 5-gold nanorods;
[0034] Figure 2 SEM images of nanofiber composite hydrogel: (a) fibers are evenly distributed, (b) fibers are agglomerated;
[0035] Figure 3 Cumulative release profiles of anti-inflammatory drugs from nanofibrous composite hydrogels under near-infrared light on / off cycle irradiation. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0037] Preparation of GelMA: Gelatin (gel strength ~260g Bloom, Shanghai MacLean Biochemical Technology Co., Ltd.) was dissolved in PBS solution at 55°C in a water bath, and then methacrylic anhydride was added dropwise and stirred for 3 hours in a 50°C water bath; then PBS solution 4 times the amount of the original solution was added to terminate the reaction, and stirring was continued for more than 30 minutes. The resulting solution was dialyzed with a dialysis bag for 7 days and finally freeze-dried to obtain GelMA.
[0038] Example 1
[0039] Preparation of nanofiber composite hydrogel:
[0040] (1) Preparation of spinning solution:
[0041] PLGA (intrinsic viscosity 0.8 dl / g, Jinan Daigang Bioengineering Co., Ltd., 0.2 g / mL) with a monomer ratio of 75:25 was dissolved in hexafluoroisopropanol solvent and stirred for 24 hours until completely dissolved to obtain a spinning solution; then 0.3 wt% of gold nanorods were added thereto and stirred for 6 hours until the solution was uniform; finally, 20 wt% of the small molecule anti-inflammatory drug diclofenac sodium (DS) was added to the spinning solution and stirred for 8 hours until the drug was completely dissolved.
[0042] (2) Preparation of electrospun fiber membrane:
[0043] The spinning solution prepared in step 1 is placed in a micro-syringe, and the nanofiber membrane is prepared by electrospinning, with an injection speed of 1 mL / h, a spinning voltage of 10 kV, a receiving distance of 15 cm, an ambient temperature of 25±1°C, and an ambient relative humidity of 40±5%. The prepared fiber membrane is then vacuum dried at 37°C for more than 3 h and stored for later use.
[0044] (3) Preparation of short fibers: The electrospun nanofiber membrane prepared in step (2) was cut into fiber blocks of 2 cm × 2 cm in size, and after aminolysis (the fiber blocks were immersed in a 2 w / v% 1,6-hexanediamine solution for 60 min and washed), they were placed in a 0.5 w / v% polyvinyl alcohol (PVA) solution, and then the fiber blocks were broken into short fibers by a homogenizer to obtain a short fiber dispersion. The short fiber dispersion was placed in a -20°C refrigerator for 12 h, taken out and placed in a freeze dryer for freeze drying for more than 24 h to obtain PLGA short fibers with photothermal properties.
[0045] (4) Preparation of nanofiber composite hydrogel precursor solution:
[0046] Dissolve the synthesized GelMA (10 wt / v%) in deionized water, stir in a water bath at 55°C for 2 h until the solution is uniform, and obtain solution 1; add photoinitiator I2959 (1 w / v%) to solution 1, stir for 30 min until the solution is uniform, and obtain mixed solution 2; then add the short fibers (1 w / v%) prepared in step 3 to mixed solution 2, stir at 37°C for 60 min until the short fibers are uniformly dispersed, and obtain mixed solution 3; continue to add the macromolecular drug chemokine SDF-1α (8 kDa, PeproTech, 100 ng / mL) to mixed solution 3, stir at 37°C for 10 min until the solution is uniform, and obtain nanofiber composite hydrogel precursor solution. (5) Preparation of nanofiber composite hydrogel: Spray the nanofiber composite hydrogel precursor solution into a receiving dish, place it under 365 nm ultraviolet light, and obtain a nanofiber composite hydrogel.
[0047] The microstructure of the nanofiber composite hydrogel prepared in Example 1 was characterized by scanning electron microscopy. Figure 2 As shown in (a), it can be found that the short fibers are evenly distributed on the pore walls of the hydrogel.
[0048] The photo-controlled drug release performance of the nanofiber composite hydrogel prepared in Example 1 was tested by high performance liquid chromatography (HPLC). Figure 3 As shown, it can be found that the release amount of small molecule anti-inflammatory drugs in the composite hydrogel is significantly increased under near-infrared light conditions.
[0049] Example 2
[0050] The preparation method of nanofiber composite hydrogel is the same as that of Example 1, except that the injection speed used in the preparation of the electrospun fiber membrane in step (2) is 2 mL / h, the relative humidity of the environment is 65±5%, and the fibers of the prepared fiber membrane are bonded to each other.
[0051] The microstructure of the nanofiber composite hydrogel prepared in Example 2 was characterized by scanning electron microscopy. Figure 2 As shown in (b), it can be found that the short fibers are unevenly distributed and agglomerated.
[0052] Example 3
[0053] The preparation method of nanofiber composite hydrogel is the same as that of Example 1, except that the monomer ratio of PLGA used in the spinning solution in step (1) is 90:10. The release amount of small molecule anti-inflammatory drugs in the composite hydrogel under near-infrared light conditions is significantly reduced compared with that in Example 1.
Claims
1. A method for preparing a nanofiber composite hydrogel, comprising: (1) mixing polylactic acid-co-glycolic acid copolymer PLGA, a solvent, and gold nanorods, then adding a small molecule drug, stirring and dissolving to obtain a spinning solution, and then electrospinning to obtain an electrospun nanofiber membrane; (2) mixing the electrospun nanofiber membrane after aminolysis and the polyvinyl alcohol (PVA) solution, homogenizing, and freeze-drying to obtain PLGA short fibers; (3) dissolving methacrylated gelatin GelMA in deionized water by stirring in a water bath to obtain a solution, and then mixing with an initiator, PLGA short fibers, and a macromolecular drug to obtain a precursor solution; (4) Spraying the precursor solution onto a receiving dish and irradiating it with ultraviolet light to obtain a nanofiber composite hydrogel.
2. The preparation method according to claim 1, characterized in that: In the step (1), the molar ratio of lactic acid to glycolic acid in PLGA is 70:30 to 90:10; the solvent is one or more of hexafluoroisopropanol, chloroform, dichloromethane, and NN dimethylformamide; The small molecule drug is a small molecule anti-inflammatory drug; the small molecule anti-inflammatory drug includes one or more of aspirin, diclofenac sodium, and nimesulide.
3. The preparation method according to claim 1, characterized in that: In the step (1), the concentration of PLGA in the solvent is 0.1-0.25 g / mL; the content of the gold nanorods relative to PLGA is 0.05-0.35 wt %, and the content of the small molecule drug relative to PLGA is 5-25 wt %.
4. The preparation method according to claim 1, characterized in that: The electrospinning process in step (1) comprises: placing the spinning solution in a micro-syringe, the injection speed is 0.1-2.5 mL / h, the spinning voltage is 6-15 kV, the receiving distance is 10-20 cm, the ambient temperature is 25±1° C., and the ambient relative humidity is 30-70%; The electrospun nanofiber membrane is vacuum dried.
5. The preparation method according to claim 1, characterized in that: The electrospun nanofiber membrane in step (2) is a sheared electrospun nanofiber membrane; the concentration of the PVA solution is 0.1-1 w / v%; In the step (2), the homogenization speed is 8000-16000 rpm for 5-20 min; the freeze drying is performed by placing the mixture at -20°C for 10-12 h and then freeze drying the mixture for more than 24 h.
6. The preparation method according to claim 1, characterized in that: The initiator in step (3) is photoinitiator I2959; the macromolecular drug is at least one of human stromal cell derived factor-1α (SDF-1α), interleukin-8 (IL-8), and monocyte chemoattractant protein-1 (MCP-1).
7. The preparation method according to claim 1, characterized in that: In the precursor solution of step (3), the concentration of methacryloyl gelatin is 5-15 w / v%, the concentration of photoinitiator is 0.1-1.5 w / v%, the concentration of PLGA short fibers is 0.1-3 w / v%, and the concentration of macromolecular drugs is 50-300 ng / mL.
8. The preparation method according to claim 1, characterized in that: The reaction in step (4) is performed by irradiating the mixture under 365 nm ultraviolet light for 1-10 min.
9. A nanofiber composite hydrogel prepared by the method of claim 1.
10. Use of the nanofiber composite hydrogel according to claim 9 in the field of bacterially infected skin repair dressings.