Multistage porous carbon nitride material as well as preparation method and application thereof
By using melamine, cyanuric acid and cobalt salt salt thermal reaction to prepare hierarchical porous carbon nitride materials, the low efficiency problem of existing carbon nitride materials in photocatalytic reactions is solved, and efficient photocatalytic effects and material properties are achieved. Improved stability.
Patent Information
- Application Number
- CN202310376010.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-15
AI Technical Summary
The low efficiency and instability of existing carbon nitride materials in photocatalytic reactions, especially the insufficient conductivity and visible light absorption range of graphitic phase carbon nitride materials, limit their industrial promotion and application.
Melamine, cyanuric acid and cobalt salts are used as precursors to prepare multi-level porous carbon nitride materials through hydrothermal reaction, avoiding the use of organic solvents and templates, adjusting the concentration ratio of reactants to control the material structure and improve the photocatalytic reaction efficiency.
It achieves a simple and green preparation without external templates, significantly improves the specific surface area and photocatalytic reaction efficiency of carbon nitride materials, provides a rich pore structure and active sites, and improves photocatalytic activity.
Smart Images

Figure HDA0004170412230000011 
Figure HDA0004170412230000021 
Figure HDA0004170412230000031
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of carbon nitride material preparation, and in particular to a carbon nitride material with a controllable multi-level porous structure, a preparation method thereof, and an application thereof in a photocatalytic reaction. Background Art
[0002] Photocatalytic technology is a catalytic reaction driven by solar energy that can achieve energy conversion and storage. Among them, photocatalytic reduction of carbon dioxide (CO2) technology can convert CO2 into high value-added products such as hydrocarbon fuels such as methanol, methane, carbon monoxide (CO), and is a potential way to utilize CO2.
[0003] The development of photocatalysis began in the 1970s, but the low efficiency and poor stability of photocatalytic materials limit their feasibility in industrial application. Graphite carbon nitride (g-C3N4) has been favored by researchers due to its suitable band gap (2.7eV), low cost, and high thermal and chemical stability. However, graphite carbon nitride materials still have the following disadvantages: high recombination efficiency of photogenerated carriers, poor conductivity and visible light absorption range.
[0004] To solve the above problems, a large number of strategies for modifying carbon nitride materials have emerged, such as structural design, co-catalysts or heteroatom loading. From the perspective of heteroatom loading, rich heteroatoms with different functions, including metal heteroatoms and non-metal heteroatoms, have been successfully introduced into the surface or skeleton of carbon nitride, such as metal heteroatoms platinum and palladium that act as co-catalysts, and non-metallic elements such as sulfur and phosphorus that are used to change the surface electronic structure. From a structural perspective, in addition to two-dimensional layered carbon nitride, mesoporous carbon nitride and tubular hollow carbon nitride have also been developed.
[0005] Generally speaking, the edge of carbon nitride is more likely to achieve catalytic reactions. Therefore, two-dimensional carbon nitride with a porous structure is theoretically more conducive to improving catalytic efficiency, and the unsaturated sites at the porous structure are more conducive to the loading of heterogeneous atoms. There are many methods for preparing carbon nitride with rich porous structures, such as template method, solvent thermal method, multiple calcination method, etc.
[0006] However, the above-mentioned preparation method has the phenomena of template removal, use of organic solvents, and high energy consumption. For example, the invention patent application CN114931965A discloses a porous graphite phase carbon nitride supported non-precious metal bismuth catalyst, which uses melamine, phosphorous acid and bismuth salicylate as raw materials, and prepares the precursor by hydrothermal method. The precursor is dispersed in a mixed solvent of ethanol and glycerol, stirred and refluxed under a 90°C water bath, then separated and washed, and dried for standby use. The dried intermediate is then calcined at high temperature in an inert atmosphere to prepare a bismuth-loaded porous graphite phase carbon nitride (Bi-PCN) catalyst. The porous structure of the catalyst promotes the effective contact between the material and the adsorbed molecules and the dispersion of heteroatom bismuth, and the load of non-precious metal bismuth greatly improves the light absorption of carbon nitride materials in the visible light range. However, a variety of reagents are used in the preparation process of the above-mentioned catalyst, and the obtained catalyst presents a two-dimensional sheet structure and does not have the controllability of the morphology.
[0007] Therefore, there is an urgent need to find a simpler, green and controllable method to prepare carbon nitride materials with rich pore structures. Summary of the invention
[0008] The purpose of the present invention is to provide a carbon nitride material with a multi-level porous structure and a preparation method and use thereof, aiming to improve the catalytic reaction efficiency of the carbon nitride material in a photocatalytic reaction by regulating the structure of the obtained carbon nitride material.
[0009] In order to achieve the above-mentioned object of the invention, the present invention provides a method for preparing a multi-level porous carbon nitride material, which comprises:
[0010] Providing melamine aqueous solution, cyanuric acid aqueous solution and cobalt salt;
[0011] Mixing the melamine aqueous solution with the cyanuric acid aqueous solution to obtain a mixed solution;
[0012] The mixed solution and the cobalt salt are mixed and subjected to hydrothermal reaction to obtain a precursor;
[0013] The precursor is calcined to obtain a multi-level porous carbon nitride material.
[0014] Another aspect of the present invention provides a multi-level porous carbon nitride material, which is prepared by the preparation method provided by the present invention.
[0015] In another aspect, the present invention provides use of the multi-level porous carbon nitride material in a photocatalytic reaction.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] 1) In the preparation method of the multi-level porous carbon nitride material provided by the present invention, melamine, cyanuric acid and cobalt salt are used as precursors of carbon nitride. No organic solvent is required in the preparation process, and no external template or molding aid is introduced. It has the advantages of simple process and greenness, and also avoids the problem of covering the active sites of carbon nitride and affecting the utilization rate of the catalyst body by the use of organic aids;
[0018] 2) In the preparation method of the multi-level porous carbon nitride material provided by the present invention, by adjusting the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt, the structure of the obtained multi-level porous carbon nitride material can be controlled, and the adsorption of the reaction raw materials and the multiple utilization effect of the incident light by the carbon nitride material can be further improved, thereby significantly improving the efficiency of the photocatalytic reaction;
[0019] 3) The carbon nitride material provided by the present invention is a three-dimensional multi-level porous material loaded with cobalt, and its specific surface area is 130-220m 2 / g, the cross-sectional size is micron-level, and the material surface and interior have rich pore structures, which are beneficial to the adsorption of reaction raw materials and provide active sites in the photocatalytic reaction, and have high photocatalytic reaction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The scanning electron microscope image of the carbon nitride material provided in Example 1 of the present invention; wherein, a is a scanning electron microscope image (SEM) of the CN-5 sample, and the overall morphology of the sample is uniform; b is an enlarged SEM image, and it can be seen that the filamentous carbon nitride forms nanosheets, and part of the filamentous carbon nitride on one side is connected with part of the filamentous carbon nitride on the other side; c is a further enlarged SEM image, which clearly shows the structure and size of the filamentous carbon nitride of CN-5;
[0021] Figure 2 The scanning electron microscope image of the carbon nitride material provided in Example 2 of the present invention; wherein a is a scanning electron microscope image (SEM) of the CN-1 sample; b is an enlarged SEM image showing the internal flaky structure;
[0022] Figure 3 A scanning electron microscope image of the carbon nitride material provided in Example 3 of the present invention;
[0023] Figure 4 A scanning electron microscope image of the carbon nitride material provided in Example 4 of the present invention;
[0024] Figure 5 A scanning electron microscope image of the carbon nitride material provided in Example 5 of the present invention;
[0025] Figure 6 XRD diagram of the carbon nitride material provided in Examples 1 and 5 of the present invention;
[0026] Figure 7 FTIR images of carbon nitride materials provided in Examples 1 to 5 of the present invention;
[0027] Figure 8 These are the thermogravimetric analysis results of the carbon nitride materials provided in Examples 1 to 5 of the present invention. DETAILED DESCRIPTION
[0028] The inventors of the present invention have found in their research that when carbon nitride materials are prepared using melamine, cyanuric acid and cobalt salt as raw materials, the concentration of melamine-cyanuric acid and the amount of cobalt salt added have a direct effect on the morphology (e.g., pores) of the obtained carbon nitride materials, and the morphology of the carbon nitride materials is correlated with their catalytic efficiency in photocatalytic reactions. On this basis, the present invention was completed.
[0029] Specifically, an embodiment of the present invention provides a method for preparing a multi-level porous carbon nitride material, which comprises:
[0030] S1, providing a melamine aqueous solution, a cyanuric acid aqueous solution and a cobalt salt;
[0031] S2, mixing the melamine aqueous solution and the cyanuric acid aqueous solution to obtain a mixed solution;
[0032] S3, the mixed solution and the cobalt salt are mixed and hydrothermally reacted to obtain a precursor;
[0033] S4. The precursor is calcined to obtain a multi-level porous carbon nitride material.
[0034] Specifically, in S1, in some embodiments, the concentration of the melamine aqueous solution is 20-100 mmol / L; the concentration of the cyanuric acid aqueous solution is 20-100 mmol / L. In some preferred embodiments, the concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution are 50-100 mmol / L. A higher concentration is conducive to the explosive crystallization of melamine-cyanuric acid macromolecules, thereby obtaining a precursor with a small microscopic grain size, and the microscopic size of the carbon nitride material obtained after calcination is small, which is conducive to increasing the specific surface area of the material. Specifically, the concentration of the melamine aqueous solution is 20mmol / L, 30mmol / L, 40mmol / L, 50mmol / L, 60mmol / L, 70mmol / L, 80mmol / L, 90mmol / L or 100mmol / L; the concentration of the cyanuric acid aqueous solution is 20mmol / L, 30mmol / L, 40mmol / L, 50mmol / L, 60mmol / L, 70mmol / L, 80mmol / L, 90mmol / L or 100mmol / L.
[0035] In some embodiments, the cobalt salt is cobalt nitrate or cobalt chloride. The inventors of the present invention have found that the carbon nitride material provided by the embodiment of the present invention has a good catalytic effect when loaded with cobalt, which is presumably because the structure of the carbon nitride material is more conducive to the transfer of electrons during the catalytic reaction when loaded with cobalt.
[0036] In some embodiments, the concentration of the cobalt salt is 5-30 mmol / L. Specifically, the concentration of the cobalt salt is 5 mmol / L, 10 mmol / L, 15 mmol / L, 20 mmol / L, 25 mmol / L or 30 mmol / L.
[0037] In S2, when the melamine aqueous solution and the cyanuric acid aqueous solution are mixed, the two are preassembled by hydrogen bonding to form a melamine-cyanuric acid macromolecule, which is one of the basic structures for the subsequent formation of a three-dimensional multi-layered structure of carbon nitride. In some preferred embodiments, the melamine aqueous solution and the cyanuric acid aqueous solution are mixed in equal volumes and equimolar concentrations.
[0038] In some embodiments, the mixing treatment may be carried out by stirring, and the mixing treatment time is 0.5-2 hours. Specifically, the mixing treatment time is 0.5 hours, 1 hour, 1.5 hours or 2 hours.
[0039] In some embodiments, the pH of the mixed solution obtained by the mixing treatment is adjusted to 1-2. In the embodiments of the present invention, by adjusting the pH of the mixed solution within this range, it is beneficial to form a monodisperse cobalt atom loading form in the hydrothermal synthesis and avoid the existence of cobalt oxide. In some specific embodiments, the pH is adjusted to 1, 1.5 or 2. The embodiments of the present invention do not particularly limit the method for adjusting the pH, for example, it can be adjusted by adding an appropriate amount of HCl.
[0040] In S3, the mixed solution and the cobalt salt are mixed by stirring. In some embodiments, the mixed solution and the cobalt salt are mixed for 2-4 hours. In some specific embodiments, the mixing time is 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours.
[0041] In some embodiments, the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt is (3-7.5):1, preferably, the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt is (3-4.5):1. Wherein, when the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt is (3.5-4.5):1, the obtained carbon nitride material is a micro-nanoscale material composed of stacked nanosheets formed by filamentous carbon nitride, and the specific surface area is 190-220m 2 / g, and the diameter of the filamentous carbon nitride is 20-70nm, and the length of the filamentous carbon nitride is 0.5-4.5μm (wherein the filamentous carbon nitride has basically or completely no branching structure, and part of the filamentous carbon nitride on one side is linked with part of the filamentous carbon nitride on the other side). When the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt is ≥6:1, the obtained carbon nitride material is a micro-nanoscale material formed by stacking carbon nitride nanosheets (whose thickness is less than 100nm), and the specific surface area is 130-160m 2 / g (wherein, the carbon nitride nanosheets do not contain filamentous carbon nitride structures or dendritic carbon nitride structures). When the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt is (4.5-5.5):1, the obtained carbon nitride material is a micro-nanoscale material composed of stacked nanosheets formed by dendritic carbon nitride, and the specific surface area is 150-170m 2 / g (wherein, the dendritic carbon nitride is a dendritic structure with multiple branches, and the branches on the dendritic carbon nitride are not only connected to other branches on the nanosheet layer where it is located, but also can be connected to branches on other nanosheet layers, thereby forming a rich pore structure).
[0042] As described above, the embodiment of the present invention can control the internal structure of the obtained carbon nitride material by controlling the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt, thereby obtaining a multi-level porous carbon nitride material with a larger specific surface area for photocatalytic reaction. Specifically, the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt is 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1 or 7.5:1.
[0043] As a preferred embodiment, the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt is (3.5-4.5):1, such as 3.5:1, 3.6:1, 3.7:1, 3.8:1, 3.9:1, 4.0:1, 4.1:1, 4.2:1, 4.3:1, 4.4:1 or 4.5:1. At this time, the obtained carbon nitride material is composed of a network formed by filamentous carbon nitride, with a rich pore structure on the surface and inside, and there is no problem of dense stacking, and the specific surface area is larger, which is conducive to light penetration into the interior of the material, extending the light path, and thus improving the photocatalytic activity.
[0044] In some embodiments, the hydrothermal reaction is carried out at 160-180°C for 10-20h. In some specific embodiments, the temperature of the hydrothermal reaction is 160°C, 165°C, 170°C, 175°C or 180°C. The time of the hydrothermal reaction is 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h or 20h. The embodiment of the present invention does not particularly limit the container for the hydrothermal reaction, for example, it can be carried out in a reactor.
[0045] After the hydrothermal reaction is completed, a crystalline product is obtained as a precursor. In some embodiments, the crystalline product is further centrifuged, washed, and dried.
[0046] In S4, in some embodiments, the calcination treatment is carried out in an inert atmosphere at 500-550°C for 2-4h. In some specific embodiments, the calcination temperature is 500°C, 510°C, 520°C, 530°C, 540°C or 550°C. In some specific embodiments, the calcination time is 2h, 2.5h, 3h, 3.5h or 4h. Preferably, the inert atmosphere is N2 or Ar2; further preferably, the inert atmosphere is introduced in an amount of 100ml / min. The embodiment of the present invention does not particularly limit the calcination equipment, for example, it can be carried out in a tubular furnace.
[0047] Correspondingly, an embodiment of the present invention further provides a multi-level porous carbon nitride material, which is prepared by the preparation method provided by the above embodiment of the present invention.
[0048] In some embodiments, the cobalt loading of the multi-level porous carbon nitride material is 2.1-11.0%. By containing cobalt in this range, the multi-level porous carbon nitride material is conducive to the transfer of electrons in the catalytic reaction as a catalyst. When the cobalt content is higher than 11.0%, the catalytic performance cannot be improved, which may be due to the excessive agglomeration of cobalt atoms affecting the exposure of active sites; when the cobalt content is lower than 2.1%, the coordination effect between cobalt ions and melamine-cyanuric acid macromolecules is reduced, which is not conducive to the formation of a multi-level porous structure of carbon nitride materials.
[0049] As described above, the embodiment of the present invention can regulate the internal structure of the obtained carbon nitride material by controlling the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt. During the preparation process, the melamine-cyanuric acid macromolecules self-assemble to form a hydrogen-bonded melamine-cyanuric acid supramolecular precursor, and at the same time, the free cobalt ions form a coordination effect with the CN bonds in the supramolecular to obtain a composite precursor. On this basis, the calcination treatment further affects the formation process of carbon nitride, and it is speculated that the cobalt ions will peel off the carbon nitride of the sheet layer between the layers and within the layers, and finally form a multi-level porous structure carbon nitride. When the ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt is (3.5-4.5): 1, a sufficient amount of cobalt ions can form an intercalation layer between the layers of the precursor, and at the same time form a ligand in the layer, and spontaneously peel off and polycondense to reduce the surface tension during the calcination process to obtain a multi-level porous carbon nitride composed of a network formed by filamentous carbon nitride. The formation of this structure can not only increase the specific surface area of the carbon nitride catalyst, but also provide more sites for the loading of cobalt atoms. When the content of cobalt ions is reduced, it is not enough to form ligands in the layer, and the obtained carbon nitride presents micro-nano carbon nitride stacked in layers. Accordingly, according to the morphological differences, the multi-level porous carbon nitride materials provided in the embodiments of the present invention can be divided into the following three categories:
[0050] (1) The multi-level porous carbon nitride material is a micro-nanoscale material composed of stacked nanosheets formed by filamentous carbon nitride, with a specific surface area of 190-210 m 2 / g, and the diameter of the filamentous carbon nitride is 20-70nm, and the length of the filamentous carbon nitride is 0.5-4.5μm;
[0051] (2) The multi-level porous carbon nitride material is a micro-nanoscale material formed by stacking nanosheet carbon nitride, with a specific surface area of 130-160m 2 / g, and the thickness of the carbon nitride nanosheet is less than 100nm;
[0052] (3) The multi-level porous carbon nitride material is a micro-nanoscale material composed of stacked nanosheets formed by dendritic carbon nitride, with a specific surface area of 150-170 m 2 / g.
[0053] In some embodiments, the diameter of the filamentous carbon nitride (i.e., the diameter of the filament) is 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, or 70 nm; the length of the filamentous carbon nitride (i.e., the length of the filament) is 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, or 4.5 μm.
[0054] In some embodiments, the cross-sectional length of the micro-nanoscale material formed by the filamentous carbon nitride is 2 to 5 μm, for example, 2 μm, 3 μm, 4 μm or 5 μm.
[0055] In some embodiments, the cross-sectional length of the micro-nanoscale material formed by stacking the nanosheet carbon nitride is 10-20 μm, for example, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm or 20 μm.
[0056] In some embodiments, the cross-sectional length of the micro-nanoscale material formed by the dendritic carbon nitride is 2 to 5 μm, for example, 2 μm, 3 μm, 4 μm or 5 μm.
[0057] In some embodiments, the specific surface area of the multi-level porous carbon nitride material is 130-220 m 2 / g. Specifically, the specific surface area of the multi-level porous carbon nitride material is 130m 2 / g, 140m 2 / g, 150m 2 / g, 160m 2 / g, 170m 2 / g, 180m 2 / g, 190m 2 / g, 200m 2 / g, 210m 2 / g or 220m 2 / g.
[0058] The multi-level porous carbon nitride material provided in the embodiment of the present invention can be used for the photocatalytic reduction reaction of carbon dioxide to carbon monoxide.
[0059] In some embodiments, in the catalytic reaction, CO2 gas is introduced in excess, and the ratio of H2O to the multi-level porous carbon nitride material provided in the embodiment of the present invention is 1:20 (ml:mg). For example, the amount of H2O is 5ml, and the amount of the multi-level porous carbon nitride material provided in the embodiment of the present invention is 100mg.
[0060] In order to enable the above implementation details and operations of the present invention to be clearly understood by those skilled in the art, and to significantly demonstrate the improved performance of the multi-level porous carbon nitride material and its preparation method and use in the embodiments of the present invention, the above technical scheme is illustrated by examples below.
[0061] The experimental methods in the following examples without specifying specific conditions are all conventional methods in the art. The materials used in the examples can be obtained from commercial sources unless otherwise specified.
[0062] Example 1
[0063] 1.1 Prepare 100mmol / L aqueous solutions of melamine and cyanuric acid respectively, mix and stir equal volumes (50ml each) for 0.5h, then add HCl to adjust the pH of the mixture to 2;
[0064] 1.2 Add 100 ml of 25 mmol / L cobalt nitrate to the mixed solution and stir for 4 hours;
[0065] 1.3 The solution obtained in step 1.2 was transferred to a reactor and subjected to hydrothermal reaction at 180°C for 10 h;
[0066] 1.4 After the hydrothermal reaction is completed, the product is cooled to room temperature to obtain a crystalline product, which is then centrifuged, washed, and freeze-dried to obtain a precursor;
[0067] 1.5 The precursor was placed in a tube furnace and calcined at 520°C for 2h, and an inert gas (Ar2) was introduced at a flow rate of 100ml / min for protection. After cooling, a carbon nitride material (CN-5) loaded with metallic cobalt was obtained, which was yellow in color.
[0068] 1.6 Under the irradiation of visible light, with a fixed pressure of CO2 and 5 ml of H2O as the raw materials for the catalytic reaction, and 100 mg of carbon nitride material (CN-5) as the catalyst, the yield of reducing CO2 to produce CO is 46.67 μmol / g.
[0069] Figure 1 The scanning electron microscope image of the carbon nitride material CN-5 loaded with metal cobalt shows that CN-5 is a three-dimensional network polyhedron material (cross-sectional length size 2-5 μm) composed of nanosheets stacked together by filamentous carbon nitride structures. The diameter of the filamentous carbon nitride is 20-70 nm and the length is 0.5-4.5 μm, indicating that the synthesized carbon nitride catalyst has a micro-nano multi-level structure with rich pore structures on its surface and inside, which is conducive to the adsorption of reaction raw materials and provides active sites. In addition, due to the low content of metal cobalt loaded (11.03%, obtained by thermogravimetric results, see Figure 8 ) and cobalt atoms are small, and no cobalt nanoparticles were observed.
[0070] After testing, the specific surface area of the carbon nitride material CN-5 obtained in this example is 203.05 m 2 / g.
[0071] Example 2
[0072] 2.1 Prepare 30mmol / L aqueous solutions of melamine and cyanuric acid respectively, mix and stir equal volumes (50ml each) for 0.5h, then add HCl to adjust the pH of the mixture to 2;
[0073] 2.2 Add 100 ml of 5 mmol / L cobalt nitrate to the mixture and stir for 4 hours;
[0074] 2.3 The solution obtained in step 2.2 was transferred to a reactor and subjected to hydrothermal reaction at 180°C for 10 h;
[0075] 2.4 After the hydrothermal reaction is completed, the product is cooled to room temperature to obtain a crystalline product, which is then centrifuged, washed, and freeze-dried to obtain a precursor;
[0076] 2.5 The precursor was placed in a tube furnace and calcined at 520°C for 2h, and an inert gas (Ar2) was introduced at a flow rate of 100ml / min for protection, and then cooled to obtain a carbon nitride material (CN-1) loaded with metal cobalt;
[0077] 2.6 Under the irradiation of visible light, with a fixed pressure of CO2 and 5 ml of H2O as the raw materials for the catalytic reaction, 100 mg of carbon nitride material (CN-1) as the catalyst, the yield of reducing CO2 to produce CO is 19.45 μmol / g.
[0078] Figure 2 The scanning electron microscope image of the carbon nitride material CN-1 loaded with metallic cobalt clearly shows that CN-1 is a columnar three-dimensional material (cross-sectional length dimension 10-20 μm), and the columnar body is composed of carbon nitride nanosheets (thickness <100 nm) stacked from top to bottom, with rich pore structures between and on the surface of the sheets. This structure is significantly different from that of CN-5. It is speculated that the slightly lower cobalt atomic loading failed to fully peel off the carbon nitride, resulting in too tight interlayer stacking, and the lower molar concentration of melamine and cyanuric acid made the precursor crystal size large, resulting in a larger column size, which is not conducive to the use of incident light, and thus leads to reduced photocatalytic activity.
[0079] The cobalt loading of the carbon nitride material CN-1 obtained in this example is 2.15% ( Figure 8 ). After testing, the specific surface area of the carbon nitride material CN-1 obtained in this embodiment is 136.41m 2 / g.
[0080] Example 3
[0081] 3.1 Prepare 50mmol / L aqueous solutions of melamine and cyanuric acid respectively, mix and stir equal volumes (50ml each) for 0.5h, then add HCl to adjust the pH of the mixture to 2;
[0082] 3.2 Add 100 ml of 10.0 mmol / L cobalt nitrate to the mixture and stir for 4 hours;
[0083] 3.3 The solution obtained in step 3.2 was transferred to a reactor and subjected to hydrothermal reaction at 180°C for 10 h;
[0084] 3.4 After the hydrothermal reaction is completed, the product is cooled to room temperature to obtain a crystalline product, which is then centrifuged, washed, and freeze-dried to obtain a precursor;
[0085] 3.5 The precursor was placed in a tube furnace and calcined at 520°C for 2h, and an inert gas (Ar2) was introduced at a flow rate of 100ml / min for protection, and then cooled to obtain a carbon nitride material (CN-3) loaded with metal cobalt;
[0086] 3.6 Under the irradiation of visible light, with a fixed pressure of CO2 and 5 ml of H2O as the raw materials for the catalytic reaction, 100 mg of carbon nitride material (CN-3) as the catalyst, the yield of reducing CO2 to produce CO is 36.56 μmol / g.
[0087] Figure 3 The scanning electron microscope image of the carbon nitride material CN-3 loaded with metal cobalt clearly shows that CN-3 is a three-dimensional material in the shape of a hexagonal column (cross-sectional length size 2 to 5 μm), and the column is composed of nanosheets formed by dendritic carbon nitride stacked from top to bottom, with rich pore structures between and on the surface of the sheets. Compared with CN-1, this structure has significantly more holes and tends to be a dendritic sheet structure, and the specific surface area is further increased, which is conducive to light penetration into the interior of the column, extending the light path, and thus improving the photocatalytic activity.
[0088] The cobalt loading of the carbon nitride material CN-3 obtained in this example is 6.90% ( Figure 8 ). After testing, the specific surface area of the carbon nitride material CN-3 obtained in this embodiment is 157.72m 2 / g.
[0089] Example 4
[0090] 4.1 Prepare 100mmol / L aqueous solutions of melamine and cyanuric acid respectively, mix and stir equal volumes (50ml each) for 0.5h, then add HCl to adjust the pH of the mixture to 2;
[0091] 4.2 Add 100 ml of 25 mmol / L cobalt nitrate to the mixed solution and stir for 4 hours;
[0092] 4.3 The solution obtained in step 4.2 was transferred to a reactor and subjected to hydrothermal reaction at 180°C for 20 h;
[0093] 4.4 After the hydrothermal reaction is completed, the product is cooled to room temperature to obtain a crystalline product, which is then centrifuged, washed, and freeze-dried to obtain a precursor;
[0094] 4.5 The precursor was placed in a tube furnace and calcined at 520°C for 2h, and an inert gas (Ar2) was introduced at a flow rate of 100ml / min for protection, and then cooled to obtain a carbon nitride material (CN-5A) loaded with metal cobalt;
[0095] 4.6 Under the irradiation of visible light, with a fixed pressure of CO2 and 5 ml of H2O as the raw materials for the catalytic reaction, and 100 mg of carbon nitride material (CN-5A) as the catalyst, the yield of reducing CO2 to produce CO was 48.31 μmol / g, which is close to the activity of CH-5, indicating that the hydrothermal time has little effect on the catalyst performance and is basically within the error range.
[0096] Figure 4 The scanning electron microscope image of the carbon nitride material CN-5A loaded with metal cobalt clearly shows that CN-5A is a three-dimensional polyhedral material (cross-sectional length size 2 to 5 μm), and the polyhedron is composed of stacked nanosheets formed by filamentous carbon nitride, with a diameter of 20-70nm and a length of 0.5-4.5μm. The carbon nitride material has a micro-nano multi-level structure, with rich pore structures on the surface and inside, which is conducive to the adsorption of reaction raw materials and provides active sites.
[0097] The cobalt loading of the carbon nitride material CN-5A obtained in this example is 10.79% ( Figure 8 ). After testing, the specific surface area of the carbon nitride material CN-5A obtained in this embodiment is 205.17m 2 / g.
[0098] Example 5
[0099] 5.1 Prepare 100mmol / L aqueous solutions of melamine and cyanuric acid respectively, mix and stir equal volumes (50ml each) for 0.5h, add HCl to adjust the pH of the mixture to 2, and mix and stir for 4h;
[0100] 5.2 Transfer the solution obtained in step 5.1 to a reactor and add 100 ml of deionized water. Perform hydrothermal reaction at 180°C for 10 h.
[0101] 5.3 After the hydrothermal reaction is completed, the product is cooled to room temperature to obtain a crystalline product, which is then centrifuged, washed, and freeze-dried to obtain a precursor;
[0102] 5.4 The precursor was placed in a tube furnace and calcined at 520°C for 2h, and an inert gas (Ar2) was introduced at a flow rate of 100ml / min for protection, and then cooled to obtain carbon nitride material (pCN);
[0103] 5.5 Under the irradiation of visible light, with a fixed pressure of CO2 and 5 ml of H2O as the raw materials for the catalytic reaction, and 100 mg of carbon nitride material (pCN) as the catalyst, the yield of reducing CO2 to produce CO was 17.0 μmol / g, which is much lower than the performance of cobalt-loaded carbon nitride material.
[0104] Figure 5 This is a scanning electron microscope image of the carbon nitride material pCN. It can be clearly seen that pCN is a three-dimensional material in the shape of a hollow hexagonal prism (with a cross-sectional length of 2 to 5 μm), and the column is a hollow structure with a shell at the nanoscale, indicating that the obtained carbon nitride material has a micro-nano multi-level structure.
[0105] After testing, the specific surface area of the carbon nitride material pCN obtained in this embodiment is 108.82m 2 / g.
[0106] Example 6
[0107] 6.1 Prepare 100mmol / L melamine and cyanuric acid aqueous solutions respectively, mix and stir equal volumes (50ml each) for 0.5h, then add HCl to adjust the pH of the mixture to 3;
[0108] 6.2 Add 100 ml of 25 mmol / L cobalt nitrate to the mixed solution and stir for 4 hours;
[0109] 6.3 Transfer the solution obtained in step 6.2 to a reactor and perform hydrothermal reaction at 180°C for 10 h;
[0110] 6.4 After the hydrothermal reaction is completed, the product is cooled to room temperature to obtain a crystalline product, which is then centrifuged, washed, and freeze-dried to obtain a precursor;
[0111] 6.5 The precursor was placed in a tube furnace and calcined at 520°C for 2h, and an inert gas (Ar2) was introduced at a flow rate of 100ml / min for protection. After cooling, a carbon nitride material (CN-5B) was obtained. The material was gray, which was different from the yellow color of CN-5.
[0112] 6.6 Under the irradiation of visible light, with a fixed pressure of CO2 dosage and 5ml of H2O as the raw materials for the catalytic reaction, 100mg of carbon nitride material (CN-5B) as the catalyst, the yield of reducing CO2 to generate CO was 16.67μmol / g. As the pH of the mixed solution of melamine and cyanuric acid increased, the state of the cobalt element was affected, causing it to change from an ionic state to cobalt oxide. The gray color of the carbon nitride material is formed by cobalt oxide. Cobalt oxide does not promote the electron transfer process of photocatalysis, so the photocatalytic activity of the carbon nitride material is significantly reduced.
[0113] After testing, the specific surface area of the carbon nitride material CN-5B obtained in this example is 131.33 m 2 / g.
[0114] Figure 6 XRD diagram of the carbon nitride material provided in Examples 1 and 5 of the present invention. Figure 6 It can be seen that the pCN obtained in Example 5 and the CN-5 obtained in Example 1 have the same characteristic peaks at 13.6 and 26.3°, which correspond to the diffraction peaks of the (100) and (002) crystal planes of carbon nitride, respectively, confirming that the product prepared in the examples of the present application is carbon nitride (gC3N4).
[0115] Figure 7 FTIR graph of carbon nitride materials provided in Examples 1-5 of the present invention. Figure 7 It can be seen that the carbon nitride materials prepared in Examples 1-5 have the same vibration absorption peak, which is attributed to the triazine ring structure of carbon nitride, confirming that the prepared product is carbon nitride (gC3N4).
[0116] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a multi-level porous carbon nitride material, characterized in that: include: Providing melamine aqueous solution, cyanuric acid aqueous solution and cobalt salt; Mixing the melamine aqueous solution with the cyanuric acid aqueous solution to obtain a mixed solution; The mixed solution and the cobalt salt are mixed and subjected to hydrothermal reaction to obtain a precursor; The precursor is calcined to obtain a multi-level porous carbon nitride material.
2. The preparation method according to claim 1, characterized in that: The concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution are 20-100 mmol / L respectively; and / or The cobalt salt is cobalt nitrate or cobalt chloride; and / or The concentration of the cobalt salt is 5-30 mmol / L.
3. The preparation method according to claim 1, characterized in that: The ratio of the sum of the molar concentrations of the melamine aqueous solution and the cyanuric acid aqueous solution to the molar concentration of the cobalt salt is (3-7.5):1, preferably (3-4.5):1, more preferably (3.5-4.5):1; and / or The hydrothermal reaction is carried out at 160-180° C. for 10-20 hours.
4. The preparation method according to any one of claims 1 to 3, characterized in that In the step of mixing the melamine aqueous solution with the cyanuric acid aqueous solution, the melamine aqueous solution and the cyanuric acid aqueous solution are mixed in equal volumes and at equal molar concentrations, and the mixing time is 0.5-2 hours.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The pH of the mixed solution is 1-2.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The calcination treatment is carried out in an inert atmosphere at 500-550° C. for 2-4 hours.
7. A multi-level porous carbon nitride material, characterized in that: The multi-level porous carbon nitride material is prepared by the preparation method according to any one of claims 1-6.
8. The multi-level porous carbon nitride material according to claim 7, characterized in that: The multi-level porous carbon nitride material is a micro-nanoscale material composed of stacked nanosheets formed by filamentous carbon nitride, with a specific surface area of 190-220 m 2 / g, and the diameter of the filamentous carbon nitride is 20-70nm, and the length of the filamentous carbon nitride is 0.5-4.5μm; or The multi-level porous carbon nitride material is a micro-nanoscale material formed by stacking carbon nitride nanosheets, and has a specific surface area of 130-160m 2 / g, and the thickness of the carbon nitride nanosheets is less than 100nm; or The multi-level porous carbon nitride material is a micro-nanoscale material composed of stacked nanosheets formed by dendritic carbon nitride, with a specific surface area of 150-170m 2 / g.
9. The multi-level porous carbon nitride material according to claim 7 or 8, characterized in that: The loading amount of cobalt in the multi-level porous carbon nitride material is 2.1-11.0%.
10. Use of the multi-level porous carbon nitride material prepared by the preparation method according to any one of claims 1 to 6, or the multi-level porous carbon nitride material according to claim 7 or 8 in the photocatalytic reduction of carbon dioxide to carbon monoxide.
Citation Information
Patent Citations
Transition metal doped g-C3N4 powder and preparation method thereof
CN110026219A
Transition metal carbide / graphitized carbon-like composite powder and preparation method thereof
CN110026220A
Preparation method of filamentous carbon nitride and product and application thereof
CN110170330A
Monatomic cobalt-loaded tubular carbon nitride catalyst as well as preparation method and application thereof
CN114534759A
Method for efficiently preparing melamine self-assembled supramolecular material
CN114904550A
Cited By
Low-polymerization-degree carbon nitride nanosheet containing partial supramolecular chain, preparation method of low-polymerization-degree carbon nitride nanosheet and application of low-polymerization-degree carbon nitride nanosheet in simultaneous hydrogen production and oxygen production by photocatalytic water decomposition
CN119500230A
Carbon nitride nanotube photocatalyst and preparation method thereof
CN120571624A