A method for preparing a catalyst for producing tertiary amines

Through the synergistic combination of aluminum oxide-supported copper-nickel composite and POSS-supported palladium-nickel composite, the problems of low selectivity and insufficient activity of existing catalyst reactions were solved, and the preparation of high-activity and high-selectivity catalysts were achieved, which improved the tertiary Product quality and reaction efficiency of amines.

CN118767928BActive Publication Date: 2024-11-29SHANDONG TAIYUAN CHEM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411242260.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-29
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

Existing catalysts for tertiary amine production are prone to cause impurities in side reactions, with low reaction selectivity and poor catalytic effect, resulting in insufficient reaction activity.

Method used

The coordinated combination of alumina-supported copper-nickel composite and POSS-supported palladium-nickel composite is adopted to influence the metal active ingredients to improve the reactivity and selectivity through the combination of the two support materials.

Benefits of technology

The preparation of high-activity and high-selectivity catalysts is achieved, and the product quality and reaction efficiency of tertiary amines are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a method for preparing a catalyst for producing tertiary amines. The present invention selects a copper-nickel composite supported by alumina and a palladium-nickel composite supported by POSS for synergistic combination, and through the compounding of the two carrier materials, the active components in the catalyst can influence each other, give full play to the catalytic effect of the metal active components, promote the improvement of reaction activity, and achieve high selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic synthesis, and in particular relates to a method for preparing a catalyst for producing tertiary amines. Background Art

[0002] Tertiary amines are the most important type of organic amine compounds among fatty amines. Their main use is as raw materials for cationic or zwitterionic surfactants. The vast majority of cationic and zwitterionic surfactants are derivatives of tertiary amines. Cationic and zwitterionic surfactants have unique properties such as sterilization, fabric softening, antistatic and metal corrosion inhibition, which cannot be replaced by other chemicals. This gives tertiary amines a unique position in chemical products.

[0003] The process of preparing tertiary amines by direct catalytic amination of fatty alcohols has become the main method for producing fatty tertiary amines because of its advantages of short process route, low equipment investment, basically no three wastes discharge and high product quality. The production process of tertiary amines by fatty alcohols consists of units such as batching, amination, sedimentation and distillation, among which the key units are amination and distillation, and a catalyst must be used during the amination operation. However, the existing catalysts for tertiary amine production are prone to cause side reactions and lead to the appearance of impurities. The impurities produced will continue to react to produce other impurities, the selectivity of the reaction is low, and the catalytic effect of the catalyst is poor, resulting in insufficient reaction activity.

[0004] Therefore, how to increase the reaction selectivity and the reaction activity by designing catalysts for tertiary amine production, thereby improving the tertiary amine value of the product and obtaining highly active and highly selective catalysts has become a focus that needs to be tackled. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a catalyst for the production of tertiary amines, aiming to solve the problem that the existing catalysts for the production of tertiary amines are prone to cause side reactions and lead to the formation of impurities, the impurities produced will continue to react to produce other impurities, the reaction selectivity is low, and the catalytic effect is poor resulting in insufficient reaction activity.

[0006] The present invention selects a synergistic combination of an alumina-supported copper-nickel complex and a POSS-supported palladium-nickel complex, and compounding the two carrier materials so that active components in the catalyst can influence each other, give full play to the catalytic effect of the metal active components, promote the improvement of reaction activity, and achieve high selectivity.

[0007] The technical solution of the present invention is as follows:

[0008] The present invention provides a method for preparing a catalyst for producing tertiary amines, characterized in that the preparation method comprises the following steps:

[0009] Step S1: adding 5 parts of β-cyclodextrin to 250 parts of deionized water, stirring for 0.1 h, adding 15 parts of copper nitrate and 10 parts of nickel nitrate hexahydrate, stirring for 2 h, and then adding 50 parts of aluminum oxide to obtain a solid suspension; stirring the solid suspension at room temperature for 2 h, rotary evaporating at 60° C. to obtain a solid, drying the solid, and calcining to obtain an aluminum oxide-loaded copper-nickel complex;

[0010] Step S2: adding 3 parts of palladium nitrate to 50 parts of deionized water, stirring to obtain a palladium nitrate solution, adding 5 parts of anhydrous nickel nitrate to 50 parts of deionized water, stirring to obtain a nickel nitrate solution; immersing 20 parts of POSS in 100 parts of palladium nitrate solution for 1 hour, drying at 80° C. for 24 hours to obtain a palladium-loaded solid; immersing the palladium-loaded solid in 100 parts of nickel nitrate solution for 2 hours, drying after immersion, and calcining to obtain a POSS-loaded palladium-nickel complex;

[0011] Step S3: Add 50 parts of alumina-supported copper-nickel complex and 20 parts of POSS-supported palladium-nickel complex to 200 parts of organic solvent, stir for 1 hour, add 5 parts of promoter, stir for 5 hours at 70° C., and after drying, obtain a catalyst for tertiary amine production.

[0012] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0013] As a preferred technical solution of the present invention, the aluminum oxide described in step S1 is cerium-modified aluminum oxide. The preparation method of the cerium-modified aluminum oxide is as follows: add 5 parts of aluminum oxide to 50 parts of deionized water, stir at 80°C for 1 hour, then add 3 parts of cerium nitrate and stir for 0.5 hour, stir evenly, add 1 part of sodium hydroxide and 1 part of citric acid, react for 2.5 hours, cool to room temperature, vacuum filter, wash the solid with deionized water to pH=7, dry the solid at 120°C for 24 hours, and then calcine at 600°C for 6 hours to obtain cerium-modified aluminum oxide.

[0014] In the cerium-modified alumina-loaded copper-nickel complex, copper mainly plays a dehydrogenation role, and nickel has a strong hydrogen absorption capacity and mainly plays a hydrogenation role. The simultaneous presence of copper and nickel in the catalyst can enable the catalyst to have both dehydrogenation and hydrogenation effects. With β-cyclodextrin as the main body of the metal complex, with the assistance of β-cyclodextrin, the strong interaction between the highly dispersed nickel particles and the alumina carrier prevents the loss of nickel during the reaction and improves the reaction activity of the catalyst. The nickel-cerium interaction prevents the formation of nickel aluminates, thereby forming smaller nickel nanoparticles with a narrower particle size distribution, thereby obtaining high activity and high selectivity.

[0015] Preferably, the drying temperature in step S1 is 100-120° C., the drying time is 24-36 hours, the calcination temperature is 400-450° C., and the calcination time is 4-6 hours.

[0016] As a preferred technical solution of the present invention, the POSS described in step S2 is carboxylated POSS. The preparation method of the carboxylated POSS is: add 1 part of sodium dodecyl sulfate to 100 parts of deionized water, control the temperature to 60°C, add 5 parts of vinyl POSS, stir and react for 2 hours; then add 10 parts of methacrylic acid, 2 parts of ammonium persulfate and 0.5 parts of sodium bisulfite to react for 4 hours, cool to room temperature after the reaction is completed, and dry at 110°C for 24 hours to obtain carboxylated POSS.

[0017] POSS loaded palladium-nickel complex can form palladium-nickel particles by first loading palladium and then loading nickel, and improve the reducibility of nickel. At the same time, combined with the reversible hydrogen storage capacity of cerium in the cerium-modified alumina loaded copper-nickel complex carrier, the activity is improved; the carrier carboxylation POSS has a large specific surface area and can adsorb more ammonia molecules, which is convenient for amination reaction in the pores, can increase the catalytic reaction rate, and thus increase the reaction activity.

[0018] Preferably, the drying temperature in step S2 is 90-100° C., the drying time is 36-48 hours, the calcination temperature is 350-400° C., and the calcination time is 2-4 hours.

[0019] Preferably, the organic solvent in step S3 is selected from any one of methanol, ethanol, isopropanol, or a combination of at least two thereof.

[0020] Preferably, the accelerator in step S3 is selected from any one of triethylamine, sodium hydroxide and urea, or a combination of at least two thereof.

[0021] Preferably, the drying method in step S3 is spray drying.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) β-cyclodextrin is introduced into the cerium-modified alumina-supported copper-nickel composite of the present invention as the main body of the metal complex, and the strong interaction between the highly dispersed nickel particles and the alumina carrier is utilized to prevent the loss of nickel during the reaction. The nickel-cerium interaction prevents the formation of nickel aluminate and promotes the formation of nickel nanoparticles, thereby obtaining high activity and high selectivity.

[0024] (2) The POSS-loaded palladium-nickel composite of the present invention can form palladium-nickel particles by first loading palladium and then loading nickel, and improve the reducibility of nickel. At the same time, the reversible hydrogen storage capacity of cerium in the cerium-modified alumina-loaded copper-nickel composite carrier is combined with the cerium-modified alumina-loaded copper-nickel composite carrier to synergistically improve the reaction activity. DETAILED DESCRIPTION

[0025] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0026] The sources of some components in the embodiments and comparative examples are as follows:

[0027] β-Cyclodextrin CAS No. 7585-39-9; Copper nitrate CAS No. 3251-23-8; Nickel nitrate hexahydrate CAS No. 13478-00-7 Aluminum oxide CAS No. 1344-28-1; Cerium nitrate CAS No. 10294-41-4; Sodium hydroxide CAS No. 1310-73-2; Citric acid CAS No. 77-92-9; Palladium nitrate CAS No. 10102-05-3; Anhydrous nickel nitrate CAS No. 14216-75-2; Sodium dodecyl sulfate CAS No. 151-21-3; Vinyl POSS CAS No. 69655-76-1; Methacrylic acid CAS No. 79-41-4; Ammonium persulfate CAS No. 7727-54-0; Sodium bisulfite CAS No. 7631-90-5.

[0028] Preparation of alumina-supported copper-nickel complex: Add 5 parts of β-cyclodextrin (CAS No. 7585-39-9) to 250 parts of deionized water, stir for 0.1 h, add 15 parts of copper nitrate (CAS No. 3251-23-8) and 10 parts of nickel nitrate hexahydrate (CAS No. 13478-00-7), stir for 2 h, and then add 50 parts of alumina to obtain a solid suspension; stir the solid suspension at room temperature for 2 h, rotary evaporate at 60°C to obtain a solid, dry the solid, and calcine to obtain an alumina-supported copper-nickel complex.

[0029] Preparation of POSS-loaded palladium-nickel complex: Add 3 parts of palladium nitrate (CAS No. 10102-05-3) to 50 parts of deionized water, stir evenly to obtain a palladium nitrate solution, add 5 parts of anhydrous nickel nitrate (CAS No. 14216-75-2) to 50 parts of deionized water, stir evenly to obtain a nickel nitrate solution; immerse 20 parts of vinyl POSS (CAS No. 69655-76-1) in 100 parts of palladium nitrate solution for 1 hour, and dry at 80° C. for 24 hours to obtain a palladium-loaded solid; immerse the palladium-loaded solid in 100 parts of nickel nitrate solution for 2 hours, dry after immersion, and calcine to obtain a POSS-loaded palladium-nickel complex. Example 1

[0030] This embodiment provides a method for preparing a catalyst for producing tertiary amines, comprising the following steps:

[0031] Step S1: (1) Add 5 parts of aluminum oxide (CAS No. 1344-28-1) to 50 parts of deionized water, stir at 80°C for 1 hour, then add 3 parts of cerium nitrate (CAS No. 10294-41-4) and stir for 0.5 hour. After stirring evenly, add 1 part of sodium hydroxide (CAS No. 1310-73-2) and 1 part of citric acid (CAS No. 77-92-9), react for 2.5 hours, cool to room temperature, vacuum filter, and wash the solid with deionized water to pH = 7. Dry the solid at 120°C for 24 hours, and then calcine at 600°C for 6 hours to obtain cerium-modified aluminum oxide. (2) Add 5 parts of β-cyclodextrin (CAS No. 7585-39-9) to 250 parts of deionized water, stir for 0.1 h, add 15 parts of copper nitrate (CAS No. 3251-23-8) and 10 parts of nickel nitrate hexahydrate (CAS No. 13478-00-7), stir for 2 h, and then add 50 parts of cerium-modified alumina to obtain a solid suspension; stir the solid suspension at room temperature for 2 h, rotary evaporate at 60 ° C to obtain a solid, dry the solid (temperature is 120 ° C, time is 24 h), and calcine (temperature is 400 ° C, time is 6 h) to obtain a cerium-modified alumina-loaded copper-nickel complex.

[0032] Step S2: (1) Add 1 part of sodium dodecyl sulfate (CAS No. 151-21-3) to 100 parts of deionized water, control the temperature to 60°C, add 5 parts of vinyl POSS (CAS No. 69655-76-1), and stir to react for 2 hours; then add 10 parts of methacrylic acid (CAS No. 79-41-4), 2 parts of ammonium persulfate (CAS No. 7727-54-0) and 0.5 parts of sodium bisulfite (CAS No. 7631-90-5) and react for 4 hours. After the reaction is completed, cool to room temperature, dry at 110°C for 24 hours to obtain carboxylated POSS. (2) Add 3 parts of palladium nitrate (CAS No. 10102-05-3) to 50 parts of deionized water, stir evenly to obtain a palladium nitrate solution, add 5 parts of anhydrous nickel nitrate (CAS No. 14216-75-2) to 50 parts of deionized water, stir evenly to obtain a nickel nitrate solution; immerse 20 parts of carboxylated POSS in 100 parts of palladium nitrate solution for 1 hour, and dry at 80°C for 24 hours to obtain a solid loaded with palladium; immerse the palladium-loaded solid in 100 parts of nickel nitrate solution for 2 hours, dry after immersion (temperature is 100°C, drying time is 36 hours), and calcine (temperature is 400°C, calcination time is 2 hours) to obtain a carboxylated POSS loaded with palladium-nickel complex.

[0033] Step S3: Add 50 parts of cerium-modified alumina-loaded copper-nickel complex and 20 parts of carboxylated POSS-loaded palladium-nickel complex to 200 parts of methanol, stir for 1 hour, add 5 parts of sodium hydroxide, stir at 70° C. for 5 hours, and spray dry to obtain a catalyst for tertiary amine production. Example 2

[0034] This embodiment provides a method for preparing a catalyst for producing tertiary amines, comprising the following steps:

[0035] Step S1: (1) Add 5 parts of aluminum oxide (CAS No. 1344-28-1) to 50 parts of deionized water, stir at 80°C for 1 hour, then add 3 parts of cerium nitrate (CAS No. 10294-41-4) and stir for 0.5 hour. After stirring evenly, add 1 part of sodium hydroxide (CAS No. 1310-73-2) and 1 part of citric acid (CAS No. 77-92-9), react for 2.5 hours, cool to room temperature, vacuum filter, and wash the solid with deionized water to pH = 7. Dry the solid at 120°C for 24 hours, and then calcine at 600°C for 6 hours to obtain cerium-modified aluminum oxide. (2) Add 5 parts of β-cyclodextrin (CAS No. 7585-39-9) to 250 parts of deionized water, stir for 0.1 h, add 15 parts of copper nitrate (CAS No. 3251-23-8) and 10 parts of nickel nitrate hexahydrate (CAS No. 13478-00-7), stir for 2 h, and then add 50 parts of cerium-modified alumina to obtain a solid suspension; stir the solid suspension at room temperature for 2 h, rotary evaporate at 60 ° C to obtain a solid, dry the solid (temperature is 100 ° C, time is 36 h), and calcine (temperature is 450 ° C, time is 4 h) to obtain a cerium-modified alumina-loaded copper-nickel complex.

[0036] Step S2: (1) Add 1 part of sodium dodecyl sulfate (CAS No. 151-21-3) to 100 parts of deionized water, control the temperature to 60°C, add 5 parts of vinyl POSS (CAS No. 69655-76-1), and stir to react for 2 hours; then add 10 parts of methacrylic acid (CAS No. 79-41-4), 2 parts of ammonium persulfate (CAS No. 7727-54-0) and 0.5 parts of sodium bisulfite (CAS No. 7631-90-5) and react for 4 hours. After the reaction is completed, cool to room temperature, dry at 110°C for 24 hours to obtain carboxylated POSS. (2) Add 3 parts of palladium nitrate (CAS No. 10102-05-3) to 50 parts of deionized water and stir to obtain a palladium nitrate solution; add 5 parts of anhydrous nickel nitrate (CAS No. 14216-75-2) to 50 parts of deionized water and stir to obtain a nickel nitrate solution; immerse 20 parts of carboxylated POSS in 100 parts of palladium nitrate solution for 1 hour, and dry at 80°C for 24 hours to obtain a solid loaded with palladium; immerse the solid loaded with palladium in 100 parts of nickel nitrate solution for 2 hours, dry after immersion (temperature is 90°C, drying time is 48 hours), and calcine (temperature is 350°C, calcination time is 4 hours) to obtain a carboxylated POSS loaded with palladium-nickel complex.

[0037] Step S3: Add 50 parts of cerium-modified alumina-loaded copper-nickel complex and 20 parts of carboxylated POSS-loaded palladium-nickel complex to 200 parts of isopropanol, stir for 1 hour, add 5 parts of triethylamine, stir at 70° C. for 5 hours, and spray dry to obtain a catalyst for tertiary amine production. Example 3

[0038] This embodiment provides a method for preparing a catalyst for producing tertiary amines, comprising the following steps:

[0039] Step S1: (1) Add 5 parts of aluminum oxide (CAS No. 1344-28-1) to 50 parts of deionized water, stir at 80°C for 1 hour, then add 3 parts of cerium nitrate (CAS No. 10294-41-4) and stir for 0.5 hour. After stirring evenly, add 1 part of sodium hydroxide (CAS No. 1310-73-2) and 1 part of citric acid (CAS No. 77-92-9), react for 2.5 hours, cool to room temperature, vacuum filter, and wash the solid with deionized water to pH = 7. Dry the solid at 120°C for 24 hours, and then calcine at 600°C for 6 hours to obtain cerium-modified aluminum oxide. (2) Add 5 parts of β-cyclodextrin (CAS No. 7585-39-9) to 250 parts of deionized water, stir for 0.1 h, add 15 parts of copper nitrate (CAS No. 3251-23-8) and 10 parts of nickel nitrate hexahydrate (CAS No. 13478-00-7), stir for 2 h, and then add 50 parts of cerium-modified alumina to obtain a solid suspension; stir the solid suspension at room temperature for 2 h, rotary evaporate at 60 ° C to obtain a solid, dry the solid (temperature 110 ° C, time 30 h), and calcine (temperature 420 ° C, time 5 h) to obtain a cerium-modified alumina-loaded copper-nickel complex.

[0040] Step S2: (1) Add 1 part of sodium dodecyl sulfate (CAS No. 151-21-3) to 100 parts of deionized water, control the temperature to 60°C, add 5 parts of vinyl POSS (CAS No. 69655-76-1), and stir to react for 2 hours; then add 10 parts of methacrylic acid (CAS No. 79-41-4), 2 parts of ammonium persulfate (CAS No. 7727-54-0) and 0.5 parts of sodium bisulfite (CAS No. 7631-90-5) and react for 4 hours. After the reaction is completed, cool to room temperature, dry at 110°C for 24 hours to obtain carboxylated POSS. (2) Add 3 parts of palladium nitrate (CAS No. 10102-05-3) to 50 parts of deionized water, stir evenly to obtain a palladium nitrate solution, add 5 parts of anhydrous nickel nitrate (CAS No. 14216-75-2) to 50 parts of deionized water, stir evenly to obtain a nickel nitrate solution; immerse 20 parts of carboxylated POSS in 100 parts of palladium nitrate solution for 1 hour, and dry at 80°C for 24 hours to obtain a solid loaded with palladium; immerse the solid loaded with palladium in 100 parts of nickel nitrate solution for 2 hours, dry after immersion (temperature is 95°C, drying time is 40 hours), and calcine (temperature is 380°C, calcination time is 3 hours) to obtain a carboxylated POSS loaded with palladium-nickel complex.

[0041] Step S3: Add 50 parts of cerium-modified alumina-loaded copper-nickel complex and 20 parts of carboxylated POSS-loaded palladium-nickel complex to 200 parts of ethanol, stir for 1 hour, add 5 parts of urea, stir at 70° C. for 5 hours, and spray dry to obtain a catalyst for tertiary amine production. Example 4

[0042] This embodiment provides a method for preparing a catalyst for producing tertiary amines. The difference from Embodiment 1 is that in this embodiment, the cerium-modified alumina-supported copper-nickel composite is replaced by an alumina-supported copper-nickel composite. Example 5

[0043] This embodiment provides a method for preparing a catalyst for producing tertiary amines. The difference from Embodiment 1 is that in this embodiment, the carboxylated POSS-supported palladium-nickel complex is replaced by a POSS-supported palladium-nickel complex.

[0044] Comparative Example 1

[0045] This comparative example provides a method for preparing a catalyst for the production of tertiary amines, comprising the following steps: preparation of an alumina-loaded copper complex: adding 15 parts of copper nitrate (CAS No. 3251-23-8) to 250 parts of deionized water, stirring for 2 hours, and then adding 50 parts of alumina to obtain a solid suspension; stirring the solid suspension at room temperature for 2 hours, rotary evaporating at 60°C to obtain a solid, drying the solid (temperature of 100°C for 36 hours), and calcining (temperature of 450°C for 4 hours) to obtain an alumina-loaded copper complex, which is a catalyst for the production of tertiary amines.

[0046] Comparative Example 2

[0047] This comparative example provides a method for preparing a catalyst for the production of tertiary amines, comprising the following steps: adding 5 parts of β-cyclodextrin (CAS No. 7585-39-9) to 250 parts of deionized water, stirring for 0.1 h, adding 15 parts of copper nitrate (CAS No. 3251-23-8) and 10 parts of nickel nitrate hexahydrate (CAS No. 13478-00-7), stirring for 2 h, and then adding 50 parts of aluminum oxide to obtain a solid suspension; stirring the solid suspension at room temperature for 2 h, rotary evaporating at 60° C. to obtain a solid, drying the solid (temperature of 100° C. for 36 h), and calcining (temperature of 450° C. for 4 h) to obtain an aluminum oxide-supported copper-nickel complex, wherein the aluminum oxide-supported copper-nickel complex is the catalyst for the production of tertiary amines.

[0048] Comparative Example 3

[0049] This comparative example provides a method for preparing a catalyst for producing tertiary amines, comprising the following steps: adding 5 parts of aluminum oxide (CAS No. 1344-28-1) to 50 parts of deionized water, stirring at 80°C for 1 hour, adding 3 parts of cerium nitrate (CAS No. 10294-41-4) and stirring for 0.5 hour, adding 1 part of sodium hydroxide (CAS No. 1310-73-2) and 1 part of citric acid (CAS No. 77-92-9) after stirring evenly, reacting for 2.5 hours, cooling to room temperature, vacuum filtering, washing the solid with deionized water to pH=7, drying the solid at 120°C for 24 hours, and then calcining at 600°C for 6 hours to obtain cerium-modified aluminum oxide. Add 5 parts of β-cyclodextrin (CAS No. 7585-39-9) to 250 parts of deionized water, stir for 0.1h, add 15 parts of copper nitrate (CAS No. 3251-23-8) and 10 parts of nickel nitrate hexahydrate (CAS No. 13478-00-7), stir for 2h, and then add 50 parts of cerium-modified alumina to obtain a solid suspension; stir the solid suspension at room temperature for 2h, rotary evaporate at 60°C to obtain a solid, dry the solid (temperature is 100°C, time is 36h), calcine (temperature is 450°C, time is 4h) to obtain a cerium-modified alumina-loaded copper-nickel complex, and the cerium-modified alumina-loaded copper-nickel complex is a catalyst for tertiary amine production. Example 6

[0050] The catalysts provided in the above examples and comparative examples were respectively used for the preparation of tertiary amines, and the preparation process is as follows:

[0051] 1000 parts of decanol (CAS No. 85566-12-7) and 10 parts of catalyst were added into the reactor, stirred evenly, and hydrogen was introduced to the bottom of the reactor at a rate of 100 L / min. After 5 minutes, the oil bath was turned on for heating, the temperature was raised to 190°C, and the temperature was kept for 2 hours. The temperature in the reactor was adjusted to 180°C by oil bath, and liquid ammonia (CAS No. 7664-41-7) and hydrogen were introduced to the bottom of the reactor at a rate of 70 L / min, respectively, and the temperature was kept for 5 hours. The reaction liquid was distilled to obtain the finished product.

[0052] The tertiary amine value of the finished product provided in the application example was measured, and the test was performed with reference to the method of patent "CN111841552A".

[0053] The specific determination method of tertiary amine value is as follows: weigh about 0.30g sample into a 100ml beaker, add 10ml acetic anhydride (CAS No. 108-24-7), then add 30ml isopropanol (CAS No. 67-63-0), mix well. Add 3 drops of indicator, titrate with 0.1mol / L hydrochloric acid standard solution until it suddenly turns bright yellow as the end point, and record the corresponding volume (V0).

[0054] Calculate the tertiary amine value (mgKOH / g): = (V0×C×56.1) / m;

[0055] V0: volume of hydrochloric acid standard solution consumed for titrating amine value, ml;

[0056] C: concentration of hydrochloric acid standard solution, mol / L;

[0057] m: sample mass, g;

[0058] 56.1: Molar mass of potassium hydroxide, g / mol.

[0059] The above performance test data is shown in Table 1:

[0060] Table 1 Performance test results

[0061]

[0062] From the above content, it can be seen that the present invention obtains a catalyst for tertiary amine production by selecting a synergistic combination of alumina-supported copper-nickel composite and POSS-supported palladium-nickel composite, and by compounding the carrier materials of the two. The tertiary amine value of the finished products prepared by the catalyst (Application Examples 1 to 3) is 136 to 138 mgKOH / g.

[0063] Compared with Application Example 1, if cerium-modified alumina is not used to load copper-nickel composite, the tertiary amine value in the finished product is reduced (Application Example 4); compared with Application Example 1, if carboxylated POSS is not used to load palladium-nickel composite, the tertiary amine value in the finished product is reduced (Application Example 5).

[0064] The catalyst of Comparative Example 1 does not adopt the technical innovation of the present invention, so the performance is poor, and the tertiary amine value in the prepared finished product is 85 mgKOH / g (Application Example 6); compared with Application Example 6, if alumina-supported copper-nickel composite is used as a catalyst, the tertiary amine value in the finished product is increased (Application Example 7); compared with Application Example 6, if cerium-modified alumina-supported copper-nickel composite is used as a catalyst, the tertiary amine value in the finished product is increased (Application Example 8).

[0065] The present invention selects a synergistic combination of an alumina-supported copper-nickel complex and a POSS-supported palladium-nickel complex, and compounding the two carrier materials so that active components in the catalyst can influence each other, give full play to the catalytic effect of the metal active components, promote the improvement of reaction activity, and achieve high selectivity.

[0066] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a catalyst for tertiary amine production, characterized in that: The preparation method comprises the following steps: Step S1: adding 5 parts of β-cyclodextrin to 250 parts of deionized water, stirring for 0.1 h, adding 15 parts of copper nitrate and 10 parts of nickel nitrate hexahydrate, stirring for 2 h, and then adding 50 parts of aluminum oxide to obtain a solid suspension; stirring the solid suspension at room temperature for 2 h, rotary evaporating at 60° C. to obtain a solid, drying the solid, and calcining to obtain an aluminum oxide-loaded copper-nickel complex; Step S2: adding 3 parts of palladium nitrate to 50 parts of deionized water, stirring to obtain a palladium nitrate solution, adding 5 parts of anhydrous nickel nitrate to 50 parts of deionized water, stirring to obtain a nickel nitrate solution; immersing 20 parts of POSS in 100 parts of palladium nitrate solution for 1 hour, drying at 80° C. for 24 hours to obtain a palladium-loaded solid; immersing the palladium-loaded solid in 100 parts of nickel nitrate solution for 2 hours, drying after immersion, and calcining to obtain a POSS-loaded palladium-nickel complex; Step S3: adding 50 parts of alumina-supported copper-nickel complex and 20 parts of POSS-supported palladium-nickel complex to 200 parts of organic solvent, stirring for 1 hour, adding 5 parts of accelerator, stirring for 5 hours at 70° C., and drying to obtain a catalyst for tertiary amine production; The POSS described in step S2 is carboxylated POSS; the preparation method of the carboxylated POSS is: add 1 part of sodium dodecyl sulfate to 100 parts of deionized water, control the temperature to 60°C, add 5 parts of vinyl POSS, and stir to react for 2h; then add 10 parts of methacrylic acid, 2 parts of ammonium persulfate and 0.5 part of sodium bisulfite to react for 4h, cool to room temperature after the reaction is completed, and dry at 110°C for 24h to obtain carboxylated POSS; The accelerator described in step S3 is selected from any one of triethylamine, sodium hydroxide, and urea, or a combination of at least two thereof.

2. The method for preparing a catalyst for producing tertiary amines according to claim 1, characterized in that: The aluminum oxide described in step S1 is cerium-modified aluminum oxide.

3. The method for preparing a catalyst for producing tertiary amines according to claim 2, characterized in that: The preparation method of the cerium-modified alumina is as follows: add 5 parts of alumina to 50 parts of deionized water, stir at 80°C for 1 hour, then add 3 parts of cerium nitrate and stir for 0.5 hour, add 1 part of sodium hydroxide and 1 part of citric acid after stirring evenly, react for 2.5 hours, cool to room temperature, vacuum filter, wash the solid with deionized water to pH=7, dry the solid at 120°C for 24 hours, and then calcine at 600°C for 6 hours to obtain cerium-modified alumina.

4. The method for preparing a catalyst for producing tertiary amines according to claim 1, characterized in that: The drying temperature in step S1 is 100-120° C., the drying time is 24-36 hours, the calcination temperature is 400-450° C., and the calcination time is 4-6 hours.

5. The method for preparing a catalyst for producing tertiary amines according to claim 1, characterized in that: The drying temperature in step S2 is 90-100° C., the drying time is 36-48 hours, the calcination temperature is 350-400° C., and the calcination time is 2-4 hours.

6. The method for preparing a catalyst for producing tertiary amines according to claim 1, characterized in that: The organic solvent described in step S3 is selected from any one of methanol, ethanol, and isopropanol, or a combination of at least two of them.

7. The method for preparing a catalyst for producing tertiary amines according to claim 1, characterized in that: The drying method described in step S3 is spray drying.

Citation Information

Patent Citations

  • Routing of network traffic

    CA1310732C

  • Milk receiver

    CA51213A

  • Tertiary amine preparation process

    CN103270015A

  • Catalyst for synthesizing Trioctyl / tridecylaklylamines and preparation method and application of catalyst