High-alkali-resistance ultralow-temperature denitration catalyst as well as preparation method and application thereof

By using materials such as Al2O3, CeO2, and SiO2 combined with copper, cobalt, iron, and indium salts to prepare highly alkali-resistant and ultra-low-temperature denitration catalysts in the biomass power generation industry, the problem of unstable efficiency caused by alkalosis of catalysts in the biomass power generation industry is solved. Efficient denitration and long-life catalyst performance are achieved.

CN118767925AActive Publication Date: 2024-10-15XIAN RES INST OF CHINA COAL TECH & ENG GRP CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410767863.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

The efficiency of SNCR denitration catalysts in the biomass power generation industry is unstable due to alkalosis and cannot meet the emission requirements below 50mg/Nm3. There is an urgent need for denitration catalysts with high alkali resistance.

Method used

Al2O3, CeO2 and SiO2 are used as carriers, combined with active components such as copper salts, cobalt salts, iron salts and indium salts, to prepare high alkali-resistant ultra-low temperature denitration catalysts through ball milling, impregnation and roasting steps to form multi-metallic active sites to improve Catalytic activity and resistance to alkali.

Benefits of technology

The denitrification efficiency and alkali resistance of the catalyst are significantly improved, and the life of the catalyst is extended. The initial denitrification efficiency reaches 90%, and the loss rate after salt leaching is less than 7.5%, meeting the denitrification needs of the biomass power generation industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004893122890000081
    Figure BDA0004893122890000081
  • Figure BDA0004893122890000091
    Figure BDA0004893122890000091
Patent Text Reader

Abstract

The invention provides a high-alkali-resistance ultralow-temperature denitration catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: mixing Al2O3, CeO2 and SiO2 in a mass ratio of 100: (4-6): (3-4) to obtain a carrier raw material; sequentially carrying out ball milling, drying and screening on the carrier raw material to obtain carrier powder; the preparation method comprises the following steps: dissolving a formula amount of an active component in deionized water to obtain an active component solution, the active component being prepared by compounding a copper salt, a cobalt salt, an iron salt and an indium salt; impregnating the carrier powder obtained in the step 1 into the active component solution obtained in the step 2, and sequentially performing standing, drying and roasting treatment to obtain precursor powder; mixing the precursor powder, an adhesive and deionized water, and stirring at a constant temperature to prepare active slurry; the pretreated substrate is added into the active slurry for vacuum impregnation treatment, the volume ratio of the substrate to the active slurry is 1: 3, and then the substrate is obtained through drying and calcination; the high-alkali-resistance ultralow-temperature denitration catalyst provided by the invention is used for a biomass boiler, is high in activity and does not cause secondary pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of denitration, and in particular to a highly alkali-resistant ultra-low temperature denitration catalyst, a preparation method and an application thereof. Background Art

[0002] At present, the main energy consumption in my country is still fossil fuels headed by coal. However, with the increasing consumption of fossil energy, it is urgent to seek clean and renewable energy. Statistics show that the total amount of biomass resources that can be used as energy in China is about 460 million tons of standard coal per year, but the actual amount of biomass energy is 22 million tons of standard coal, accounting for only 4.78% of the total amount of biomass resources. Therefore, biomass energy will become an important direction for the development of renewable energy in my country in the future.

[0003] The dust generated by the biomass power generation industry contains a large amount of alkaline elements such as Na and K, which can easily lead to alkali poisoning of the SNCR catalyst, resulting in a SNCR denitrification efficiency of 10% to 25% for the biomass grate furnace and 40% to 60% for the biomass circulating fluidized bed. The denitrification efficiency is unstable and cannot stably meet the emission requirement of 50mg / Nm 3 Therefore, there is an urgent need to develop a highly alkali-resistant SCR denitrification catalyst with excellent performance. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a highly alkali-resistant ultra-low temperature denitrification catalyst, a preparation method and an application thereof, so as to solve the technical problem that the traditional SCR catalyst in the prior art is not suitable for the biomass power generation industry.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:

[0006] A method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst, characterized in that it comprises the following steps:

[0007] Step 1, mixing Al2O3, CeO2 and SiO2 in a mass ratio of 100:(4-6):(3-4) to obtain a carrier raw material; ball milling, drying and sieving the carrier raw material in sequence to obtain a carrier powder;

[0008] Step 2, dissolving the active component in the formula amount in deionized water to obtain an active component solution, wherein the active component is compounded from copper salt, cobalt salt, iron salt and indium salt;

[0009] Step 3, immersing the carrier powder obtained in step 1 in the active component solution obtained in step 2, and sequentially subjecting the mixture to standing, drying and calcining to obtain a precursor powder; the mass ratio of the carrier powder to the active component is (77-87): (13-23).

[0010] Step 4, mixing the precursor powder, the binder and deionized water, and stirring at a constant temperature to obtain an active slurry;

[0011] Step 5: adding the pretreated substrate to the active slurry for vacuum impregnation to obtain an impregnated product, wherein the volume ratio of the substrate to the active slurry is 1:3; and drying and calcining the obtained impregnated product.

[0012] The present invention also has the following technical features:

[0013] Specifically, in step 1, the ball milling speed is 300-600 r / min, the ball milling time is 24-36 h, during the ball milling process, the solid-liquid ratio of the carrier raw material to deionized water is 1.0:0.4-0.6, and the mass ratio of the grinding balls to the carrier raw material is (5.0-10.0):1.0; the drying temperature is 70-110° C., and the drying time is 30 min-2 h; and the product is sieved through a 100-150 mesh sieve.

[0014] Furthermore, in the active components, the copper salt is calculated as CuO, the cobalt salt is calculated as CoO, the iron salt is calculated as Fe2O3, and the indium salt is calculated as In2O3, and the mass ratio is CuO:CoO:Fe2O3:In2O3=(2~8):(5~7):(1~2):(0.1~0.2).

[0015] Furthermore, in step 3, the standing time is 20 to 30 hours; the drying temperature is 90-110° C., and the drying time is 12 to 18 hours; the roasting temperature is 700-750° C., and the roasting time is 4 to 6 hours.

[0016] Furthermore, the adhesive is selected from one or more of hydroxymethyl cellulose, polyvinyl alcohol and polyvinyl acetate.

[0017] Furthermore, in step 4, the mass ratio of the precursor powder to deionized water is 1:

[0018] (4.5~5.5), constant temperature stirring temperature is 50~100℃, constant temperature stirring time is 3~5h.

[0019] Furthermore, in step 5, the vacuum degree of the vacuum impregnation treatment is 10 -3 Pa~10 -5 Pa, the impregnation time is 2 to 5 hours; the drying temperature is 105 to 200°C, and the drying time is 10 to 15 hours; the calcination temperature is 480 to 530°C, and the calcination time is 5 to 8 hours.

[0020] Furthermore, the matrix is ​​selected from one or more of a cordierite matrix, a vermiculite matrix, a mullite matrix and a attapulgite matrix;

[0021] The pretreatment comprises: adding the matrix raw material into a dilute nitric acid solution with a mass fraction of 3-5% and soaking it for 0.5-1.0h to obtain a slurry; circulating deionized water to remove the residual acid in the slurry, and adjusting the pH of the slurry to ≥7 during the cleaning process; drying the cleaned slurry at 80-100°C for 10-12h, and then calcining it at 500-550°C for 2-3h to obtain the slurry.

[0022] The present invention also provides a highly alkali-resistant ultra-low temperature denitration catalyst, which is prepared by the above-mentioned preparation method.

[0023] The present invention also protects the application of the high alkali resistance and ultra-low temperature denitration catalyst prepared by the above preparation method in denitration in the biomass power generation industry.

[0024] Compared with the prior art, the present invention has the following technical effects:

[0025] The high alkali resistance and ultra-low temperature denitration catalyst provided by the present invention is suitable for the biomass power generation industry, which solves the problem of denitration catalyst deactivation due to high alkali in flue gas in the biomass power generation industry, and prolongs the life of the catalyst while meeting the catalytic effect. DETAILED DESCRIPTION

[0026] Specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.

[0027] Active component selection basis: CuO can achieve It is beneficial to the adsorption of reducing agents and NO X decomposition, increasing the reducing agent to reduce NO X activity; CoO can promote the generation of chemically adsorbed oxygen and oxygen vacancies; Fe2O3 has the performance of lowering the initial reduction temperature and promoting low-temperature NH3-SCR reaction. At the same time, compared with other metals, Fe has a lower cost, which is conducive to factory application; In2O3 has oxygen affinity and dynamic migration characteristics. The electronic properties of the indium-copper-cobalt-iron surface can form multi-metal active sites, thereby improving its catalytic activity, and thus making the catalyst show high activity and high alkalinity resistance.

[0028] Support selection basis: Al2O3 has high thermal stability, is easy to shape, and is easy to prevent catalyst sintering. It also has excellent surface pore structure, large specific surface area, and high porosity, which is conducive to the adsorption of nitrogen-containing substances. At the same time, as an amphoteric oxide, Al2O3 has abundant acid sites and can adsorb NO and NH3 well, promoting the catalytic reaction. CeO2 can cause electron imbalance on the catalyst surface, forming oxygen vacancies and unsaturated chemical bonds, thereby increasing the concentration of chemically adsorbed oxygen on the surface and improving the redox ability of the catalyst. SiO2 has strong hydrophobic properties, which can ensure that the catalyst is not affected by water vapor during operation, and can also improve the N2 selectivity of the catalyst. Cerium-aluminum-silicon can form a solid solution of fluorite structure at a certain ratio. This structure and lattice can promote the reduction of NO, so that cerium exhibits higher activity and alkalinity resistance than titanium.

[0029] Basis for matrix selection: Natural products such as cordierite have sufficient mechanical strength and specific surface area and are easily available.

[0030] Example 1

[0031] In accordance with the above technical scheme, this embodiment discloses a method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst, comprising the following steps:

[0032] Step 1, carrier preparation, Al2O3, CeO2 and SiO2 in a mass ratio of 100:4:3 are mixed to obtain a carrier raw material, ball milled in a ball mill at a speed of 300-600r / min for 24-36h, then placed in a drying oven at 70-110°C for 30min, and then sieved with a 100-mesh stainless steel standard sieve and collected to obtain a carrier powder;

[0033] Step 2, preparation of active components: Cu(NO3)2·3H2O, Co(NO3)2·6H2O, Fe(NO3)3·9H2O and In(NO3)3·4H2O were dissolved in deionized water in a mass ratio of CuO:CoO:Fe2O3:In2O3=2:5:1:0.1 to prepare an active component solution;

[0034] Step 3, according to the mass ratio of active component to carrier powder of 13:87 and the numerical ratio of active component volume to carrier powder mass of 4:3, the carrier powder obtained in step 1 is immersed in the active component solution obtained in step 2, standing at room temperature for 24 hours, drying at 90-110° C. for 12 hours, and calcining at 700-750° C. for 4 hours to obtain a precursor powder;

[0035] Step 4, mixing the precursor powder and deionized water in a mass ratio of 1:5, adding hydroxymethyl cellulose, and stirring at a constant temperature of 50-100° C. for 3-5 hours to obtain an active slurry;

[0036] Step 5, soaking the cordierite substrate in a 3-5% mass fraction dilute nitric acid solution for 0.5-1.0h, and washing with deionized water to remove the residual acid. At the same time, adding ammonia water to make the pH ≥ 7 during the deionized water washing process, and then drying the slurry in an oven at 80°C for 12h, calcining at 500°C for 2h to obtain a pretreated cordierite matrix, and calcining the pretreated cordierite substrate at room temperature, 10 -3 Pa~10 -5 The catalyst was immersed in the active slurry for 2 to 5 hours under a vacuum degree of Pa, then dried at 105 to 200°C for 10 to 15 hours, and finally calcined at 500°C for 6 hours to obtain a highly alkali-resistant ultra-low temperature denitrification catalyst, with a volume ratio of the matrix to the active slurry of 1:3.

[0037] The high alkali resistance ultra-low temperature denitration catalyst prepared in this example was subjected to a denitration test in the laboratory. The conditions of the denitration test were: 150°C, 12 vol.% H2O, NO X 500mg / m 3 、NH3:NO X =1, airspeed 5000h -1 .

[0038] The alkali resistance of the catalyst was verified by comparing the changes in denitrification efficiency before and after salt impregnation treatment. The salt impregnation treatment process included: preparing a mixed solution containing 0.1 mol / L potassium nitrate, 0.1 mol / L potassium chloride, 0.1 mol / L potassium sulfate, 0.1 mol / L sodium nitrate, 0.1 mol / L sodium chloride, and 0.1 mol / L sodium sulfate, and immersing the high alkali resistance and ultra-low temperature denitrification catalyst prepared in this embodiment in the mixed solution at room temperature. The volume ratio of the high alkali resistance and ultra-low temperature denitrification catalyst to the volume of the mixed solution was 1:3, and the immersion time was 30 min. After the impregnation was completed, the catalyst was taken out and allowed to stand for 12 h, dried in a muffle furnace at 120°C, and calcined at 500°C for 4 h, to finally obtain an alkali metal poisoning catalyst.

[0039] The comparison results of the denitrification efficiency of the catalyst before and after salt impregnation treatment are shown in Table 1.

[0040] The XRF characterization data of the catalyst before and after impregnation are shown in Table 2.

[0041] Example 2

[0042] This embodiment discloses a method for preparing a highly alkali-resistant ultra-low temperature denitrification catalyst. The steps of the method are the same as those of Example 1, except that: in this embodiment, in step 1, the carrier raw material component Al2O3:CeO2:SiO2=100:5:3.5; in step 2, the corresponding Cu(NO3)2·3H2O, Co(NO3)2·6H2O, Fe(NO3)3·9H2O and In(NO3)3·4H2O are dissolved in deionized water according to the mass ratio of CuO:CoO:Fe2O3:In2O3=5:6:1.5:0.15; in step 3, the mass ratio of the carrier powder to the active component is 82:18.

[0043] The high alkali resistance and ultra-low temperature denitration catalyst prepared in this example was used for denitration test in the laboratory. The denitration test conditions were: 150°C, 12 vol.% H2O, NO X 500mg / m 3 、NH3:NO X =1, airspeed 5000h -1 The alkali resistance of the catalyst was verified by comparing the changes in the denitration efficiency before and after the salt impregnation treatment. The salt impregnation treatment process was the same as that of Example 1.

[0044] The comparison results of the denitrification efficiency of the catalyst before and after salt impregnation treatment are shown in Table 1.

[0045] The XRF characterization data of the catalyst before and after impregnation are shown in Table 2.

[0046] Example 3

[0047] This embodiment discloses a method for preparing a highly alkali-resistant ultra-low temperature denitrification catalyst. The steps of the method are the same as those of Example 1, except that: in this embodiment, in step 1, the carrier raw material component Al2O3:CeO2:SiO2=100:6:4; in this embodiment, in step 2, the corresponding Cu(NO3)2·3H2O, Co(NO3)2·6H2O, Fe(NO3)3·9H2O, In(NO3)3·4H2O are dissolved in deionized water according to the mass ratio of CuO:CoO:Fe2O3:In2O3=8:7:2:0.2; in this embodiment, in step 3, the mass ratio of the carrier powder to the active component is 77:23.

[0048] The high alkali resistance and ultra-low temperature denitration catalyst prepared in this example was used for denitration test in the laboratory. The denitration test conditions were: 150°C, 12 vol.% H2O, NO X 500mg / m 3 、NH3:NO X =1, airspeed 5000h -1The alkali resistance of the catalyst was verified by comparing the changes in the denitration efficiency before and after the salt impregnation treatment. The salt impregnation treatment process was the same as that of Example 1.

[0049] The comparison results of the denitrification efficiency of the catalyst before and after salt impregnation treatment are shown in Table 1.

[0050] The XRF characterization data of the catalyst before and after impregnation are shown in Table 2.

[0051] Comparative Example 1

[0052] The difference between Comparative Example 1 and Example 2 is that, with reference to the formula of the existing denitration catalyst (authorization announcement number: CN107983354B), the preparation method is the same as Example 2, and the final catalyst prepared contains 89.90gAl2O3, 4.49g CeO2, 3.15g SiO2, 0.99g CuO, 1.18g CoO and 0.29g Fe2O3 in 100g of the catalyst.

[0053] The catalyst prepared in this comparative example was subjected to a denitration test in the laboratory. The denitration test conditions were: 150°C, 12 vol.% H2O, NO X 500mg / m 3 、NH3:NO X =1, airspeed 5000h -1 The alkali resistance of the catalyst was verified by comparing the changes in the denitration efficiency before and after the salt impregnation treatment. The salt impregnation treatment process was the same as that of Example 1.

[0054] The comparison results of the denitrification efficiency of the catalyst before and after salt impregnation treatment are shown in Table 1.

[0055] The XRF characterization data of the catalyst before and after impregnation are shown in Table 2.

[0056] Comparative Example 2

[0057] The difference between Comparative Example 2 and Example 2 is that, with reference to the formula of the domestic peer denitration catalyst (authorization announcement number: CN103846094 B), the preparation method is the same as Example 2, and the final catalyst prepared contains 89.87gAl2O3, 4.49g TiO2, 3.15g SiO2, 0.99g CuO, 1.18g CoO, 0.29g Fe2O3 and 0.03g In2O3 in 100g catalyst.

[0058] The catalyst prepared in this comparative example was subjected to a denitration test in the laboratory. The denitration test conditions were: 150°C, 12 vol.% H2O, NO X 500mg / m 3 、NH3:NO X =1, airspeed 5000h -1The alkali resistance of the catalyst was verified by comparing the changes in the denitration efficiency before and after the salt impregnation treatment. The salt impregnation treatment process was the same as that of Example 1.

[0059] The comparison results of the denitrification efficiency of the catalyst before and after salt impregnation treatment are shown in Table 1.

[0060] The XRF characterization data of the catalyst before and after impregnation are shown in Table 2.

[0061]

[0062] Table 1. Denitrification filter material test results

[0063] It can be seen from Table 1 that under the same experimental conditions, the initial denitration efficiency of the catalysts provided in Examples 1 to 3 is 90%, which is significantly higher than that in Comparative Examples 1 and 2, indicating that the catalysts prepared by the method of the present application exhibit higher activity; the efficiency loss rates after salt immersion are all less than 7.5%, which is significantly lower than that in Comparative Examples 1 and 2, and the lower the loss rate, the better the alkali resistance of the catalyst and the longer the operating life; in summary, the high alkali resistance and ultra-low temperature denitration catalyst provided in the present application has excellent denitration performance and salt and alkali resistance.

[0064]

[0065] Table 2. XRF characterization results of denitrification catalysts

[0066] It can be seen from the above table that the alkali metal did enter the catalyst surface after salt immersion, proving that the salt immersion method is effective.

[0067] By comparing the above comparative examples with the embodiments, it can be seen that: thanks to the oxygen affinity and dynamic migration characteristics of indium, its doping can change the electronic properties of the copper-cobalt-iron surface and form multi-metal active sites, thereby improving the catalytic activity of copper-cobalt-iron, and then making the catalyst exhibit high activity (denitrification efficiency) and high alkali resistance (the smaller the denitrification efficiency loss rate after salt leaching, the better); thanks to the unique and powerful oxygen storage and release function of cerium, cerium-aluminum-silicon can form a fluorite-type solid solution at a certain ratio. This structure and lattice can promote the reduction of NO, so that cerium exhibits higher activity and alkali resistance than titanium.

[0068] Application Example 1

[0069] In this application example, the high alkali resistance ultra-low temperature denitration catalyst prepared in Example 2 is used for denitration of flue gas from a biomass boiler. The flue gas at the tail end of the biomass boiler is: NO X Concentration 220mg / m 3 ; SO2 concentration 220mg / m 3 ; Particle concentration 43mg / m 3 , NO in flue gas is discharged after denitration deviceX Concentration <50 mg / m 3 , and the efficiency hardly decreased after 168 hours of stable operation, and the average denitrification efficiency was 86.86% after 168 hours of operation.

[0070] Comparative Example 3

[0071] In this application example, the existing commercial medium-temperature catalyst is used for the denitrification of flue gas from a biomass boiler. The flue gas at the tail end of the biomass boiler is: NO X Concentration 220mg / m 3 ; SO2 concentration 220mg / m 3 ; Particle concentration 43mg / m 3 , NO in flue gas is discharged after denitration device X Concentration>50mg / m 3 After 168 hours of operation, the denitrification efficiency dropped from 81.2% to 77.8%.

[0072] It can be seen from Application Example 1 and Comparative Example 3 that:

[0073] The highly alkali-resistant ultra-low temperature denitration catalyst prepared by the method of the present invention is suitable for denitration in the biomass power generation industry, can effectively resist the influence of alkali metals in flue gas, reduce micropore blockage of the catalyst, neutralize the acid content on the catalyst surface, and prolong the activity and life of the catalyst.

[0074] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0075] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst, characterized in that: The following steps are involved: Step 1, mixing Al2O3, CeO2 and SiO2 in a mass ratio of 100:(4-6):(3-4) to obtain a carrier raw material; ball milling, drying and sieving the carrier raw material in sequence to obtain a carrier powder; Step 2, dissolving the active component in the formula amount in deionized water to obtain an active component solution, wherein the active component is compounded from copper salt, cobalt salt, iron salt and indium salt; Step 3, immersing the carrier powder obtained in step 1 in the active component solution obtained in step 2, and sequentially subjecting the mixture to standing, drying and calcining to obtain a precursor powder; the mass ratio of the carrier powder to the active component is (77-87): (13-23). Step 4, mixing the precursor powder, the binder and deionized water, and stirring at a constant temperature to obtain an active slurry; Step 5: adding the pretreated substrate to the active slurry for vacuum impregnation to obtain an impregnated product, wherein the volume ratio of the substrate to the active slurry is 1:3; and drying and calcining the obtained impregnated product.

2. The method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst according to claim 1, characterized in that: In the step 1, the ball milling speed is 300-600 r / min, the ball milling time is 24-36 h, during the ball milling process, the solid-liquid ratio of the carrier raw material to deionized water is 1.0:0.4-0.6, and the mass ratio of the grinding balls to the carrier raw material is (5.0-10.0):1.0; the drying temperature is 70-110° C., and the drying time is 30 min-2 h; and the product is sieved through a 100-150 mesh sieve.

3. The method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst according to claim 1, characterized in that: Among the active components, the copper salt is calculated as CuO, the cobalt salt is calculated as CoO, the iron salt is calculated as Fe2O3, and the indium salt is calculated as In2O3, and the mass ratio is CuO:CoO:Fe2O3:In2O3=(2-8):(5-7):(1-2):(0.1-0.2).

4. The method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst according to claim 1, characterized in that: In the step 3, the standing time is 20 to 30 hours; the drying temperature is 90-110° C., and the drying time is 12 to 18 hours; the roasting temperature is 700-750° C., and the roasting time is 4 to 6 hours.

5. The method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst according to claim 1, characterized in that: The adhesive is selected from one or more of hydroxymethyl cellulose, polyvinyl alcohol and polyvinyl acetate.

6. The method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst according to claim 1, characterized in that: In step 4, the mass ratio of the precursor powder to deionized water is 1:(4.5-5.5), the constant temperature stirring temperature is 50-100° C., and the constant temperature stirring time is 3-5 hours.

7. The method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst according to claim 1, characterized in that: In step 5, the vacuum degree of the vacuum impregnation treatment is 10 -3 Pa~10 -5 Pa, the impregnation time is 2 to 5 hours; the drying temperature is 105 to 200°C, and the drying time is 10 to 15 hours; the calcination temperature is 480 to 530°C, and the calcination time is 5 to 8 hours.

8. The method for preparing a highly alkali-resistant ultra-low temperature denitration catalyst according to claim 1, characterized in that: The matrix is ​​selected from one or more of a cordierite matrix, a vermiculite matrix, a mullite matrix and a attapulgite matrix; The pretreatment comprises: adding the matrix raw material into a dilute nitric acid solution with a mass fraction of 3-5% and soaking it for 0.5-1.0h to obtain a slurry; circulating deionized water to remove the residual acid in the slurry, and adjusting the pH of the slurry to ≥7 during the cleaning process; drying the cleaned slurry at 80-100°C for 10-12h, and then calcining it at 500-550°C for 2-3h to obtain the slurry.

9. A highly alkali-resistant ultra-low temperature denitration catalyst, characterized in that: The method is as described in any one of claims 1 to 8.

10. Use of the high alkali resistance and ultra-low temperature denitration catalyst prepared by the preparation method according to any one of claims 1 to 8 in denitration in the biomass power generation industry.

Citation Information

Patent Citations

  • Catalyst capable of catalyzing and decomposing N2O under high-temperature water-oxygen supplying condition and preparation method of catalyst

    CN104475112A

  • Coated low-temperature flue gas denitration catalyst, and preparation method and application thereof

    CN105126827A

  • Preparation method of novel hydrogen catalytic combustion non-noble metal catalyst

    CN110787808A

  • Low-temperature CO-SCR denitration Cu-Fe / AC catalyst as well as preparation method and application thereof

    CN112371126A

  • Low-temperature denitration catalyst and preparation method thereof

    CN113198487A