Catalytic oxidation catalyst coated with silicon carbide carrier as well as preparation method and application of catalytic oxidation catalyst

By coating zirconium-aluminum composite oxide, molecular sieve, manganese oxide and other materials on the silicon carbide carrier, the thermal conductivity efficiency and heat resistance of the catalyst are improved, and the problem of untimely heat conduction in VOCs treatment in the existing technology is solved. Efficient and stable catalytic oxidation effect is achieved.

CN118767977APending Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310372147.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing catalytic oxidation treatment technology for VOCs, the reaction process releases a large amount of heat and the heat is not transferred in time, resulting in local temperature rise and poor catalyst activity.

Method used

The catalytic oxidation catalyst is coated with silicon carbide carrier. The coating contains zirconium-aluminum composite oxide, molecular sieve, manganese oxide and active precious metal components. The thermal conductivity efficiency, heat resistance and low-temperature ignition of the catalyst are improved through a specific preparation method. active.

Benefits of technology

The catalyst achieves high conversion efficiency, thermal stability and low ignition temperature, is suitable for the removal of various types of VOCs, and improves treatment efficiency and safety.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of catalytic oxidation catalysts, and discloses a silicon carbide carrier coated catalytic oxidation catalyst as well as a preparation method and application thereof. The catalytic oxidation catalyst coated with the silicon carbide carrier comprises the silicon carbide carrier and a coating coated on the silicon carbide carrier, the coating contains zirconium-aluminum composite oxide, a molecular sieve, manganese oxide and active noble metal components, the total coating amount of the coating is 60-180g / L, and the noble metal loading amount is 0.2-2g / L. The catalytic oxidation catalyst provided by the invention has the advantages of low initiation temperature, high conversion efficiency, good thermal stability and the like, and is suitable for removal of various VOCs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalytic oxidation catalyst preparation, and in particular to a catalytic oxidation catalyst coated with a silicon carbide carrier, and a preparation method and application thereof. Background Art

[0002] At present, the widely used methods for treating volatile organic compounds (VOCs) mainly include adsorption, condensation, thermal combustion and catalytic oxidation. Catalytic oxidation has many advantages such as high treatment efficiency, less secondary pollution and high safety factor. Therefore, whether from the perspective of economy or environmental protection, catalytic oxidation technology has become one of the most commonly used methods for controlling VOCs pollution. The core of catalytic oxidation technology is reflected in the performance of the catalyst, which directly determines the efficiency of VOCs removal. According to the different active components, catalysts can be divided into two categories: precious metal catalysts and non-precious metal catalysts. Generally speaking, compared with non-precious metal catalysts, precious metal catalysts show higher VOCs treatment activity, better selectivity and longer service life, and the loading amount of active components is relatively lower. Typical precious metal active components mainly include gold, silver and platinum group metals (Pt, Pd, Rh, Ru, etc.), among which precious metal catalysts loaded with Pt and Pd have been industrialized.

[0003] The catalyst used in industry is composed of a carrier and a coating applied on the carrier. The carrier is mostly made of cordierite ceramics, and some use iron-chromium-aluminum metal carriers, mullite carriers, silicon carbide (SiC) carriers, etc. The material of the carrier determines the characteristics of the carrier. For example, although the thermal conductivity of the iron-chromium-aluminum metal carrier is good, the firmness of its bonding with the coating is low; the thermal conductivity of the cordierite ceramic carrier is slightly lower, but it has better coating bonding, a lower thermal expansion coefficient and a higher safety factor.

[0004] Compared with cordierite, SiC has better heat resistance, corrosion resistance and thermal conductivity. Its high temperature resistance, mechanical strength and thermal conductivity are much higher than cordierite, and it can withstand more severe use environments. Moreover, the pore structure of SiC is controllable, and honeycomb ceramics with high porosity and uniform pore size distribution can be prepared. Its temperature field distribution is more uniform due to high porosity and strong thermal diffusion performance. With its excellent thermal conductivity, high temperature resistance and corrosion resistance, SiC is gradually replacing cordierite as the first choice of honeycomb ceramic material for the new generation, and its market prospects are increasingly broad.

[0005] In the actual industrial application process, when the concentration of VOCs is high, the VOCs reaction releases a lot of heat. Due to the low heat transfer coefficient of ordinary catalysts, the heat cannot be conducted well, resulting in local overheating of the catalyst bed, sintering and deactivation of the catalyst, and also bringing certain safety hazards. In addition, the existing catalysts have low catalytic activity at low temperatures. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems of local high temperature and poor low-temperature activity of the catalyst caused by large heat release and untimely heat conduction in the existing catalytic oxidation treatment technology for VOCs, and to provide a catalytic oxidation catalyst coated with a silicon carbide carrier and its preparation method and application. The catalytic oxidation catalyst has the advantages of low ignition temperature, high conversion efficiency, good thermal stability, etc., and is suitable for the removal of various types of VOCs.

[0007] In order to achieve the above-mentioned objectives, the present invention provides, on one hand, a catalytic oxidation catalyst coated with a silicon carbide carrier, comprising a silicon carbide carrier and a coating coated on the silicon carbide carrier, wherein the coating contains a zirconium-aluminum composite oxide, a molecular sieve, a manganese oxide and an active precious metal component, the total coating amount of the coating is 60-180 g / L, and the precious metal loading amount is 0.2-2 g / L.

[0008] Preferably, the noble metal in the active noble metal component is a combination of Pt and Pd.

[0009] Preferably, the mass ratio of Pt to Pd is 0.1-10:1, preferably 1.5-8.5:1.

[0010] Preferably, in the coating, the mass of the zirconium-aluminum composite oxide accounts for 50-80% of the total weight of the coating.

[0011] Preferably, in the zirconium-aluminum composite oxide, the mass ratio of ZrO2 to Al2O3 is 1:9-39.

[0012] Preferably, in the coating, the mass of the molecular sieve accounts for 10-30% of the total mass of the coating.

[0013] Preferably, the molecular sieve is at least one of β-type molecular sieve, CHA-type molecular sieve and MFI-type molecular sieve.

[0014] Preferably, in the coating, the mass of the manganese oxide accounts for 5-20% of the total mass of the coating.

[0015] Preferably, the silicon carbide carrier is an integral silicon carbide honeycomb ceramic carrier or a spliced ​​silicon carbide honeycomb ceramic carrier.

[0016] Preferably, the pore density of the silicon carbide carrier is 200-600 mesh.

[0017] A second aspect of the present invention provides a method for preparing the above-mentioned silicon carbide carrier-coated catalytic oxidation catalyst, the method comprising the following steps:

[0018] (1) mixing zirconium-aluminum composite oxide and molecular sieve in deionized water and ball milling to prepare a slurry;

[0019] (2) mixing a noble metal precursor solution and an organic acid additive, and then mixing the mixture with the slurry obtained in step (1), and then mixing the obtained mixture with a manganese salt to obtain a coating slurry;

[0020] (3) The silicon carbide carrier is immersed in the coating slurry, and then purged, dried and calcined in sequence.

[0021] Preferably, in step (1), the ratio of the total mass of the zirconium-aluminum composite oxide and the molecular sieve to the mass of deionized water is 2:3-8.

[0022] Preferably, the ball milling process controls the particle size D of the slurry. 90 8-30μm.

[0023] Preferably, in step (2), the mass ratio of the noble metal content in the noble metal precursor solution to the amount of the organic acid auxiliary agent is 1:2-30, preferably 1:5-16.

[0024] Preferably, the noble metal precursor is selected from platinum nitrate, platinum chloride, chloroplatinic acid, palladium nitrate, palladium chloride and chloropalladic acid.

[0025] Preferably, the organic acid adjuvant is at least one of glycine, citric acid and tartaric acid.

[0026] Preferably, the manganese salt is selected from manganese nitrate, manganese chloride, manganese bromide and potassium permanganate.

[0027] Preferably, the operation process of step (3) is: immersing the silicon carbide carrier in the coating slurry, taking it out after soaking for 1-5 minutes, blowing through the channels inside the silicon carbide carrier, the blowing time is 0.5-3 minutes, then drying at 100-150°C for 5-12 hours, and then calcining at 400-550°C for 1-3 hours.

[0028] Preferably, the method also includes preparing zirconium-aluminum composite oxide according to the following steps: weighing zirconium oxynitrate and active Al2O3 powder, and preparing an aqueous zirconium oxynitrate solution according to the saturated adsorption amount of Al2O3, adding the prepared aqueous zirconium oxynitrate solution dropwise to the active Al2O3 powder and continuously stirring for 3-10 hours, then standing and aging for 4-18 hours, drying at 100-160°C, and then calcining at 400-600°C for 2-4 hours.

[0029] The third aspect of the present invention provides the use of the catalytic oxidation catalyst coated with the silicon carbide carrier or the catalytic oxidation catalyst coated with the silicon carbide carrier prepared by the above method in the catalytic combustion process of VOCs.

[0030] In the catalytic oxidation catalyst coated with a silicon carbide carrier described in the present invention, the silicon carbide carrier (especially the integral silicon carbide honeycomb ceramic carrier or the spliced ​​silicon carbide honeycomb ceramic carrier) has the advantages of high thermal conductivity, heat resistance, corrosion resistance and high mechanical strength; in the catalyst coating, zirconium-aluminum composite oxide is used as the base coating, and the doping of ZrO2 in the activated alumina can stabilize the active precious metals (such as Pt, Pd), significantly improving the heat resistance of the coating; in addition, in the catalyst coating, the addition of molecular sieves can help the catalyst adsorb VOCs at low temperature, desorb at high temperature, and then catalytically oxidize by the catalyst, thereby further improving the conversion rate of pollutant treatment.

[0031] Moreover, in the method for preparing a catalytic oxidation catalyst coated with a silicon carbide carrier of the present invention, by using an organic acid additive, on the one hand, the adsorption state of active precious metals (such as Pt, Pd) on the surface and inside of the base coating can be changed to a certain extent, thereby achieving uniform loading and controllable distribution of the precious metals; on the other hand, the use of a weakly reducing organic acid can adjust the Mn valence state of manganese oxide (MnOx) in the catalyst coating (increasing the content of Mn3O4 to a certain extent), thereby significantly improving the low-temperature oxidation ability of the catalyst, especially the low-temperature ignition activity.

[0032] The preparation method of the present invention is simple, the steps are easy to operate, and it is particularly suitable for industrial large-scale production. The prepared catalyst has outstanding ignition activity, high conversion efficiency, and high thermal stability, and is suitable for the removal of various types of VOCs.

[0033] The catalyst of the present invention is suitable for treating low-concentration VOCs, and can treat various types of VOCs such as hydrocarbons, benzene, aldehydes, esters, etc. It has the characteristics of fast heating rate, good selectivity, high conversion efficiency and high thermal stability, and has broad application prospects. DETAILED DESCRIPTION

[0034] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0035] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0036] The catalytic oxidation catalyst coated with a silicon carbide carrier of the present invention comprises a silicon carbide carrier and a coating coated on the silicon carbide carrier, wherein the coating contains zirconium-aluminum composite oxide, molecular sieve, manganese oxide and active precious metal components.

[0037] In the catalytic oxidation catalyst coated with a silicon carbide carrier according to the present invention, the total coating amount of the coating is 60-180 g / L, specifically, for example, 60 g / L, 70 g / L, 80 g / L, 90 g / L, 100 g / L, 110 g / L, 120 g / L, 130 g / L, 140 g / L, 150 g / L, 160 g / L, 170 g / L or 180 g / L. In this article, the total coating amount of the coating refers to the coating amount (in grams) of the coating material relative to the volume of the silicon carbide carrier per liter.

[0038] In the catalytic oxidation catalyst coated with the silicon carbide carrier of the present invention, the precious metal loading is 0.2-2 g / L, preferably 0.5-1.5 g / L, specifically, for example, 0.5 g / L, 0.6 g / L, 0.7 g / L, 0.8 g / L, 0.9 g / L, 1 g / L, 1.1 g / L, 1.2 g / L, 1.3 g / L, 1.4 g / L or 1.5 g / L. In this article, the precious metal loading refers to the loading amount (in grams) of the active precious metal component in the coating in terms of precious metal elements relative to the volume of the silicon carbide carrier per liter.

[0039] In the catalytic oxidation catalyst coated with a silicon carbide carrier of the present invention, the precious metal in the active precious metal component can be various precious metals conventional in the art, such as Pt, Pd, Au, etc. In a more preferred embodiment, the precious metal in the active precious metal component is Pt and / or Pd. More preferably, the precious metal in the active precious metal component is a combination of Pt and Pd. When the precious metal in the active precious metal component is a combination of Pt and Pd, the mass ratio of Pt to Pd is 0.1-10:1, preferably 1.5-8.5:1, specifically, for example, it can be 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1, 2.2:1, 2.4:1, 2.5:1, 2.8:1, 3:1, 3.2:1, 3.5:1, 3.8:1, 4:1, 4.5:1, 4.8:1, 5:1, 5.1:1, 5.5:1, 5.8:1, 6:1, 6.5:1, 6.8:1, 7:1, 7.5:1, 7.8:1, 8:1, 8.2:1, 8.4:1 or 8.5:1.

[0040] In the catalytic oxidation catalyst coated with a silicon carbide carrier described in the present invention, preferably, in the coating, the mass of the zirconium-aluminum composite oxide accounts for 50-80% of the total weight of the coating, specifically, for example, it can be 50%, 52%, 55%, 58%, 60%, 63%, 65%, 67%, 70%, 72%, 75%, 78% or 80%.

[0041] In the catalytic oxidation catalyst coated with a silicon carbide carrier described in the present invention, in the zirconium-aluminum composite oxide, the mass ratio of ZrO2 to Al2O3 can be 1:9-39, specifically, for example, it can be 1:9, 1:10, 1:12, 1:14, 1:15, 1:16, 1:18, 1:20, 1:22, 1:24, 1:25, 1:26, 1:28, 1:30, 1:32, 1:34, 1:35, 1:36, 1:38 or 1:39.

[0042] In the catalytic oxidation catalyst coated with a silicon carbide carrier described in the present invention, preferably, in the coating, the mass of the molecular sieve accounts for 10-30% of the total mass of the coating, specifically, for example, it can be 10%, 12%, 14%, 15%, 16%, 18%, 20%, 22%, 24%, 25%, 26%, 28% or 30%.

[0043] In the present invention, the molecular sieve may be at least one of a β-type molecular sieve, a CHA-type molecular sieve and an MFI-type molecular sieve.

[0044] In the catalytic oxidation catalyst coated with a silicon carbide carrier of the present invention, preferably, in the coating, the mass of the manganese oxide accounts for 5-20% of the total mass of the coating, specifically, for example, it can be 5%, 6%, 8%, 10%, 12%, 14%, 15%, 16%, 18% or 20%. In the present invention, the manganese oxide includes Mn3O4, Mn2O3, MnO2, etc.

[0045] In the catalytic oxidation catalyst coated with a silicon carbide carrier of the present invention, the silicon carbide carrier is preferably a silicon carbide honeycomb ceramic carrier. The pore density of the silicon carbide honeycomb ceramic carrier can be 200-600 mesh, specifically, for example, 200 mesh, 250 mesh, 300 mesh, 400 mesh, 500 mesh or 600 mesh. In this article, the pore density refers to the number of holes per inch of the carrier, for example, 200 mesh means that there are 200 holes per inch of the carrier, and 200×200 holes per square inch of the carrier. In a specific embodiment, the silicon carbide carrier is a monolithic silicon carbide honeycomb ceramic carrier or a spliced ​​silicon carbide honeycomb ceramic carrier.

[0046] In some specific embodiments, the catalytic oxidation catalyst coated with a silicon carbide carrier includes a silicon carbide honeycomb ceramic carrier and a coating coated on the silicon carbide honeycomb ceramic carrier, the coating containing zirconium-aluminum composite oxide, molecular sieve, manganese oxide and active precious metal components, the total coating amount of the coating is 60-180 g / L, and the precious metal loading amount is 0.2-2 g / L, wherein the precious metal in the active precious metal component is a combination of Pt and Pd, and the mass ratio of Pt to Pd is 0.1-10:1.

[0047] In other specific embodiments, the catalytic oxidation catalyst coated with a silicon carbide carrier includes a silicon carbide honeycomb ceramic carrier and a coating coated on the silicon carbide honeycomb ceramic carrier, the coating containing zirconium-aluminum composite oxide, molecular sieve, manganese oxide and active precious metal components, the total coating amount of the coating is 60-180 g / L, and the precious metal loading amount is 0.2-2 g / L, wherein the precious metal in the active precious metal component is a combination of Pt and Pd, and the mass ratio of Pt to Pd is 0.1-10:1, and in the coating, the mass of the zirconium-aluminum composite oxide accounts for 50-80% of the total weight of the coating, the mass of the molecular sieve accounts for 10-30% of the total mass of the coating, and the mass of the manganese oxide accounts for 5-20% of the total mass of the coating.

[0048] In other specific embodiments, the catalytic oxidation catalyst coated on the silicon carbide carrier comprises a silicon carbide honeycomb ceramic carrier and a coating coated on the silicon carbide honeycomb ceramic carrier, wherein the coating contains a zirconium-aluminum composite oxide, a molecular sieve, a manganese oxide and an active precious metal component, wherein the total coating amount of the coating is 60-180 g / L, and the precious metal loading amount is 0.2-2 g / L, wherein the precious metal in the active precious metal component is a combination of Pt and Pd, and the mass ratio of Pt to Pd is 0.1-10:1, and in the coating In the layer, the mass of the zirconium-aluminum composite oxide accounts for 50-80% of the total weight of the coating, the mass of the molecular sieve accounts for 10-30% of the total weight of the coating, and the mass of the manganese oxide accounts for 5-20% of the total weight of the coating; in the zirconium-aluminum composite oxide, the mass ratio of ZrO2 to Al2O3 is 1:9-39; the molecular sieve is at least one of β-type molecular sieve, CHA-type molecular sieve and MFI-type molecular sieve; the silicon carbide honeycomb ceramic carrier is an integral silicon carbide honeycomb ceramic carrier or a spliced ​​silicon carbide honeycomb ceramic carrier.

[0049] In other specific embodiments, the catalytic oxidation catalyst coated on the silicon carbide carrier includes a silicon carbide honeycomb ceramic carrier and a coating coated on the silicon carbide honeycomb ceramic carrier, wherein the coating contains a zirconium-aluminum composite oxide, a molecular sieve, a manganese oxide, and an active precious metal component, wherein the total coating amount of the coating is 60-180 g / L, and the precious metal loading amount is 0.5-1.5 g / L, wherein the precious metal in the active precious metal component is a combination of Pt and Pd, and the mass ratio of Pt to Pd is 1.5-8.5:1, and in the coating, the zirconium -The mass of the zirconium-aluminum composite oxide accounts for 50-80% of the total weight of the coating, the mass of the molecular sieve accounts for 10-30% of the total mass of the coating, and the mass of the manganese oxide accounts for 5-20% of the total mass of the coating; in the zirconium-aluminum composite oxide, the mass ratio of ZrO2 to Al2O3 is 1:9-39; the molecular sieve is at least one of a β-type molecular sieve, a CHA-type molecular sieve and an MFI-type molecular sieve; the silicon carbide honeycomb ceramic carrier is an integral silicon carbide honeycomb ceramic carrier or a spliced ​​silicon carbide honeycomb ceramic carrier, and its pore density is 200-600 meshes.

[0050] The present invention also provides a method for preparing the above-mentioned catalytic oxidation catalyst coated with a silicon carbide carrier, the method comprising the following steps:

[0051] (1) mixing zirconium-aluminum composite oxide and molecular sieve in deionized water and ball milling to prepare a slurry;

[0052] (2) mixing a noble metal precursor solution and an organic acid additive, and then mixing the mixture with the slurry obtained in step (1), and then mixing the obtained mixture with a manganese salt to obtain a coating slurry;

[0053] (3) The silicon carbide carrier is immersed in the coating slurry, and then purged, dried and calcined in sequence.

[0054] In step (1), the ratio of the total mass of the zirconium-aluminum composite oxide and the molecular sieve to the mass of deionized water is 2:3-8, specifically, for example, 2:3, 2:4, 2:5, 2:6, 2:7 or 2:8.

[0055] In step (1), the ball milling process controls the particle size D of the slurry. 90 8-30μm.

[0056] In the method of the present invention, the zirconium-aluminum composite oxide can be prepared by an equal volume impregnation method, and the specific preparation process may include:

[0057] Weigh zirconyl nitrate and active Al2O3 powder, and prepare an aqueous zirconyl nitrate solution according to the saturated adsorption amount of Al2O3, add the prepared aqueous zirconyl nitrate solution dropwise into the active Al2O3 powder and continue stirring for 3-10 hours, then let it stand for 4-18 hours, dry it at 100-160°C, and then calcine it at 400-600°C for 2-4 hours.

[0058] In the method described in the present invention, the molecular sieve may be at least one of a β-type molecular sieve, a CHA-type molecular sieve and an MFI-type molecular sieve.

[0059] In step (2), the mass ratio of the noble metal content in the noble metal precursor solution to the amount of the organic acid additive is 1:2-30, preferably 1:5-16.

[0060] In the method of the present invention, the noble metal precursor is selected from platinum nitrate, platinum chloride, chloroplatinic acid, palladium nitrate, palladium chloride and chloropalladic acid.

[0061] In the method of the present invention, the organic acid auxiliary agent is at least one of glycine, citric acid and tartaric acid.

[0062] In the method of the present invention, the manganese salt is selected from manganese nitrate, manganese chloride, manganese bromide and potassium permanganate.

[0063] In step (3), the specific operation process is: immersing the silicon carbide carrier in the coating slurry, taking it out after soaking for 1-5 minutes, blowing through the channels inside the silicon carbide carrier, the blowing time is 0.5-3 minutes, then drying at 100-150°C for 5-12 hours, and then calcining at 400-550°C for 1-3 hours.

[0064] In some specific embodiments, the method for preparing the catalytic oxidation catalyst coated with a silicon carbide carrier comprises:

[0065] The zirconium-aluminum composite oxide and the molecular sieve are mixed and ball-milled in deionized water to prepare a slurry, wherein the total mass ratio of the zirconium-aluminum composite oxide and the molecular sieve to the mass of the deionized water is 2:3-8, and the ball-milling process controls the particle size D of the slurry. 90 8-30μm;

[0066] Mixing a noble metal precursor solution and an organic acid additive, then mixing with the slurry, and then mixing the obtained mixture with a manganese salt to obtain a coating slurry, wherein the mass ratio of the noble metal content in the noble metal precursor solution to the amount of the organic acid additive is 1:2-30;

[0067] The silicon carbide honeycomb ceramic carrier is immersed in the coating slurry, taken out after soaking for 1-5 minutes, and the channels inside the silicon carbide honeycomb ceramic carrier are blown through for 0.5-3 minutes, followed by drying at 100-150°C for 5-12 hours, and then calcining at 400-550°C for 1-3 hours.

[0068] In other specific embodiments, the method for preparing the catalytic oxidation catalyst coated with a silicon carbide carrier comprises:

[0069] Weigh zirconium oxynitrate and active Al2O3 powder, prepare an aqueous zirconium oxynitrate solution according to the saturated adsorption amount of Al2O3, drop the prepared aqueous zirconium oxynitrate solution into the active Al2O3 powder and continue stirring for 3-10 hours, then stand for aging for 4-18 hours, dry at 100-160°C, and then calcine at 400-600°C for 2-4 hours to obtain a zirconium-aluminum composite oxide;

[0070] The prepared zirconium-aluminum composite oxide and molecular sieve are mixed and ball-milled in deionized water to prepare a slurry, wherein the total mass ratio of the zirconium-aluminum composite oxide and the molecular sieve to the mass of the deionized water is 2:3-8, and the ball-milling process controls the particle size D of the slurry. 90 8-30μm;

[0071] Mixing a noble metal precursor solution and an organic acid additive, then mixing with the slurry, and then mixing the obtained mixture with a manganese salt to obtain a coating slurry, wherein the mass ratio of the noble metal content in the noble metal precursor solution to the amount of the organic acid additive is 1:5-16;

[0072] The silicon carbide honeycomb ceramic carrier is immersed in the coating slurry, and taken out after soaking for 1-5 minutes, and the channels inside the silicon carbide honeycomb ceramic carrier are blown through for 0.5-3 minutes, and then dried at 100-150° C. for 5-12 hours, and then calcined at 400-550° C. for 1-3 hours;

[0073] Among them, the precious metal precursors are platinum nitrate and palladium nitrate, the molecular sieve can be at least one of β-type molecular sieve, CHA-type molecular sieve and MFI-type molecular sieve, the organic acid additive is at least one of glycine, citric acid and tartaric acid, the manganese salt is manganese nitrate, and the silicon carbide honeycomb ceramic carrier is an integral silicon carbide honeycomb ceramic carrier or a spliced ​​silicon carbide honeycomb ceramic carrier, and its pore density is 200-600 mesh.

[0074] The present invention also provides the use of the catalytic oxidation catalyst coated with the silicon carbide carrier or the catalytic oxidation catalyst coated with the silicon carbide carrier prepared by the above method in the catalytic combustion process of VOCs.

[0075] In the present invention, the catalytic oxidation catalyst coated with the silicon carbide carrier is suitable for low-concentration VOCs treatment occasions, and can treat various types of VOCs such as hydrocarbons, benzene, aldehydes, esters, etc. Because it has the characteristics of fast heating rate, good selectivity, high conversion efficiency and high thermal stability, it has broad application prospects.

[0076] The catalytic oxidation catalyst coated with a silicon carbide carrier and its preparation method and application are further described below by way of examples. The examples are implemented based on the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following examples.

[0077] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are all commercially available.

[0078] Example 1

[0079] In the catalytic oxidation catalyst prepared in this embodiment, the catalyst carrier is a spliced ​​silicon carbide honeycomb ceramic carrier with a volume of 1.4 liters and a pore density of 200 meshes; the coating contains zirconium-aluminum composite oxide, β molecular sieve and manganese oxide, the total coating amount of the coating is 160 g / L, the precious metal loading amount is 1.3 g / L, and the mass ratio of precious metal Pt to precious metal Pd is 6:1.

[0080] The specific preparation process is as follows:

[0081] (1) Preparation of zirconium-aluminum composite oxide by equal volume impregnation method: 570 g of Al2O3 powder and 80 g of zirconium oxynitrate were weighed, and a zirconium oxynitrate solution was prepared according to the saturated adsorption capacity of Al2O3. The prepared zirconium oxynitrate solution was added dropwise to Al2O3 and stirred for 8 h. The mixture was then allowed to stand and aged for 12 h. The mixture was then dried at 120°C for 12 h. The zirconium-aluminum composite oxide was calcined in a muffle furnace at 550°C for 2 h to obtain a zirconium-aluminum composite oxide, wherein the mass ratio of ZrO2 to Al2O3 was 1:13.

[0082] (2) Preparation of coating slurry: Weigh 1300 g of deionized water, add 530 g of zirconium-aluminum composite oxide and 120 g of β molecular sieve in sequence, stir evenly to form a coating slurry, and ball mill the slurry until the slurry particle size is D 90 The resulting slurry was continuously stirred to obtain coating slurry 1-1.

[0083] (3) Loading of precious metals: Mix a platinum nitrate solution containing 4.992 g of pure Pt and a palladium nitrate solution containing 1.105 g of pure Pd, add 40 g of glycine to the precious metal solution and stir for 1 h, then add the above solution dropwise to the coating slurry 1-1 and stir for 2 h to obtain slurry 1-2.

[0084] (4) Adding manganese oxide: 150 g of manganese nitrate solution (concentration: 50 wt%) was added to slurry 1-2 to form coating slurry I.

[0085] (5) Coating slurry on the carrier: The spliced ​​silicon carbide honeycomb ceramic carrier is immersed in the coating slurry I, and taken out after soaking for 2 minutes. Then, the excess slurry on the surface of the carrier and inside the pores is blown off with compressed air for 2 minutes. The carrier is then placed in an oven for drying at 120°C for 8 hours, and calcined in a muffle furnace at 550°C for 2 hours to obtain catalytic oxidation catalyst A.

[0086] Example 2

[0087] In the catalytic oxidation catalyst prepared in this embodiment, the catalyst carrier is a spliced ​​silicon carbide honeycomb ceramic carrier with a volume of 1.4 liters and a pore density of 200 meshes; the coating contains zirconium-aluminum composite oxide, β molecular sieve and manganese oxide, the total coating amount of the coating is 130 g / L, the precious metal loading amount is 1.0 g / L, and the mass ratio of precious metal Pt to precious metal Pd is 1.8:1.

[0088] The specific preparation process is as follows:

[0089] (1) Preparation of zirconium-aluminum composite oxide by equal volume impregnation method: 400 g of Al2O3 powder and 40 g of zirconium oxynitrate were weighed, and a zirconium oxynitrate solution was prepared according to the saturated adsorption capacity of Al2O3. The prepared zirconium oxynitrate solution was added dropwise to Al2O3 and stirred for 5 h. The mixture was then allowed to stand and aged for 12 h. The mixture was then dried at 120°C for 12 h. The zirconium-aluminum composite oxide was calcined in a muffle furnace at 550°C for 2 h to obtain a zirconium-aluminum composite oxide, wherein the mass ratio of ZrO2 to Al2O3 was 1:18.5.

[0090] (2) Preparation of coating slurry: Weigh 900 g of deionized water, add 400 g of zirconium-aluminum composite oxide and 120 g of β molecular sieve in sequence, stir evenly to form a coating slurry, and ball grind the slurry until the slurry particle size D 90 The resulting slurry was continuously stirred to obtain coating slurry 2-1.

[0091] (3) Loading of precious metals: Mix a platinum nitrate solution containing 2.736 g of pure Pt and a palladium nitrate solution containing 1.983 g of pure Pd, add 53 g of citric acid to the precious metal solution and stir for 1 h, then add the above solution dropwise to the coating slurry 2-1 and stir for 2 h to obtain slurry 2-2.

[0092] (4) Addition of manganese oxide: 200 g of manganese nitrate solution (concentration: 50 wt%) was added to slurry 2-2 to form coating slurry II.

[0093] (5) Slurry coating on the carrier: The spliced ​​silicon carbide honeycomb ceramic carrier is immersed in the coating slurry II, and taken out after soaking for 2 minutes. Then, the excess slurry on the surface of the carrier and inside the pores is blown off with compressed air for 2 minutes. The carrier is then placed in an oven for drying at 120°C for 8 hours, and calcined in a muffle furnace at 550°C for 2 hours to obtain catalytic oxidation catalyst B.

[0094] Example 3

[0095] In the catalytic oxidation catalyst prepared in this embodiment, the catalyst carrier is a spliced ​​silicon carbide honeycomb ceramic carrier with a volume of 1.4 liters and a pore density of 200 meshes; the coating contains zirconium-aluminum composite oxide, CHA type molecular sieve and manganese oxide, the total coating amount of the coating is 110 g / L, the precious metal loading amount is 1.1 g / L, and the mass ratio of precious metal Pt to precious metal Pd is 5.1:1.

[0096] The specific preparation process is as follows:

[0097] (1) Preparation of zirconium-aluminum composite oxide by equal volume impregnation method: 540 g of Al2O3 powder and 112.8 g of zirconium oxynitrate were weighed, and a zirconium oxynitrate solution was prepared according to the saturated adsorption capacity of Al2O3. The prepared zirconium oxynitrate solution was added dropwise to Al2O3 and stirred for 5 h, then allowed to stand and aged for 12 h, and then dried at 120°C for 12 h. The zirconium-aluminum composite oxide was calcined in a muffle furnace at 550°C for 2 h, wherein the mass ratio of ZrO2 to Al2O3 was 1:8.5.

[0098] (2) Preparation of coating slurry: Weigh 900 g of deionized water, add 450 g of zirconium-aluminum composite oxide and 100 g of CHA molecular sieve in sequence, stir evenly to form a coating slurry, and ball mill the slurry until the slurry particle size is D 90 The obtained slurry was continuously stirred to obtain coating slurry 3-1;

[0099] (3) Loading of precious metals: Mix a platinum nitrate solution containing 4.826 g of pure Pt and a palladium nitrate solution containing 1.248 g of pure Pd, add 40 g of tartaric acid to the precious metal solution and stir for 1 h, then add the above solution dropwise to the coating slurry 3-1 and stir for 2 h to obtain slurry 3-2.

[0100] (4) Addition of manganese oxide: 100 g of manganese nitrate solution (concentration: 50 wt%) was added to slurry 3-2 to form coating slurry III.

[0101] (5) Coating slurry on the carrier: The spliced ​​silicon carbide honeycomb ceramic carrier is immersed in the coating slurry III, and taken out after soaking for 2 minutes. Then, the excess slurry on the surface of the carrier and inside the pores is blown off with compressed air for 2 minutes. The carrier is then placed in an oven for drying at 120°C for 8 hours, and calcined in a muffle furnace at 550°C for 2 hours to obtain catalytic oxidation catalyst C.

[0102] Example 4

[0103] In the catalytic oxidation catalyst prepared in this embodiment, the catalyst carrier is a spliced ​​silicon carbide honeycomb ceramic carrier with a volume of 1.4 liters and a pore density of 200 meshes; the coating contains zirconium-aluminum composite oxide, MFI type molecular sieve and manganese oxide, the total coating amount of the coating is 90 g / L, the precious metal loading amount is 0.8 g / L, and the mass ratio of precious metal Pt to precious metal Pd is 4:1.

[0104] The specific preparation process is as follows:

[0105] (1) Preparation of zirconium-aluminum composite oxide by equal volume impregnation method: 200 g of Al2O3 powder and 20 g of zirconium oxynitrate were weighed, and a zirconium oxynitrate solution was prepared according to the saturated adsorption capacity of Al2O3. The prepared zirconium oxynitrate solution was added dropwise to Al2O3 and stirred for 4 h, then allowed to stand and aged for 15 h, and then dried at 120°C for 12 h. The zirconium-aluminum composite oxide was calcined in a muffle furnace at 600°C for 3 h, wherein the mass ratio of ZrO2 to Al2O3 was 1:18.5.

[0106] (2) Preparation of coating slurry: Weigh 1000 g of deionized water, add 180 g of zirconium-aluminum composite oxide and 70 g of MFI molecular sieve in sequence, stir evenly to form a coating slurry, and ball mill the slurry until the slurry particle size is D 90 The resulting slurry was continuously stirred to obtain coating slurry 4-1.

[0107] (3) Loading of precious metals: Mix a platinum nitrate solution containing 1.628 g of pure Pt and a palladium nitrate solution containing 0.915 g of pure Pd, add 40 g of glycine to the precious metal solution and stir for 1 h, then add the above solution dropwise to the coating slurry 4-1 and stir for 2 h to obtain slurry 4-2.

[0108] (4) Addition of manganese oxide: 80 g of manganese nitrate solution (concentration: 50 wt%) was added to slurry 4-2 to form coating slurry IV.

[0109] (5) Slurry coating on the carrier: The spliced ​​silicon carbide honeycomb ceramic carrier is immersed in the coating slurry IV, and taken out after soaking for 2 minutes. Then, the excess slurry on the surface of the carrier and inside the pores is blown off with compressed air for 2 minutes. The carrier is then placed in an oven for drying at 120°C for 8 hours, and calcined in a muffle furnace at 550°C for 2 hours to obtain catalytic oxidation catalyst D.

[0110] Example 5

[0111] In the catalytic oxidation catalyst prepared in this embodiment, the catalyst carrier is a spliced ​​silicon carbide honeycomb ceramic carrier with a volume of 1.4 liters and a pore density of 200 meshes; the coating contains zirconium-aluminum composite oxide, β molecular sieve and manganese oxide, the total coating amount of the coating is 60 g / L, the precious metal loading amount is 0.5 g / L, and the mass ratio of precious metal Pt to precious metal Pd is 8.4:1.

[0112] The specific preparation process is as follows:

[0113] (1) Preparation of zirconium-aluminum composite oxide by equal volume impregnation method: 570 g of Al2O3 powder and 52 g of zirconium oxynitrate were weighed, and a zirconium oxynitrate solution was prepared according to the saturated adsorption capacity of Al2O3. The prepared zirconium oxynitrate solution was added dropwise to Al2O3 and stirred for 5 h. The mixture was then allowed to stand and aged for 12 h. The mixture was then dried at 120°C for 12 h. The zirconium-aluminum composite oxide was calcined in a muffle furnace at 550°C for 2 h to obtain a zirconium-aluminum composite oxide, wherein the mass ratio of ZrO2 to Al2O3 was 1:20.

[0114] (2) Preparation of coating slurry: Weigh 650 g of deionized water, add 265 g of zirconium-aluminum composite oxide and 60 g of β molecular sieve in sequence, stir evenly to form a coating slurry, and ball mill the slurry until the slurry particle size D 90 The resulting slurry was continuously stirred to obtain coating slurry 5-1.

[0115] (3) Loading of precious metals: Mix a platinum nitrate solution containing 2.612 g of pure Pt and a palladium nitrate solution containing 1.415 g of pure Pd, add 40 g of tartaric acid to the precious metal solution and stir for 1 h, then add the above solution dropwise to the coating slurry 5-1 and stir for 2 h to obtain slurry 5-2.

[0116] (4) Adding manganese oxide: 80 g of manganese nitrate solution (concentration: 50 wt%) was added to slurry 5-2 to form coating slurry V.

[0117] (5) Coating slurry on the carrier: The spliced ​​silicon carbide honeycomb ceramic carrier is immersed in the coating slurry V, and taken out after soaking for 2 minutes. Then, the excess slurry on the surface of the carrier and inside the pores is blown off with compressed air for 2 minutes. The carrier is then placed in an oven for drying at 120°C for 8 hours, and calcined in a muffle furnace at 550°C for 2 hours to obtain the catalytic oxidation catalyst E.

[0118] Example 6

[0119] A catalytic oxidation catalyst was prepared according to the method of Example 1, except that the carrier used in the slurry coating process was a monolithic silicon carbide honeycomb ceramic carrier with a volume of 1.4 liters and a pore density of 400 meshes, and finally a catalytic oxidation catalyst F was obtained.

[0120] Example 7

[0121] A catalytic oxidation catalyst was prepared according to the method of Example 1, except that during the noble metal loading process, the amount of platinum nitrate and palladium nitrate was controlled so that the mass ratio of Pt to Pd in ​​the finally prepared catalyst was 0.2:1, and finally catalytic oxidation catalyst G was obtained.

[0122] Example 8

[0123] A catalytic oxidation catalyst was prepared according to the method of Example 1, except that, during the noble metal loading process, the amount of platinum nitrate and palladium nitrate was controlled so that the mass ratio of Pt to Pd in ​​the finally prepared catalyst was 10:1, and finally a catalytic oxidation catalyst H was obtained.

[0124] Example 9

[0125] A catalytic oxidation catalyst was prepared according to the method of Example 1, except that in the process of preparing the zirconium-aluminum composite oxide, the amount of Al2O3 powder and zirconium oxynitrate was controlled so that the mass ratio of ZrO2 to Al2O3 in the prepared zirconium-aluminum composite oxide was 1:5, and finally catalytic oxidation catalyst I was obtained.

[0126] Example 10

[0127] A catalytic oxidation catalyst was prepared according to the method of Example 1, except that in the process of preparing the zirconium-aluminum composite oxide, the amount of Al2O3 powder and zirconium oxynitrate was controlled so that the mass ratio of ZrO2 to Al2O3 in the prepared zirconium-aluminum composite oxide was 1:45, and finally catalytic oxidation catalyst J was obtained.

[0128] Comparative Example 1

[0129] A catalytic oxidation catalyst was prepared according to the method of Example 1, except that the carrier used in the slurry coating process was a cordierite honeycomb ceramic carrier, and finally a catalytic oxidation catalyst Cat-D-1 was obtained.

[0130] Comparative Example 2

[0131] The catalytic oxidation catalyst was prepared according to the method of Example 1, except that during the coating of the slurry, the total coating amount of the coating was controlled to 50 g / L, and finally the catalytic oxidation catalyst Cat-D-2 was obtained.

[0132] Comparative Example 3

[0133] The catalytic oxidation catalyst was prepared according to the method of Example 1, except that during the coating of the slurry, the precious metal loading was controlled to 0.1 g / L, and finally the catalytic oxidation catalyst Cat-D-3 was obtained.

[0134] Test Example 1

[0135] The performance of the catalytic oxidation catalyst samples prepared in Examples 1-10 and Comparative Examples 1-3 was evaluated:

[0136] The prepared catalytic oxidation catalyst samples were used to evaluate the catalytic combustion activity of VOCs. The test conditions were as follows: 1000ppm toluene, 600ppm propane, 10% O2, 5% H2O, N2 balance gas, reaction temperature 80-500℃, space velocity 30000h -1 The T of the catalytic oxidation catalyst sample was obtained. 50 and T of the catalyst samples 99 The specific results are listed in Table 1.

[0137] Table 1: T of catalytic oxidation catalyst samples for toluene 50 、T 99

[0138] Catalytic oxidation catalyst <![CDATA[T 50 (℃)]]> <![CDATA[T 99 (℃)]]> A 211 239 B 223 250 C 220 248 D 230 258 E 236 262 F 206 236 G 233 255 H 245 263 I 243 267 J 248 270 Cat-D-1 239 261 Cat-D-2 258 273 Cat-D-3 265 280

[0139] Table 2: T of catalytic oxidation catalyst samples for propane 50 、T 99

[0140] Catalytic oxidation catalyst <![CDATA[T 50 (℃)]]> <![CDATA[T 99 (℃)]]> A 334 368 B 351 387 C 329 360 D 344 375 E 346 379 F 320 352 G 358 382 H 343 373 I 348 377 J 352 389 Cat-D-1 361 402 Cat-D-2 370 411 Cat-D-3 381 426

[0141] It can be seen from Tables 1 and 2 that the T 50 and T 99 are lower than the catalytic oxidation catalysts prepared in Comparative Examples 1-3, while T 50 is the reaction temperature at which the pollutant conversion rate reaches 50%, T 50 The lower the catalyst is, the better the ignition activity is.99 is the reaction temperature at which the pollutant conversion rate reaches 99%, T 99 The lower the value, the higher the conversion efficiency of the catalyst. Therefore, the catalytic oxidation catalyst prepared by the preparation method of the present invention has good ignition activity and conversion efficiency.

[0142] Test Example 2

[0143] The thermal conductivity of the catalytic oxidation catalyst samples prepared in Examples 1-10 and Comparative Examples 1-3 was tested, and the test results are shown in Table 3 below.

[0144] Table 3: Thermal conductivity test results of catalytic oxidation catalyst samples

[0145] Catalytic oxidation catalyst Thermal conductivity (W / m·K) A 76.4 B 75.7 C 74.2 D 73.7 E 73.1 F 76.4 G 76.0 H 76.2 I 68.2 J 75.3 Cat-D-1 1.5 Cat-D-2 72.8 Cat-D-3 73.6

[0146] It can be seen from Table 3 that the thermal conductivity of the catalyst is greatly affected by the carrier, and the thermal conductivity of the silicon carbide carrier is much greater than that of the cordierite carrier; the catalyst coating layer has little effect on the thermal conductivity of the catalyst.

[0147] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A catalytic oxidation catalyst coated with a silicon carbide carrier, characterized in that: The invention comprises a silicon carbide carrier and a coating coated on the silicon carbide carrier, wherein the coating contains zirconium-aluminum composite oxide, molecular sieve, manganese oxide and active precious metal components, the total coating amount of the coating is 60-180 g / L, and the precious metal loading amount is 0.2-2 g / L.

2. The catalytic oxidation catalyst coated with a silicon carbide carrier according to claim 1, characterized in that The noble metal in the active noble metal component is a combination of Pt and Pd; Preferably, the mass ratio of Pt to Pd is 0.1-10:1, preferably 1.5-8.5:

1.

3. The catalytic oxidation catalyst coated with a silicon carbide carrier according to claim 1 or 2, characterized in that: In the coating, the mass of the zirconium-aluminum composite oxide accounts for 50-80% of the total weight of the coating.

4. The catalytic oxidation catalyst coated with a silicon carbide carrier according to claim 3, characterized in that In the zirconium-aluminum composite oxide, the mass ratio of ZrO2 to Al2O3 is 1:9-39.

5. The catalytic oxidation catalyst coated with a silicon carbide carrier according to claim 1 or 2, characterized in that: In the coating, the mass of the molecular sieve accounts for 10-30% of the total mass of the coating.

6. The catalytic oxidation catalyst coated with a silicon carbide carrier according to claim 5, characterized in that The molecular sieve is at least one of a β-type molecular sieve, a CHA-type molecular sieve and an MFI-type molecular sieve.

7. The catalytic oxidation catalyst coated with a silicon carbide carrier according to claim 1 or 2, characterized in that: In the coating, the mass of the manganese oxide accounts for 5-20% of the total mass of the coating.

8. The catalytic oxidation catalyst coated with a silicon carbide carrier according to any one of claims 1 to 7, characterized in that The silicon carbide carrier is an integral silicon carbide honeycomb ceramic carrier or a spliced ​​silicon carbide honeycomb ceramic carrier; Preferably, the pore density of the silicon carbide carrier is 200-600 mesh.

9. A method for preparing a catalytic oxidation catalyst coated with a silicon carbide carrier according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: (1) mixing zirconium-aluminum composite oxide and molecular sieve in deionized water and ball milling to prepare a slurry; (2) mixing a noble metal precursor solution and an organic acid additive, and then mixing the mixture with the slurry obtained in step (1), and then mixing the obtained mixture with a manganese salt to obtain a coating slurry; (3) The silicon carbide carrier is immersed in the coating slurry, and then purged, dried and calcined in sequence.

10. The method according to claim 9, characterized in that In step (1), the ratio of the total mass of the zirconium-aluminum composite oxide and the molecular sieve to the mass of deionized water is 2:3-8; Preferably, the ball milling process controls the particle size D of the slurry. 90 8-30μm.

11. The method according to claim 9, characterized in that In step (2), the mass ratio of the noble metal content in the noble metal precursor solution to the amount of the organic acid additive is 1:2-30, preferably 1:5-16; Preferably, the noble metal precursor is selected from platinum nitrate, platinum chloride, chloroplatinic acid, palladium nitrate, palladium chloride and chloropalladic acid; Preferably, the organic acid adjuvant is at least one of glycine, citric acid and tartaric acid.

12. The method according to claim 9, characterized in that The manganese salt is selected from manganese nitrate, manganese chloride, manganese bromide and potassium permanganate.

13. The method according to claim 9, characterized in that The operation process of step (3) is: immersing the silicon carbide carrier in the coating slurry, taking it out after soaking for 1-5 minutes, blowing through the channels inside the silicon carbide carrier, the blowing time is 0.5-3 minutes, then drying at 100-150°C for 5-12 hours, and then calcining at 400-550°C for 1-3 hours.

14. The method according to any one of claims 9 to 13, characterized in that: The method also includes preparing the zirconium-aluminum composite oxide according to the following steps: Weigh zirconyl nitrate and active Al2O3 powder, and prepare an aqueous zirconyl nitrate solution according to the saturated adsorption amount of Al2O3, add the prepared aqueous zirconyl nitrate solution dropwise into the active Al2O3 powder and continue stirring for 3-10 hours, then let it stand for 4-18 hours, dry it at 100-160°C, and then calcine it at 400-600°C for 2-4 hours.

15. Use of the catalytic oxidation catalyst coated on a silicon carbide carrier as described in any one of claims 1 to 8 or the catalytic oxidation catalyst coated on a silicon carbide carrier prepared by the method described in any one of claims 9 to 14 in the catalytic combustion process of VOCs.

Citation Information

Patent Citations

  • Molecular sieve coating load manganese based composite oxide integrated catalyst and preparation method thereof

    CN102407154A

  • Preparation method of SiC foam, SiC foam monolithic catalyst for catalytic combustion of methane, and preparation method thereof

    CN108686714A

  • Additive-containing alumina, preparation method of alumina, and alumina-containing catalyst

    CN109364905A

  • Porous nano manganese oxide catalyst, preparation and application thereof

    CN110404530A

  • Catalyst and preparation method thereof

    CN113198439A