Selective hydrogenation catalyst as well as preparation method and application thereof
By confining platinum nanoparticles in the mesoporous core-shell structure, the small molecule H2 is brought into contact with Pt, and the large molecule phenylacetylene is isolated, which solves the problem of excessive hydrogenation of olefins in the selective hydrogenation reaction of alkynes and improves the efficiency of the catalyst selectivity and cost-effectiveness.
Patent Information
- Application Number
- CN202410875630.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult for existing catalysts to avoid excessive hydrogenation of olefins into alkanes in the selective hydrogenation reaction of alkynes, resulting in low selectivity, and the high cost of precious metal catalysts limits industrial application.
By confining platinum nanoparticles in the micropores of the mesoporous core-shell structure, the small molecule H2 is used to directly contact the active center Pt to isolate the macromolecule phenylacetylene, so that alkynes can only be added to alkenes to avoid excessive hydrogenation. , improve the selectivity of the catalyst.
The selectivity of the catalyst is improved, excessive hydrogenation of alkynes is avoided, the usage of precious metals is reduced, the production cost is reduced, and the industrial application potential of the catalyst is enhanced.
Smart Images

Figure CN118767970A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, in particular to a selective hydrogenation catalyst and a preparation method and application thereof. Background Art
[0002] Selective hydrogenation of alkynes (C≡C) to olefins (C=C) is an important industrial reaction. The hydrogenation of alkynes is a reaction that reacts by adding two hydrogen atoms to adsorbed alkyne molecules. The process consists of two consecutive steps: in the first stage, the alkynes are partially hydrogenated to the corresponding olefins, and in the second stage, the intermediate olefins are hydrogenated to alkanes in turn. Since the desired product is the intermediate olefin, the main challenge of the selective hydrogenation of alkynes is to avoid or minimize the hydrogenation of olefins to alkanes. Therefore, it is required to select a hydrogenation catalyst with the best selectivity for olefins and the highest catalytic activity.
[0003] In the prior art, the commonly used catalysts for catalyzing the hydrogenation of alkynes are catalysts supported by precious metals such as Pd, Pt, Ru, Au, and Rh, but the expensiveness of precious metal catalysts limits their application in large-scale production. Therefore, improving the selectivity of precious metal-supported catalysts for olefins is conducive to their promotion and application in industry. Summary of the invention
[0004] In view of the above problems, the present invention provides a selective hydrogenation catalyst and a preparation method and application thereof that overcome the above problems or at least partially solve the above problems. The prepared selective hydrogenation catalyst confines platinum nanoparticles that are prone to over-hydrogenation in the micropores of the mesoporous core-shell structure. The platinum nanoparticles can only contact with small molecules of H2 but not with large molecules of phenylacetylene, so that alkynes are only added to olefins, thereby avoiding over-hydrogenation of alkynes, and thus improving the selectivity of the selective hydrogenation catalyst.
[0005] Specifically, the present invention provides a method for preparing a selective hydrogenation catalyst, comprising the following steps:
[0006] S1: sodium hydroxide and 3-trimercaptopropyltrimethoxysilane are added to deionized water for hydrolysis, and then HAuCl4 is added to react to obtain solution I;
[0007] S2: dissolving hexadecyltrimethylammonium bromide solution and triethanolamine in deionized water and mixing them evenly; then adding Pt-TS-1 seed solution to react and obtain a mixed solution;
[0008] S3: adding a decahydronaphthalene solution containing tetraethyl orthosilicate to the mixed solution, reacting for 10-14 hours, washing and drying the reaction product to obtain an intermediate; dissolving the intermediate in hydrochloric acid to obtain solution II;
[0009] S4: adding the solution I to the solution II for reaction, washing, extracting, drying and calcining to obtain the selective hydrogenation catalyst.
[0010] Preferably, in step S1, the mass ratio of the sodium hydroxide, the 3-trimercaptopropyltrimethoxysilane, the deionized water and HAuCl4 is 1:(1-1.5):(10-50):(1-12);
[0011] The hydrolysis time is 20-38 min, and the reaction time is 20-40 min.
[0012] Preferably, in step S2, the volume ratio of the triethanolamine, the hexadecyltrimethylammonium bromide solution, the deionized water and the Pt-TS-1 seed solution is 1:(120-180):(100-150):(28-36);
[0013] The mass fraction of cetyltrimethylammonium bromide in the cetyltrimethylammonium bromide solution is 20-30wt%;
[0014] The reaction conditions include: ultrasonic mixing for 10-20 min, and stirring for 50-80 min.
[0015] Preferably, in step S3, the volume ratio of the decalin solution to the second mixed solution is 1:(2-3);
[0016] The volume percentage of tetraethyl orthosilicate in the decalin solution is 20 v / v%;
[0017] The reaction conditions include: reaction temperature of 55-65°C, stirring speed of 120-180rpm, and reaction time of 10-14h;
[0018] The drying process includes: a drying temperature of 90-110° C. and a drying time of 10-14 hours.
[0019] Preferably, in step S3, the dissolving comprises: adding 0.8-1.3 g of the intermediate into 60-80 ml of hydrochloric acid, ultrasonicating for 8-15 min, and stirring for 20-40 min; wherein the concentration of the hydrochloric acid is 2 mol / L.
[0020] Preferably, in step S4, the reaction comprises: stirring at 40-48°C for 50-75 min, and then refluxing at 110-125°C for 5-7 h;
[0021] The washing comprises centrifugal washing with deionized water and / or ethanol;
[0022] The extraction agent of the extraction is ethanol;
[0023] The calcination time is 110-125 minutes, and the calcination temperature is 320-360°C.
[0024] Preferably, the Pt-TS-1 seed solution is prepared by the following method:
[0025] TS-1 zeolite is used as a seed, tetrapropylammonium hydroxide is used as a structure directing agent to etch and crystallize mesoporous zeolite particles, and Pt is deposited in the mesopores of the mesoporous zeolite particles to obtain Pt-TS-1 seed crystals; the Pt-TS-1 seed crystals are dispersed in deionized water to obtain the Pt-TS-1 seed crystal solution.
[0026] The present invention provides a selective hydrogenation catalyst prepared according to any one of the preparation methods described above.
[0027] Preferably, the loading amount of Au in the selective hydrogenation catalyst is 0.0-1.0 wt%.
[0028] The invention provides an application of a selective hydrogenation catalyst in the selective hydrogenation reaction of alkynes.
[0029] The beneficial effects of the present invention are:
[0030] In the selective hydrogenation catalyst provided by the present invention, since the platinum nanoparticles that are prone to over-hydrogenation are confined in the micropores of the mesoporous core-shell structure, small molecules H2 can freely enter and exit the micropores, can directly contact the active center Pt, and dissociate into hydrogen atoms; while the large molecule phenylacetylene is isolated outside the TS-1 crystal nucleus due to the micropore channel effect, and is difficult to directly contact the active center Pt, so that alkynes are only added to olefins, thereby avoiding over-hydrogenation of alkynes, thereby improving the selectivity of this series of catalysts.
[0031] Based on the following detailed description of specific embodiments of the present invention in conjunction with the accompanying drawings, those skilled in the art will become more aware of the above and other objects, advantages and features of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a schematic model diagram of a selective hydrogenation catalyst;
[0033] Figure 2 is a TEM image of a selective hydrogenation catalyst in an embodiment of the present invention;
[0034] Figure 3 CO-TPD spectra of selected hydrogenation catalysts in the embodiments of the present invention;
[0035] Figure 4 The pore size distribution diagram of the selected hydrogenation catalyst in the embodiment of the present invention;
[0036] Figure 5The relationship between the conversion rate of phenylacetylene and the reaction time under different catalysts;
[0037] Figure 6 The relationship between the yield of styrene and the reaction time under different catalysts;
[0038] Figure 7 TPD spectra of selected hydrogenation catalysts in the examples of the present invention. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is described in detail below in conjunction with specific embodiments and experimental data. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0040] Unless otherwise specified, the raw materials, reagents and equipment involved in the embodiments of the present invention can be obtained through commercial channels.
[0041] The present invention provides a method for preparing a selective hydrogenation catalyst, comprising the following steps:
[0042] S1: sodium hydroxide and 3-trimercaptopropyltrimethoxysilane are added to deionized water for hydrolysis, and then HAuCl4 is added to react to obtain solution I;
[0043] S2: dissolving hexadecyltrimethylammonium bromide solution and triethanolamine in deionized water and mixing them evenly; then adding Pt-TS-1 seed solution to react and obtain a mixed solution;
[0044] S3: adding a decahydronaphthalene solution containing tetraethyl orthosilicate to the mixed solution and reacting for 10-14 hours, washing and drying the reaction product to obtain an intermediate; dissolving the intermediate in hydrochloric acid to obtain solution II;
[0045] S4: adding solution I into solution II for reaction, washing, extracting, drying and calcining to obtain a selective hydrogenation catalyst.
[0046] The present invention confines platinum nanoparticles that are prone to over-hydrogenation in the micropores of the mesoporous core-shell structure, so that small molecules H2 can freely enter and exit the micropores, can directly contact the active center Pt, and dissociate into hydrogen atoms; while the large molecule phenylacetylene is isolated outside the TS-1 crystal nucleus due to the micropore channel effect, and is difficult to directly contact the active center Pt, so that alkynes are only added to olefins, thereby avoiding over-hydrogenation of alkynes, and thus improving the selectivity of the series of catalysts.
[0047] In step S1 of the present invention, the mass ratio of sodium hydroxide, 3-trimercaptopropyltrimethoxysilane, deionized water and HAuCl4 is 1:(1-1.5):(10-50):(1-12). The hydrolysis time is 20-38 minutes, and the reaction time is 20-40 minutes.
[0048] In step S2, the volume ratio of triethanolamine, hexadecyltrimethylammonium bromide solution, deionized water and Pt-TS-1 seed solution is 1:(120-180):(100-150):(28-36). The mass fraction of hexadecyltrimethylammonium bromide in the hexadecyltrimethylammonium bromide solution is 20-30wt%. The reaction conditions include: ultrasonic mixing for 10-20min and stirring for 50-80min.
[0049] In step S3, the volume ratio of the decahydronaphthalene solution to the second mixed solution is 1:(2-3). The volume percentage of tetraethyl orthosilicate in the decahydronaphthalene solution is 20v / v%. The reaction conditions include: the reaction temperature is 55-65°C, the stirring speed is 120-180rpm, and the reaction time is 10-14h. Drying includes: the drying temperature is 90-110°C, and the drying time is 10-14h. Dissolving includes: adding 0.8-1.3g of the intermediate to 60-80ml of hydrochloric acid, ultrasonicating for 8-15min, and stirring for 20-40min; wherein the concentration of hydrochloric acid is 2mol / L.
[0050] In step S4, the reaction includes: stirring at 40-48°C for 50-75 minutes, and then refluxing at 110-125°C for 5-7 hours. Washing includes centrifugal washing with deionized water and / or ethanol. The extractant for extraction is ethanol. The roasting time for roasting is 110-125 minutes, and the roasting temperature is 320-360°C.
[0051] The Pt-TS-1 seed solution in the present invention is prepared by the following method:
[0052] Using TS-1 zeolite as a seed and tetrapropylammonium hydroxide as a structure directing agent, mesoporous zeolite particles are etched and crystallized to synthesize, and Pt is deposited in the mesopores of the mesoporous zeolite particles to obtain Pt-TS-1 seed crystals; the Pt-TS-1 seed crystals are dispersed in deionized water to obtain a Pt-TS-1 seed crystal solution.
[0053] The present invention provides a preparation method of the above technical solution to prepare a selective hydrogenation catalyst.
[0054] The present invention provides application of the selective hydrogenation catalyst of the above technical solution in the selective hydrogenation reaction of alkynes.
[0055] The selective hydrogenation catalyst provided by the present invention and its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0056] Example 1
[0057] 46.72 g of 25 wt% tetrapropylammonium hydroxide solution and 8.68 g of deionized water were stirred and mixed in an ice-water bath, and then 40 g of tetraethyl orthosilicate and 2.64 g of tetrabutyl titanate were added and stirred until the tetraethyl orthosilicate and tetrabutyl titanate were completely hydrolyzed. Then, the mixture was transferred to a 70°C water bath, 48 g of isopropanol was slowly added dropwise, and stirring was continued for 1 hour. The resulting mixed solution was used as the first solution.
[0058] 0.1 g of sodium hydroxide and 0.12 g of 3-trimercaptopropyltrimethoxysilane were dissolved in 2.0 g of deionized water, and hydrolyzed for 20 min. Then 6.16 mL of H2PtCl6 (100 mM) was added dropwise, and stirring was continued for 20 min. The resulting mixed solution was used as the second solution.
[0059] The second solution was slowly added dropwise to the first solution, and the mixture was stirred in a 70°C water bath for 30 min. The resulting solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene and placed in a timed oven for crystallization at 170°C for 24 h to obtain a Pt-TS-1 nanocrystal solution. The Pt-TS-1 nanocrystals were centrifugally washed five times with deionized water and dispersed in 45 mL of deionized water to obtain a Pt-TS-1 seed solution.
[0060] 24 mL of hexadecyltrimethylammonium bromide solution (25 wt%), 0.18 g of triethanolamine and 20 mL of deionized water were fully mixed in a 100 mL round-bottom flask; then slowly stirred for 30 min in a 60°C oil bath (stirring speed was maintained at 150 rpm). After ultrasonic dispersion of the Pt-TS-1 seed solution for 1 h, 5 ml was slowly added dropwise to the round-bottom flask, and then the round-bottom flask was ultrasonicated for 15 min and stirred for 60 min.
[0061] Use a glass rod to slowly introduce 22 ml of decahydronaphthalene solution containing tetraethyl orthosilicate (the volume percentage of tetraethyl orthosilicate is 20 v / v%) into the round-bottom flask. The bottom of the glass rod is flush with the liquid level in the flask. The whole process is controlled between 30-60 seconds. Then continue the reaction at 60°C and 150 rpm for 12 hours. After the reaction is completed, the reaction product is centrifuged and washed five times with deionized water, and dried in a vacuum drying oven at 100°C for 12 hours to obtain an intermediate. Add 1 g of the dried intermediate powder and 70 ml of hydrochloric acid (2 mol / L) to a round-bottom flask, ultrasonicate for 10 minutes, and stir for 30 minutes to obtain solution II.
[0062] 0.16 g of sodium hydroxide and 0.2 g of 3-trimercaptopropyltrimethoxysilane were dissolved in 4.0 g of deionized water, hydrolyzed for 30 min, and then 0.1 ml of HAuCl4 was added dropwise, and stirring was continued for 30 min to obtain Solution I.
[0063] Solution I was added dropwise to solution II under stirring, stirred in a 45°C oil bath for 1 h, and then the mixture was heated to 120°C and refluxed for 6 h. Finally, the obtained sample was washed with deionized water and ethanol by centrifugation, extracted with ethanol three times, dried, and calcined at 350°C for 2 h to obtain a selective hydrogenation catalyst; recorded as Pt-Au / TDMSN (Au: 0.2wt%) catalyst.
[0064] Example 2
[0065] 46.72 g of 25 wt% tetrapropylammonium hydroxide solution and 8.68 g of deionized water were stirred and mixed in an ice-water bath, and then 40 g of tetraethyl orthosilicate and 2.64 g of tetrabutyl titanate were added and stirred until the tetraethyl orthosilicate and tetrabutyl titanate were completely hydrolyzed. Then, the mixture was transferred to a 70°C water bath, 48 g of isopropanol was slowly added dropwise, and stirring was continued for 1 hour. The resulting mixed solution was used as the first solution.
[0066] 0.1 g of sodium hydroxide and 0.12 g of 3-trimercaptopropyltrimethoxysilane were dissolved in 2.0 g of deionized water, and hydrolyzed for 20 min. Then 6.16 mL of H2PtCl6 (100 mM) was added dropwise, and stirring was continued for 20 min. The resulting mixed solution was used as the second solution.
[0067] The second solution was slowly added dropwise to the first solution, and the mixture was stirred in a 70°C water bath for 30 min. The resulting solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene and placed in a timed oven for crystallization at 170°C for 24 h to obtain a Pt-TS-1 nanocrystal solution. The Pt-TS-1 nanocrystals were centrifugally washed five times with deionized water and dispersed in 45 mL of deionized water to obtain a Pt-TS-1 seed solution.
[0068] 24 mL of hexadecyltrimethylammonium bromide solution (25 wt%), 0.18 g of triethanolamine and 20 mL of deionized water were fully mixed in a 100 mL round-bottom flask; then slowly stirred for 30 min in a 60°C oil bath (stirring speed was maintained at 150 rpm). After ultrasonic dispersion of the Pt-TS-1 seed solution for 1 h, 5 ml was slowly added dropwise to the round-bottom flask, and then the round-bottom flask was ultrasonicated for 15 min and stirred for 60 min.
[0069] Use a glass rod to slowly introduce 22 ml of decahydronaphthalene solution containing tetraethyl orthosilicate (the volume percentage of tetraethyl orthosilicate is 20 v / v%) into the round-bottom flask. The bottom of the glass rod is flush with the liquid level in the flask. The whole process is controlled between 30-60 seconds. Then continue the reaction at 60°C and 150 rpm for 12 hours. After the reaction is completed, the reaction product is centrifuged and washed five times with deionized water, and dried in a vacuum drying oven at 100°C for 12 hours to obtain an intermediate. Add 1 g of the dried intermediate powder and 70 ml of hydrochloric acid (2 mol / L) to a round-bottom flask, ultrasonicate for 10 minutes, and stir for 30 minutes to obtain solution II.
[0070] 0.16 g of sodium hydroxide and 0.2 g of 3-trimercaptopropyltrimethoxysilane were dissolved in 4.0 g of deionized water, hydrolyzed for 30 min, and then 0.3 ml of HAuCl4 was added dropwise, and stirring was continued for 30 min to obtain Solution I.
[0071] Solution I was added dropwise to solution II under stirring, stirred in a 45°C oil bath for 1 h, and then the mixture was heated to 120°C and refluxed for 6 h. Finally, the obtained sample was washed with deionized water and ethanol by centrifugation, extracted with ethanol three times, dried, and calcined at 350°C for 2 h to obtain a selective hydrogenation catalyst; recorded as Pt-Au / TDMSN (Au: 0.6wt%) catalyst.
[0072] Example 3
[0073] 46.72 g of 25 wt% tetrapropylammonium hydroxide solution and 8.68 g of deionized water were stirred and mixed in an ice-water bath, and then 40 g of tetraethyl orthosilicate and 2.64 g of tetrabutyl titanate were added and stirred until the tetraethyl orthosilicate and tetrabutyl titanate were completely hydrolyzed. Then, the mixture was transferred to a 70°C water bath, 48 g of isopropanol was slowly added dropwise, and stirring was continued for 1 hour. The resulting mixed solution was used as the first solution.
[0074] 0.1 g of sodium hydroxide and 0.12 g of 3-trimercaptopropyltrimethoxysilane were dissolved in 2.0 g of deionized water, and hydrolyzed for 20 min. Then 6.16 mL of H2PtCl6 (100 mM) was added dropwise, and stirring was continued for 20 min. The resulting mixed solution was used as the second solution.
[0075] The second solution was slowly added dropwise to the first solution, and the mixture was stirred in a 70°C water bath for 30 min. The resulting solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene and placed in a timed oven for crystallization at 170°C for 24 h to obtain a Pt-TS-1 nanocrystal solution. The Pt-TS-1 nanocrystals were centrifugally washed five times with deionized water and dispersed in 45 mL of deionized water to obtain a Pt-TS-1 seed solution.
[0076] 24 mL of hexadecyltrimethylammonium bromide solution (25 wt%), 0.18 g of triethanolamine and 20 mL of deionized water were fully mixed in a 100 mL round-bottom flask; then slowly stirred for 30 min in a 60°C oil bath (stirring speed was maintained at 150 rpm). After ultrasonic dispersion of the Pt-TS-1 seed solution for 1 h, 5 ml was slowly added dropwise to the round-bottom flask, and then the round-bottom flask was ultrasonicated for 15 min and stirred for 60 min.
[0077] Use a glass rod to slowly introduce 22 ml of decahydronaphthalene solution containing tetraethyl orthosilicate (the volume percentage of tetraethyl orthosilicate is 20 v / v%) into the round-bottom flask. The bottom of the glass rod is flush with the liquid level in the flask. The whole process is controlled between 30-60 seconds. Then continue the reaction at 60°C and 150 rpm for 12 hours. After the reaction is completed, the reaction product is centrifuged and washed five times with deionized water, and dried in a vacuum drying oven at 100°C for 12 hours to obtain an intermediate. Add 1 g of the dried intermediate powder and 70 ml of hydrochloric acid (2 mol / L) to a round-bottom flask, ultrasonicate for 10 minutes, and stir for 30 minutes to obtain solution II.
[0078] 0.16 g of sodium hydroxide and 0.2 g of 3-trimercaptopropyltrimethoxysilane were dissolved in 4.0 g of deionized water, hydrolyzed for 30 min, and then 0.5 ml of HAuCl4 was added dropwise, and stirring was continued for 30 min to obtain Solution I.
[0079] Solution I was added dropwise to solution II under stirring, stirred in a 45°C oil bath for 1 h, and then the mixture was heated to 120°C and refluxed for 6 h. Finally, the obtained sample was washed with deionized water and ethanol by centrifugation, extracted with ethanol three times, dried, and calcined at 350°C for 2 h to obtain a selective hydrogenation catalyst; recorded as Pt-Au / TDMSN (Au: 1.0wt%) catalyst.
[0080] Example 4
[0081] 46.72 g of 25 wt% tetrapropylammonium hydroxide solution and 8.68 g of deionized water were stirred and mixed in an ice-water bath, and then 40 g of tetraethyl orthosilicate and 2.64 g of tetrabutyl titanate were added and stirred until the tetraethyl orthosilicate and tetrabutyl titanate were completely hydrolyzed. Then, the mixture was transferred to a 70°C water bath, 48 g of isopropanol was slowly added dropwise, and stirring was continued for 1 hour. The resulting mixed solution was used as the first solution.
[0082] 0.1 g of sodium hydroxide and 0.12 g of 3-trimercaptopropyltrimethoxysilane were dissolved in 2.0 g of deionized water, and hydrolyzed for 20 min. Then 6.16 mL of H2PtCl6 (100 mM) was added dropwise, and stirring was continued for 20 min. The resulting mixed solution was used as the second solution.
[0083] The second solution was slowly added dropwise to the first solution, and the mixture was stirred in a 70°C water bath for 30 min. The resulting solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene and placed in a timed oven for crystallization at 170°C for 24 h to obtain a Pt-TS-1 nanocrystal solution. The Pt-TS-1 nanocrystals were centrifugally washed five times with deionized water and dispersed in 45 mL of deionized water to obtain a Pt-TS-1 seed solution.
[0084] 24 mL of hexadecyltrimethylammonium bromide solution (25 wt%), 0.18 g of triethanolamine and 20 mL of deionized water were fully mixed in a 100 mL round-bottom flask; then slowly stirred for 30 min in a 60°C oil bath (stirring speed was maintained at 150 rpm). After ultrasonic dispersion of the Pt-TS-1 seed solution for 1 h, 5 ml was slowly added dropwise to the round-bottom flask, and then the round-bottom flask was ultrasonicated for 15 min and stirred for 60 min.
[0085] Use a glass rod to slowly introduce 22 ml of decahydronaphthalene solution containing tetraethyl orthosilicate (the volume percentage of tetraethyl orthosilicate is 20 v / v%) into the round-bottom flask. The bottom of the glass rod is flush with the liquid level in the flask. The whole process is controlled between 30-60 seconds. Then continue the reaction at 60°C and 150 rpm for 12 hours. After the reaction is completed, the reaction product is centrifuged and washed five times with deionized water, and dried in a vacuum drying oven at 100°C for 12 hours to obtain an intermediate. Add 1 g of the dried intermediate powder and 70 ml of hydrochloric acid (2 mol / L) to a round-bottom flask, ultrasonicate for 10 minutes, and stir for 30 minutes to obtain solution II.
[0086] 0.16 g of sodium hydroxide and 0.2 g of 3-trimercaptopropyltrimethoxysilane were dissolved in 4.0 g of deionized water, hydrolyzed for 30 min, and stirred for another 30 min to obtain Solution I.
[0087] Solution I was added dropwise to solution II under stirring, stirred in a 45°C oil bath for 1 h, and then the mixture was heated to 120°C and refluxed for 6 h. Finally, the obtained sample was washed with deionized water and ethanol by centrifugation, extracted with ethanol three times, dried, and calcined at 350°C for 2 h to obtain the Pt / TDMSN catalyst.
[0088] The following analyses were performed on the Pt-Au / TDMSN (Au: 0.2 wt%) catalyst prepared in Example 1, the Pt-Au / TDMSN (Au: 0.6 wt%) catalyst prepared in Example 2, the Pt-Au / TDMSN (Au: 1.0 wt%) catalyst prepared in Example 3, and the Pt / TDMSN catalyst prepared in Example 4:
[0089] 1. Sample morphology
[0090] The morphology of the samples was characterized by projection electron microscopy (TEM, JEM 2100), scanning electron microscopy (SEM, SU8010) and high-resolution TEM (FEI Tecnai G2 F20).
[0091] Figure 1 is a schematic model diagram of a selective hydrogenation catalyst; Figure 2 are TEM images of each catalyst; among them, a1-a3 are TEM images of Pt / TDMSN catalysts at different sizes; b1-b3 are TEM images of Pt-Au / TDMSN (Au: 0.2wt%) catalysts at different sizes; c1-c3 are TEM images of Pt-Au / TDMSN (Au: 0.6wt%) catalysts at different sizes; d1-d3 are TEM images of Pt-Au / TDMSN (Au: 1.0wt%) catalysts at different sizes.
[0092] like Figure 2 As shown, each catalyst is monodisperse elliptical or cubic, and presents a monodisperse, uniform 3D dendritic channel structure with Pt / TS-1 molecular sieve as the core and central-radial mesoporous channels. No individual Pt / TS-1 independent crystals were observed in the figure. All Pt / TS-1 crystals were uniformly wrapped by dendritic mesoporous silica. The average particle size of each Pt-Au / TDMSN catalyst and Pt / TDMSN catalyst was 155nm, and the average shell thickness was 30nm. This shows that the Pt / TS-1 crystals are perfectly embedded in the DMSN framework, forming a Figure 1 The same core-shell structure catalyst with mesoporous micropores.
[0093] Moreover, since acid treatment was used in the Au loading operation, the outer surface of the Pt / TS-1 crystal in the catalyst was tightly connected to the junction of the mesoporous silica, and the entire mesoporous silica layer was compact and the mesopores were regular.
[0094] 2. Pore structure of catalyst
[0095] Each catalyst was heated at 10 °C min -1 The temperature was raised to 120℃ for 1h and then cooled to room temperature. N2 was converted to CO and then kept at room temperature for 1h for CO adsorption. High-purity N2 was purged at the same temperature for 1h to remove the weakly adsorbed CO. The temperature was raised to 700℃ (10℃min -1 ) to obtain the CO-TPD curve. The CO-TPD curves of each catalyst are sorted in Figure 3 middle.
[0096] The specific surface area and pore size of the catalysts prepared in Examples 1-3 and Example 4 were analyzed using Micromeritics Tristar II 3020 at a temperature of 77 K, and the relevant data are summarized in Tables 1 and Figure 4 middle.
[0097] like Figure 3 As shown in Figure 1, each catalyst exhibits similar adsorption curves at low relative pressure (P / P0 = 0.8-1.0), all with H3-type hysteresis loops and IV-type isotherms, which are signs of mesoporous structures. Figure 4 As shown, each catalyst has two peaks at 6nm and 20nm; combined with Table 1, the average mesopore size of the catalysts prepared in Examples 1-3 and Example 4 is 11nm, with similar specific surface area and micropore volume, indicating that the precious metal Au did not enter or block the micropores after introduction.
[0098] Table 1 Structural characteristics of catalysts
[0099]
[0100] 3. Catalytic performance test
[0101] Under the same conditions, the Pt-Au / TDMSN (Au: 0.2wt%) catalyst prepared in Example 1, the Pt-Au / TDMSN (Au: 0.6wt%) catalyst prepared in Example 2, the Pt-Au / TDMSN (Au: 1.0wt%) catalyst prepared in Example 3 and the Pt / TDMSN catalyst prepared in Example 4 were used as catalysts for the selective hydrogenation of phenylacetylene.
[0102] The steps of the selective hydrogenation reaction of phenylacetylene are as follows: 1.18mmol phenylacetylene, 20mg catalyst and 15ml ethanol are added to a 25ml stainless steel hydrogenation reactor. After the hydrogenation reactor is cleaned with H2 (99.9999%) three times, the H2 is pressurized to 3MPa, and the temperature is quickly raised to the required temperature (20-60°C), and the reaction is kept warm for 120min. The timing starts from 0min of the reaction, and samples are taken every 20min, and a total of 6 samples are taken until the end of the reaction. After the reaction is completed, the reactor is cooled, and the 6 liquid products are extracted by centrifugation, and the products are analyzed using a gas chromatography-mass spectrometer (GCMS-QP2020 equipped with an SH-Rxi-5Sil MS column).
[0103] The hydrogenation reaction process of phenylacetylene and the calculation formulas of reactant conversion rate, product selectivity and product yield are as follows:
[0104]
[0105] Conversion1, Selectivity1 and Yield1 represent PA conversion, PE (or PT) selectivity and PE (or PT) yield, respectively. nPA, nPE and nPT represent the molar numbers of phenylacetylene (PA), styrene (PE) and phenylethane (PT), respectively.
[0106] Figure 5 The relationship between the conversion rate of phenylacetylene and the reaction time under different catalysts is shown in Figure 2. Figure 6 This is a graph showing the relationship between the yield of styrene and reaction time under different catalysts.
[0107] like Figure 5 As shown in the figure, under the action of different catalysts, the conversion rate of each catalytic system increases with the increase of reaction time, which is in line with the general law of catalytic reaction. The conversion rate of each catalytic system reached more than 80% after 120 minutes of reaction; among them, the catalytic activity order in the hydrogenation reaction of phenylacetylene is: Pt-Au / TDMSN (Au: 1.0wt%) catalyst>Pt-Au / TDMSN (Au: 0.6wt%)>Pt-Au / TDMSN (Au: 0.2wt%) catalyst>Pt / TDMSN catalyst. This shows that Au plays a synergistic role in hydrogenation to a certain extent.
[0108] like Figure 6 As shown, Pt / TDMSN and Pt-Au / TDMSN series catalysts have similar selectivity. In order to explore the selectivity of Pt / TDMSN and Pt-Au / TDMSN series catalysts, adsorption and desorption experiments were performed again:
[0109] Taking the Pt-Au / TDMSN (Au: 0.6 wt%) catalyst prepared in Example 2 and the Pt / TDMSN catalyst prepared in Example 4 as examples, the adsorption capacity of the catalysts for CO, H2 and PA (PA: phenylacetylene) was measured.
[0110] Each catalyst was heated at 10 °C min -1 The temperature was raised to 120℃ for 1h and then cooled to room temperature. N2 was converted to CO and then kept at room temperature for 1h for CO adsorption. High-purity N2 was purged at the same temperature for 1h to remove the weakly adsorbed CO. The temperature was raised to 700℃ (10℃min -1 ) to obtain the CO-TPD curve. The test methods of PA-TPD and H2-TPD are similar to those of CO-TPD. The CO-TPD curve, H2-TPD curve, and PA-TPD curve of each catalyst are sorted in Figure 7 middle.
[0111] Figure 7In the figure, a is the CO-TPD spectrum of Pt-Au / TDMSN (Au: 0.6wt%) catalyst and Pt / TDMSN catalyst; b is the H2-TPD spectrum of Pt-Au / TDMSN (Au: 0.6wt%) catalyst and Pt / TDMSN catalyst; c is the H2-TPD spectrum of Pt-Au / TDMSN (Au: 0.6wt%) catalyst and Pt / TDMSN catalyst.
[0112] like Figure 7 As shown in Figure 2a, the CO-TPD curves of both catalysts have a weak desorption peak at around 570°C, which is due to the adsorption of CO molecules by Pt, where the kinetic diameter of CO is 0.376nm. Figure 7 -b, there is a very strong Pt desorption peak for H2 molecules at around 450-550℃, and the intensities of the two catalyst peaks are not much different, which proves that H2 molecules can enter the microporous channels and adsorb on Pt. Combined with the CO-TPD results, it is verified that the micropore size of the TDMSN core-shell structure TS-1 crystal core is mainly distributed between 0.2nm and 0.376nm. Figure 7 -c shows the desorption of phenylacetylene (PA) on the catalyst surface. In the prior art, there is a desorption peak of Pt for phenylacetylene molecules at around 550°C. Compared with the prior art, no desorption peak was detected at this temperature for Pt / TDMSN catalyst and Pt-Au / TDMSN (Au: 0.6wt%) catalyst. On the contrary, a desorption peak was detected in the range of 100-200°C. It can be inferred that the microporous structure of the TS-1 crystal nucleus of the selective hydrogenation catalyst almost completely isolates the contact between phenylacetylene molecules and Pt, so that phenylacetylene cannot be adsorbed by Pt in the micropores.
[0113] Based on the above data, it can be seen that the selective hydrogenation catalyst of the present invention successfully confines the precious metal Pt in the micropores of the mesoporous core-shell structure, and the small molecule H2 can freely enter and exit the micropores, and can directly contact the active center Pt to dissociate into hydrogen atoms; while the large molecule phenylacetylene is isolated outside the TS-1 crystal nucleus due to the micropore channel effect, and it is difficult to directly contact the active center Pt, so that the alkyne is only added to olefins, thereby avoiding excessive hydrogenation of the alkyne, and thus improving the selectivity of this series of catalysts.
[0114] The above are only preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a selective hydrogenation catalyst, characterized in that: The following steps are involved: S1: sodium hydroxide and 3-trimercaptopropyltrimethoxysilane are added to deionized water for hydrolysis, and then HAuCl4 is added to react to obtain solution I; S2: dissolving hexadecyltrimethylammonium bromide solution and triethanolamine in deionized water and mixing them evenly; then adding Pt-TS-1 seed solution to react and obtain a mixed solution; S3: adding a decahydronaphthalene solution containing tetraethyl orthosilicate to the mixed solution, reacting for 10-14 hours, washing and drying the reaction product to obtain an intermediate; Dissolving the intermediate in hydrochloric acid to obtain solution II; S4: adding the solution I to the solution II for reaction, washing, extracting, drying and calcining to obtain the selective hydrogenation catalyst.
2. The method for preparing a selective hydrogenation catalyst according to claim 1, characterized in that: In step S1, the mass ratio of the sodium hydroxide, the 3-trimercaptopropyltrimethoxysilane, the deionized water and HAuCl4 is 1:(1-1.5):(10-50):(1-12); The hydrolysis time is 20-38 min, and the reaction time is 20-40 min.
3. The method for preparing the selective hydrogenation catalyst according to claim 1, characterized in that: In step S2, the volume ratio of the triethanolamine, the hexadecyltrimethylammonium bromide solution, the deionized water and the Pt-TS-1 seed solution is 1:(120-180):(100-150):(28-36); The mass fraction of cetyltrimethylammonium bromide in the cetyltrimethylammonium bromide solution is 20-30wt%; The reaction conditions include: ultrasonic mixing for 10-20 min, and stirring for 50-80 min.
4. The method for preparing a selective hydrogenation catalyst according to claim 1, characterized in that: In step S3, the volume ratio of the decalin solution to the second mixed solution is 1:(2-3); The volume percentage of tetraethyl orthosilicate in the decahydronaphthalene solution is 20 v / v%; The reaction conditions include: reaction temperature of 55-65°C, stirring speed of 120-180rpm, and reaction time of 10-14h; The drying process includes: a drying temperature of 90-110° C. and a drying time of 10-14 hours.
5. The method for preparing a selective hydrogenation catalyst according to claim 1, characterized in that: In step S3, the dissolving comprises: adding 0.8-1.3 g of the intermediate into 60-80 ml of hydrochloric acid, ultrasonicating for 8-15 min, and stirring for 20-40 min; wherein the concentration of the hydrochloric acid is 2 mol / L.
6. The method for preparing a selective hydrogenation catalyst according to claim 1, characterized in that: In step S4, the reaction comprises: stirring at 40-48° C. for 50-75 min, and then refluxing at 110-125° C. for 5-7 h; The washing comprises centrifugal washing with deionized water and / or ethanol; The extraction agent of the extraction is ethanol; The calcination time is 110-125 minutes, and the calcination temperature is 320-360°C.
7. The method for preparing a selective hydrogenation catalyst according to claim 1, characterized in that: The Pt-TS-1 seed solution was prepared by the following method: TS-1 zeolite is used as a seed, tetrapropylammonium hydroxide is used as a structure directing agent to etch and crystallize mesoporous zeolite particles, and Pt is deposited in the mesopores of the mesoporous zeolite particles to obtain Pt-TS-1 seed crystals; the Pt-TS-1 seed crystals are dispersed in deionized water to obtain the Pt-TS-1 seed crystal solution.
8. A selective hydrogenation catalyst, characterized in that The selective hydrogenation catalyst is prepared according to the method for preparing the selective hydrogenation catalyst according to any one of claims 1 to 7.
9. The selective hydrogenation catalyst according to claim 1, characterized in that The loading amount of Au in the selective hydrogenation catalyst is 0-1.0 wt %.
10. Use of the selective hydrogenation catalyst according to claim 8 in the selective hydrogenation reaction of alkynes.
Citation Information
Patent Citations
Hydrotalcite-loaded palladium catalyst for preparing styrene through selective hydrogenation of phenylacetylene and preparation method thereof and application
CN111054333A
Metal oxide modified platinum-based catalyst, preparation method and application
CN118179588A
Cited By
Mesomicroporous core-shell molecular sieve series beta zeolite catalyst and preparation method and application thereof
CN120790222A
Mesoporous core-shell molecular sieve tandem β-zeolite catalysts, their preparation methods and applications
CN120790222B