PMIA modified ultrafiltration membrane with alkali resistance and pollution resistance as well as preparation method and application of PMIA modified ultrafiltration membrane
By bonding HLNs nanocomposites on the surface of poly(m-phenylene isophthalamide) ultrafiltration membranes, the problem of membrane performance degradation in alkaline wastewater treatment is solved, higher alkali resistance and anti-pollution performance is achieved, and simplified preparation process and reduce costs.
Patent Information
- Application Number
- CN202410944233.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-15
AI Technical Summary
Existing membrane separation technology is difficult to effectively remove alkaline substances when treating alkaline wastewater, resulting in reduced membrane performance and shortened service life. The traditional membrane preparation process is complex and costly.
A modified ultrafiltration membrane preparation method was adopted, by bonding lignin-bisphenol A diglycidyl ether nanocomposites (HLNs) and chitosan on the surface of polym-phenylene isophthalamide matrix membrane, using dip The coating method improves the alkali resistance and anti-pollution properties of the membrane.
It significantly improves the hydrophilicity, alkali resistance and interception performance of the membrane, reduces membrane fouling, extends the service life of the membrane, simplifies the preparation process and reduces production costs.
Smart Images

Figure CN118767684A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of membrane separation, and in particular relates to a PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance, and a preparation method and application thereof. Background Art
[0002] Membrane separation technology is a technology that uses semipermeable membranes to separate substances in liquids or gases. The basic principle of membrane separation technology is to use the principle of selective permeation to separate substances through semipermeable membranes. Membrane separation technology has many advantages such as energy saving, high efficiency, easy to realize automatic control, and no need to add chemicals. It has been widely used in water treatment, food processing, biomedicine, chemical industry and other fields in many industries. However, membrane pollution, especially microbial pollution, often causes the attenuation of membrane flux and the weakening of interception effect, which in turn causes the increase of operating costs and the shortening of membrane service life. This has become the main obstacle to the widespread application of membrane separation technology in drinking water and sewage and wastewater treatment. Ultrafiltration is one of the membrane separation technologies driven by pressure. Applied to liquid mixtures, most of the solutes and solute molecules are filtered out through semipermeable membranes, and water molecules and smaller molecules are retained. Ultrafiltration is usually used to remove larger particles, molecules or organic matter such as microorganisms, colloids, proteins, particles and polymers. The advantages of ultrafiltration technology are simple operation, low cost, and no need to add any chemical reagents. In particular, the experimental conditions of ultrafiltration technology are mild. Compared with evaporation and freeze-drying, there is no phase change and no change in temperature or pH. Therefore, it can prevent the denaturation, inactivation and autolysis of biological macromolecules.
[0003] The pressure resistance and heat resistance of membrane materials are necessary for the long-term operation of membrane separation processes. Poly(m-phenylene isophthalamide) has a hydrogen bond network structure, which gives it excellent mechanical properties and good thermal stability (Tg = 558K). These excellent properties make PMIA one of the key materials in the field of membrane preparation. More importantly, the main chain of PMIA contains a large number of aramid groups and hydrogen bond networks, which makes the material have good hydrophilicity, so that the PMIA membrane has good permeability and anti-fouling performance potential.
[0004] In recent years, industrial wastewater discharge has become a highly concerned issue in the field of global environmental protection. With the rapid development of industrialization, the wastewater generated in the industrial production process contains a large amount of harmful substances, such as heavy metals, chemicals, organic matter, etc., which has caused serious pollution to water resources and the ecological environment. The discharge of industrial wastewater not only has a direct impact on the quality of water bodies, but may also endanger biodiversity, affect human health, and further affect the ecological balance. In addition, industrial wastewater discharge may also lead to soil pollution, groundwater pollution and other problems, bringing long-term negative impacts to the environment. Globally, people are also increasingly aware of the importance of protecting water resources and reducing industrial wastewater discharge for sustainable development, actively exploring and promoting various environmental protection technologies and measures, and striving to improve the impact of industrial wastewater discharge on the environment.
[0005] In particular, alkaline wastewater treatment is an inevitable environmental problem in the industrial production process. Since it contains high concentrations of alkaline substances, organic matter and other harmful components, it is difficult to completely remove them through traditional treatment methods. Traditional wastewater treatment methods such as chemical precipitation have problems such as long treatment cycle, low treatment efficiency and high treatment cost. Membrane separation technology, as a wastewater treatment technology that is efficient, energy-saving and does not consume chemical substances, has the advantages of simple operation, short treatment cycle, high treatment efficiency and low treatment cost. In the treatment of alkaline wastewater, membrane separation technology can effectively remove pollutants such as organic matter and suspended particles in the wastewater, so that the treated wastewater meets the discharge standards, achieving the dual goals of resource recycling and environmental protection.
[0006] At present, the commercial membrane materials developed successively at home and abroad are mostly prepared by interfacial polymerization (US5152901, CN101352659). Interfacial polymerization is to immerse the microporous basement membrane in an aqueous solution of hydrophilic monomers, remove excessive monomer solution, and then immerse the organic solvent of a certain hydrophobic monomer to carry out liquid-liquid interface polycondensation reaction, thereby forming an ultrathin layer on a porous support. In order to obtain better membrane performance, generally, it is also necessary to undergo post-processing processes such as hydrolysis charging or ion radiation or thermal treatment. Although this preparation method can be optimized separately for active layer and supporting layer, so that film has higher separation performance and permeation flux, its preparation process is complicated, and influencing factors are more, and the production cycle is longer, and production cost is higher.
[0007] The Chinese invention patent with application number CN200910244169.0 discloses a poly(m-phenylene isophthalamide) nanofiltration membrane, which mainly adopts a phase inversion method to prepare an asymmetric nanofiltration membrane, and has a certain treatment effect on industrial wastewater. Although the film-forming process of this method is simple, the production cycle is short, the operation is convenient, and the operating cost is low, it is still difficult to solve the problem of too high alkalinity of wastewater when used for alkaline wastewater treatment, which limits the practical application of the membrane.
[0008] In view of this, the present invention is proposed. Summary of the invention
[0009] The purpose of the present invention is to provide a PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance, a preparation method and application thereof in view of the deficiencies in the prior art. A large number of HLNs particles adhere to the surface of the modified ultrafiltration membrane, and the hydrophilicity is greatly enhanced, and the membrane has better alkali resistance, anti-pollution ability and retention performance.
[0010] To achieve the purpose of the present invention, the present invention adopts the following technical solutions:
[0011] A PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance, wherein the PMIA modified ultrafiltration membrane comprises a matrix membrane and a modifier bonded to the surface of the matrix membrane by an adhesive, the matrix membrane comprises poly(m-phenylene isophthalamide), a cosolvent and an organic solvent, and the modifier is HLNs.
[0012] In the present invention, the modifier HLNs is a lignin-bisphenol A diglycidyl ether nanocomposite material.
[0013] Furthermore, the adhesive is CTS.
[0014] Furthermore, the mass ratio of the cosolvent to poly(m-phenylene isophthalamide) is (3-5):(15-18).
[0015] Furthermore, the co-solvent is lithium chloride; and the organic solvent is N,N-dimethylacetamide.
[0016] Furthermore, the thickness of the matrix membrane is 110-240 μm.
[0017] The present invention also provides a method for preparing the PMIA modified ultrafiltration membrane, wherein the preparation method comprises the following steps:
[0018] S1, adding poly(m-phenylene isophthalamide) and a co-solvent into an organic solvent and stirring evenly, and then standing to degas, to obtain a film casting solution;
[0019] S2, preparation of modifier HLNs and CTS bonding layer solution;
[0020] S2.1, preparation of modifier HLNs: dissolving bisphenol A diglycidyl ether and lignin in a mixed solution of acetone and water, stirring, filtering, pouring into deionized water, heating, centrifuging, and drying to obtain the modifier HLNs;
[0021] S2.2, preparation of CTS adhesive layer solution: adding the obtained modifier HLNs to a stirred ethanol solution, then adding chitosan solution to the solution, stirring at room temperature, to obtain a CTS adhesive layer solution;
[0022] S3. Scrape the casting liquid obtained in step S1 onto the substrate, and then place it in a deionized water gel bath for phase separation to obtain a matrix membrane. Then, immerse the surface of the matrix membrane in the CTS bonding layer solution obtained in step S2.2 to bond the HLNs to the matrix membrane. After post-treatment, the PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution properties is obtained.
[0023] The preparation method of the present invention is to scrape the casting solution prepared by polyisophthalamide metaphenylene diamine into a film, and then bond the HLNs nanocomposite material to the PMIA ultrafiltration membrane by dip coating. According to the preparation method, not only the anti-pollution ability and interception performance of the modified ultrafiltration membrane are improved, but also the modified ultrafiltration membrane is endowed with alkali resistance. Compared with other methods, dip coating modification has the following advantages: simple process, low cost, wide application range, thin coating, strong controllability, long-lasting modification effect, and is superior to conventional modification methods in stability, service life and performance.
[0024] Furthermore, in step S1, the stirring temperature is 70-90°C, the stirring time is 10-14h, the standing and degassing temperature is 70-90°C, and the standing and degassing time is 10-14h.
[0025] Furthermore, in step S2.1, the weight ratio of acetone to water in the mixed solution is 3:1.
[0026] Furthermore, in step S3, the temperature of phase separation is 23-26° C., and the time of phase separation is 15-20 s.
[0027] In the present invention, in step S3, the substrate is a glass plate.
[0028] In the present invention, in step S3, the post-treatment is specifically: transferring the dried modified ultrafiltration membrane to deionized water for immersion to remove excess impurities, and then storing it in clean deionized water.
[0029] The present invention also provides application of the PMIA modified ultrafiltration membrane in alkaline industrial wastewater treatment.
[0030] The PMIA modified ultrafiltration membrane provided by the present invention has alkali resistance and anti-pollution performance, and has broad application prospects in treating alkaline industrial wastewater.
[0031] Compared with the prior art, the present invention has the following advantages:
[0032] 1) Compared with the traditional PMIA ultrafiltration membrane, the PMIA modified ultrafiltration membrane provided by the present invention has higher hydrophilicity, significant alkali resistance and retention performance, good anti-pollution effect, and can effectively reduce the influence of membrane pollution on water flux and bovine serum albumin retention;
[0033] 2) The membrane matrix material used in the present invention is poly(m-phenylene isophthalamide), which has excellent mechanical properties, high strength, high rigidity, and can maintain excellent mechanical properties even at high temperatures. Compared with other membrane materials, poly(m-phenylene isophthalamide) has great advantages in high temperature, chemical stability, mechanical properties, electrical properties and radiation resistance, so it is widely used in many fields with high performance requirements;
[0034] 3) The preparation method is simple and efficient, the required equipment is common, the process cycle is short, the production environment requirements are not high, the manufacturing cost is low, and it can be widely used in the preparation of PMIA modified membranes;
[0035] 4) The present invention adopts a dip-coating method to prepare a PMIA modified ultrafiltration membrane. The modifier HLNs on the surface of the modified ultrafiltration membrane has a good bonding effect and is not easily dissolved with water during use, thereby avoiding poisoning of the water body and potential secondary pollution, and ensuring the durability and stability of the membrane structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a scanning electron microscope surface image of the PMIA modified ultrafiltration membrane M1 prepared in Example 1;
[0037] Figure 2 This is a scanning electron microscope surface image of the PMIA original film M0 prepared in Comparative Example 1;
[0038] Figure 3 This is a scanning electron microscope cross-sectional image of the PMIA original film M0 prepared in Comparative Example 1.
[0039] Figure 4 This is a comparison chart of the water fluxes measured after M1 to M5 in Examples 1 to 5 and M0 in Comparative Example 1 were immersed in a NaOH solution with a pH of 12 at room temperature for 12 hours;
[0040] Figure 5 This is a comparison chart of bovine serum albumin retention measured after M1-M5 in Examples 1-5 and M0 in Comparative Example 1 were immersed in a NaOH solution with a pH of 12 at room temperature for 12 hours; DETAILED DESCRIPTION
[0041] The following are specific embodiments of the present invention, and the embodiments are intended to further describe the present invention rather than to limit the present invention.
[0042] In the following examples, the modifier HLNs was prepared by improving the method in the literature T. Zou, MH Sipponen, A. Henn, Solvent-resistant lignin-epoxy hybrid nanoparticles for covalent surface modification and high-strength particulate adhesives, ACS Nano 15 (2021) 4811-4823.
[0043] Example 1
[0044] A PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance comprises a matrix membrane and a modifier bonded to the surface of the matrix membrane, wherein the matrix membrane comprises poly(m-phenylene isophthalamide), a cosolvent and an organic solvent, wherein the cosolvent is lithium chloride, the organic solvent is N,N-dimethylacetamide, the binder is CTS, and the modifier is a HLNs nanocomposite material, and is prepared by the following steps:
[0045] S1, lithium chloride and dry PMIA were dissolved in 82g DMAc at a mass ratio of 3:15, the stirring temperature was 70°C, the stirring time was 10h, and then the degassing was allowed to stand at 70°C and the degassing time was 14h to obtain a casting solution;
[0046] S2, preparation of modifier HLNs and CTS bonding layer solution;
[0047] S2.1, preparation of modifier HLNs: First, dissolve bisphenol A diglycidyl ether and lignin with a total weight of 0.87g and a weight percentage of 10wt% in 80g of a solution of acetone and water with a weight ratio of 3:1, and stir magnetically for 3h. Then filter the solution with filter paper to remove undissolved residues. Then, pour the solution quickly into 200g of deionized water under stirring, and heat at 60°C to remove acetone. Finally, obtain the modifier HLNs by centrifugation and drying;
[0048] S2.2, preparation of CTS adhesive layer solution: First, 0.53 g of HLNs was added to a stirring ethanol solution (22 mL). Then, 2 wt% chitosan solution (4 mL) was added to the above solution, and the mixture was stirred continuously for 20 min at room temperature to obtain a mixed solution, which was the CTS adhesive layer solution;
[0049] S3, the casting solution obtained in step S1 is scraped on the substrate, and then placed in a deionized water gel bath for phase separation, the phase separation temperature is 23 ° C, the phase separation time is 15s, the scraping film thickness is 180μm, and then the ultrafiltration membrane after phase separation is transferred to deionized water for immersion to remove the organic solvent, and then placed in clean deionized water for storage. After that, the surface of the matrix membrane is immersed in the CTS bonding layer solution prepared in step S2.2 for 30min, and the HLNs are bonded to the matrix membrane by dip coating. Finally, the membrane material is dried in an oven at 60 ° C for 1h to obtain the PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance, which is recorded as M1.
[0050] The surface of the M1 membrane was characterized and tested, and the SEM images obtained were as follows: Figure 1 As shown. Figure 1 It can be seen that a large number of HLNs particles adhered to the membrane surface, verifying the successful preparation of PMIA modified ultrafiltration membrane. At the same time, the stable existence of the adhesive layer also laid a solid foundation for the excellent performance of the modified membrane.
[0051] Example 2
[0052] A PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance comprises a matrix membrane and a modifier bonded to the surface of the matrix membrane, wherein the matrix membrane comprises poly(m-phenylene isophthalamide), a cosolvent and an organic solvent, wherein the cosolvent is lithium chloride, the organic solvent is N,N-dimethylacetamide, the binder is CTS, and the modifier is a HLNs nanocomposite material, and is prepared by the following steps:
[0053] S1, lithium chloride and dry PMIA were dissolved in 82g DMAc at a mass ratio of 5:18, the stirring temperature was 90°C, the stirring time was 14h, and then the degassing was allowed to stand at 90°C and the degassing time was 10h to obtain a casting solution;
[0054] S2, preparation of modifier HLNs and CTS bonding layer solution;
[0055] S2.1, preparation of modifier HLNs: First, dissolve bisphenol A diglycidyl ether and lignin with a total weight of 0.87g and a weight percentage of 20wt% in 80g of a solution of acetone and water with a weight ratio of 3:1, and stir magnetically for 3h. Then filter the solution with filter paper to remove undissolved residues. Then, pour the solution quickly into 200g of deionized water under stirring, and heat at 60°C to remove acetone. Finally, obtain the modifier HLNs by centrifugation and drying;
[0056] S2.2, preparation of CTS adhesive layer solution: First, 0.53 g of HLNs was added to a stirring ethanol solution (22 mL). Then, 2 wt% chitosan solution (4 mL) was added to the above solution, and the mixture was stirred continuously for 20 min at room temperature to obtain a mixed solution, which was the CTS adhesive layer solution;
[0057] S3, the casting solution obtained in step S1 is scraped on the substrate, and then placed in a deionized water gel bath for phase separation, the phase separation temperature is 26 ° C, the phase separation time is 20s, the scraping film thickness is 240μm, and then the ultrafiltration membrane after phase separation is transferred to deionized water for immersion to remove the organic solvent, and then placed in clean deionized water for storage. After that, the surface of the matrix membrane is immersed in the CTS bonding layer solution prepared in step S2.2 for 30min, and the HLNs are bonded to the matrix membrane by dip coating. Finally, the membrane material is dried in an oven at 60 ° C for 1h to obtain the PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance, which is recorded as M2.
[0058] Example 3
[0059] A PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance comprises a matrix membrane and a modifier bonded to the surface of the matrix membrane, wherein the matrix membrane comprises poly(m-phenylene isophthalamide), a cosolvent and an organic solvent, wherein the cosolvent is lithium chloride, the organic solvent is N,N-dimethylacetamide, the binder is CTS, and the modifier is a HLNs nanocomposite material, and is prepared by the following steps:
[0060] S1, dissolving lithium chloride and dried PMIA in 82g DMAc at a mass ratio of 4:18, stirring at 80°C for 13h, and then standing for degassing at a temperature of 80°C and a degassing time of 11h to obtain a casting solution;
[0061] S2, preparation of modifier HLNs and CTS bonding layer solution;
[0062] S2.1, preparation of modifier HLNs: First, dissolve bisphenol A diglycidyl ether and lignin with a total weight of 0.87g and a weight percentage of 30wt% in 80g of a solution of acetone and water with a weight ratio of 3:1, and stir magnetically for 3h. Then filter the solution with filter paper to remove undissolved residues. Then, pour the solution quickly into 200g of deionized water under stirring, and heat at 60°C to remove acetone. Finally, obtain the modifier HLNs by centrifugation and drying;
[0063] S2.2, preparation of CTS adhesive layer solution: First, 0.53 g of HLNs was added to a stirring ethanol solution (22 mL). Then, 2 wt% chitosan solution (4 mL) was added to the above solution, and the mixture was stirred continuously for 20 min at room temperature to obtain a mixed solution, which was the CTS adhesive layer solution;
[0064] S3, the casting solution obtained in step S1 is scraped on the substrate, and then placed in a deionized water gel bath for phase separation, the phase separation temperature is 25°C, the phase separation time is 15s, the scraping film thickness is 140μm, and then the ultrafiltration membrane after phase separation is transferred to deionized water for immersion to remove the organic solvent, and then placed in clean deionized water for storage. After that, the surface of the matrix membrane is immersed in the CTS bonding layer solution prepared in step S2.2 for 30min, and the HLNs are bonded to the matrix membrane by dip coating. Finally, the membrane material is dried in an oven at 60°C for 1h to obtain the PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance, which is recorded as M3.
[0065] Example 4
[0066] A PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance comprises a matrix membrane and a modifier bonded to the surface of the matrix membrane, wherein the matrix membrane comprises poly(m-phenylene isophthalamide), a cosolvent and an organic solvent, wherein the cosolvent is lithium chloride, the organic solvent is N,N-dimethylacetamide, the binder is CTS, and the modifier is a HLNs nanocomposite material, and is prepared by the following steps:
[0067] S1, lithium chloride and dry PMIA were dissolved in 82g DMAc at a mass ratio of 3:16, the stirring temperature was 80°C, the stirring time was 12h, and then the degassing was allowed to stand at 80°C and the degassing time was 12h to obtain a casting solution;
[0068] S2, preparation of modifier HLNs and CTS bonding layer solution;
[0069] S2.1, preparation of modifier HLNs: First, dissolve bisphenol A diglycidyl ether and lignin with a total weight of 0.87g and a weight percentage of 40wt% in 80g of a solution of acetone and water with a weight ratio of 3:1, and stir magnetically for 3h. Then filter the solution with filter paper to remove undissolved residues. Then, pour the solution quickly into 200g of deionized water under stirring, and heat at 60°C to remove acetone. Finally, obtain the modifier HLNs by centrifugation and drying;
[0070] S2.2, preparation of CTS adhesive layer solution: First, 0.53 g of HLNs was added to a stirring ethanol solution (22 mL). Then, 2 wt% chitosan solution (4 mL) was added to the above solution, and the mixture was stirred continuously for 20 min at room temperature to obtain a mixed solution, which was the CTS adhesive layer solution;
[0071] S3, the casting solution obtained in step S1 is scraped on the substrate, and then placed in a deionized water gel bath for phase separation, the phase separation temperature is 24 ° C, the phase separation time is 18s, the scraping film thickness is 210μm, and then the ultrafiltration membrane after phase separation is transferred to deionized water for immersion to remove the organic solvent, and then placed in clean deionized water for storage. After that, the surface of the matrix membrane is immersed in the CTS bonding layer solution prepared in step S2.2 for 30min, and the HLNs are bonded to the matrix membrane by dip coating. Finally, the membrane material is dried in an oven at 60 ° C for 1h to obtain the PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance, which is recorded as M4.
[0072] Example 5
[0073] A PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance comprises a matrix membrane and a modifier bonded to the surface of the matrix membrane, wherein the matrix membrane comprises poly(m-phenylene isophthalamide), a cosolvent and an organic solvent, wherein the cosolvent is lithium chloride, the organic solvent is N,N-dimethylacetamide, the binder is CTS, and the modifier is a HLNs nanocomposite material, and is prepared by the following steps:
[0074] S1, lithium chloride and dry PMIA were dissolved in 82g DMAc at a mass ratio of 4:17, the stirring temperature was 70°C, the stirring time was 10h, and then the degassing was allowed to stand at 70°C and the degassing time was 13h to obtain a casting solution;
[0075] S2, preparation of modifier HLNs and CTS bonding layer solution;
[0076] S2.1, preparation of modifier HLNs: First, dissolve bisphenol A diglycidyl ether and lignin with a total weight of 0.87g and a weight percentage of 50wt% in 80g of a solution of acetone and water with a weight ratio of 3:1, and stir magnetically for 3h. Then filter the solution with filter paper to remove undissolved residues. Then, pour the solution quickly into 200g of deionized water under stirring, and heat at 60°C to remove acetone. Finally, obtain the modifier HLNs by centrifugation and drying;
[0077] S2.2, preparation of CTS adhesive layer solution: First, 0.53 g of HLNs was added to a stirring ethanol solution (22 mL). Then, 2 wt% chitosan solution (4 mL) was added to the above solution, and the mixture was stirred continuously for 20 min at room temperature to obtain a mixed solution, which was the CTS adhesive layer solution;
[0078] S3, the casting solution obtained in step S1 is scraped on the substrate, and then placed in a deionized water gel bath for phase separation, the phase separation temperature is 24 ° C, the phase separation time is 20s, the scraping film thickness is 110μm, and then the ultrafiltration membrane after phase separation is transferred to deionized water for immersion to remove the organic solvent, and then placed in clean deionized water for storage. After that, the surface of the matrix membrane is immersed in the CTS bonding layer solution prepared in step S2.2 for 30min, and the HLNs are bonded to the matrix membrane by dip coating. Finally, the membrane material is dried in an oven at 60 ° C for 1h to obtain the PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance, which is recorded as M5.
[0079] Comparative Example 1
[0080] In this comparative example, a non-solvent induced phase separation method is used to prepare an unmodified poly (m-phenylene isophthalamide) flat membrane (i.e., does not contain HLNs). The specific preparation method is as follows:
[0081] S1, dissolving lithium chloride and PMIA in 82 g DMAc at a mass ratio of 4:18, stirring at 80°C for 12 h until fully dissolved, and then standing for degassing for 12 h to obtain a casting solution;
[0082] S2, scrape the casting liquid onto the glass plate, and the scraped film thickness is 190 μm;
[0083] S3, immersing the glass plate with the casting solution in 25°C deionized water for phase separation for 16 seconds;
[0084] S4. The membrane after phase separation is transferred to deionized water for immersion to remove excess solvent, and then placed in clean deionized water for storage to obtain an unmodified poly(m-phenylene isophthalamide) flat membrane, which is recorded as M0.
[0085] The surface and cross section of the M0 membrane were characterized and tested, and the SEM images are shown in Figure 2 , Figure 3 As shown. Figure 2 It can be seen that the smooth and clean surface characteristics of the M0 membrane lay the foundation for the smooth development of subsequent advanced manufacturing processes and is an ideal material for manufacturing modified ultrafiltration membranes. Figure 3 It can be seen that the cross-sectional view of the M0 membrane presents a morphology similar to a finger-like structure, which can effectively enhance the mechanical properties and dimensional stability of the membrane material.
[0086] Test Example 1
[0087] This test example examines the alkali resistance, anti-pollution and interception performance of the membranes prepared in the embodiments and comparative examples of the present invention.
[0088] Test method: Water flux and bovine serum albumin retention test method reference: Z.Chen, G.-E.Chen, H.-Y.Xie, et al. Photocatalytic antifouling properties of novel PVDF membranesimproved by incorporation of SnO 2 -GO nanocomposite for water treatment,Sep.Purif.Technol.259(2021)118184.
[0089] The test results are as follows Figure 4 and Figure 5 As shown. Figure 4 and Figure 5 It can be seen that compared with the unmodified polyisophthalamide flat membrane (M0) prepared in Comparative Example 1, the water flux and retention rate of the PMIA modified ultrafiltration membrane (M1, M2, M3, M4, M5) prepared by the method of the present invention are significantly improved, and have high water flux and high retention rate after being soaked in an alkaline solution, indicating that the modified membrane has strong hydrophilicity and good alkali resistance. At the same time, the high retention rate means that the membrane can effectively prevent BSA from penetrating the membrane, indicating that the membrane has a high anti-pollution ability, can effectively reduce the erosion and pollution of organic pollutants and other pollutants to the membrane, extend the service life of the membrane, and maintain the high-efficiency filtration performance of the membrane. In summary, the PMIA modified ultrafiltration membrane prepared by the method of the present invention has excellent alkali resistance, anti-pollution and retention performance.
[0090] The above describes the basic principles, main features and advantages of the present invention. It will be apparent to the skilled person that the present invention is not limited to the details of the exemplary embodiments shown, but may be implemented in other specific forms without departing from the core spirit and features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0091] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution performance, characterized in that: The PMIA modified ultrafiltration membrane comprises a matrix membrane and a modifier bonded to the surface of the matrix membrane by an adhesive, the matrix membrane comprises poly(m-phenylene isophthalamide), a cosolvent and an organic solvent, and the modifier is HLNs.
2. The PMIA modified ultrafiltration membrane according to claim 1, characterized in that The adhesive is CTS.
3. The PMIA modified ultrafiltration membrane according to claim 2, characterized in that: The mass ratio of the cosolvent to poly(m-phenylene isophthalamide) is (3-5):(15-18).
4. The PMIA modified ultrafiltration membrane according to claim 3, characterized in that The co-solvent is lithium chloride; The organic solvent is N,N-dimethylacetamide.
5. The PMIA modified ultrafiltration membrane according to claim 4, characterized in that: The thickness of the matrix membrane is 110-240 μm.
6. A method for preparing the PMIA modified ultrafiltration membrane according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: S1, adding poly(m-phenylene isophthalamide) and a co-solvent into an organic solvent and stirring evenly, and then standing to degas, to obtain a casting solution; S2, preparation of modifier HLNs and CTS bonding layer solution; S2.1, preparation of modifier HLNs: dissolving bisphenol A diglycidyl ether and lignin in a mixed solution of acetone and water, stirring, filtering, pouring into deionized water, heating, centrifuging, and drying to obtain the modifier HLNs; S2.2, preparation of CTS adhesive layer solution: adding the obtained modifier HLNs to a stirred ethanol solution, then adding chitosan solution to the solution, stirring at room temperature, to obtain a CTS adhesive layer solution; S3. Scrape the casting liquid obtained in step S1 onto the substrate, and then place it in a deionized water gel bath for phase separation to obtain a matrix membrane. Then, immerse the surface of the matrix membrane in the CTS bonding layer solution obtained in step S2.2 to bond the HLNs to the matrix membrane. After post-treatment, the PMIA modified ultrafiltration membrane with alkali resistance and anti-pollution properties is obtained.
7. The preparation method according to claim 6, characterized in that: In step S1, the stirring temperature is 70-90°C, the stirring time is 10-14 hours, the standing temperature for degassing is 70-90°C, and the standing time for degassing is 10-14 hours.
8. The preparation method according to claim 6, characterized in that: In step S2.1, the weight ratio of acetone to water in the mixed solution is 3:
1.
9. The preparation method according to claim 6, characterized in that: In step S3, the temperature of phase separation is 23-26° C., and the time of phase separation is 15-20 s.
10. Use of the PMIA modified ultrafiltration membrane according to any one of claims 1 to 5 in the treatment of alkaline industrial wastewater.
Citation Information
Patent Citations
Method for preparing polyisophthaloyl metaphenylene diamide nanofiltration membrane
CN102114391A
Polyamine-polyamide composite nanofiltration membrane for water softening
US5152901A