Pearlite steel wire and drawing process and drawing system thereof
By real-time monitoring and regulating the temperature during the steel wire drawing process, and using a spray cooling unit to suppress the crystallization of cementite lamellae, the problem of low torsional toughness of high-strength pearlitic steel wires is solved, and the torsional toughness and production quality of the steel wires are significantly improved. .
Patent Information
- Application Number
- CN202410772650.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-17
AI Technical Summary
During the drawing process of high-strength pearlitic steel wire, the increase in temperature causes the crystallization of cementite lamellae, resulting in a decrease in torsional toughness and prone to delamination fracture.
During the steel wire drawing process, the steel wire exit temperature and the drawing die temperature are monitored in real time, and the crystallization phenomenon of the cementite lamellae is suppressed by regulating the spray flow rate of the spray liquid. The spray cooling unit is used to hydrate the steel wire and the mold. For spray cooling, set the cooling target temperature at 148-153°C to control the temperature rise.
It effectively suppresses the crystallization phenomenon of cementite lamellae, improves the torsional toughness of the steel wire, reduces the risk of delamination fracture, and improves the productivity and product quality of the steel wire.
Smart Images

Figure CN118768402A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-strength steel wire processing and production, and more specifically, relates to a pearlite steel wire and a drawing process and a drawing system thereof. Background Art
[0002] High-strength pearlite steel wire is widely used in bridge, aviation, railway, automobile and other industries. After high-temperature austenitization, high-strength pearlite steel wire rod is isothermal heat treated to obtain a uniform nano-flaky ferrite (α-Fe) and cementite (Fe3C) alternating pearlite lamellar structure, and then subjected to large strain multi-pass cold drawing to obtain ultra-high strength steel wire.
[0003] During the drawing process, the pearlite lamellae become thinner, the dislocation density increases, and a large amount of heat is generated, which causes the surface temperature of the steel wire to rise. During the continuous drawing process, the temperature is difficult to reduce as it passes through the drawing die, resulting in the crystallization of the cementite lamellae in the microstructure. Crystallized cementite has a stronger barrier effect on dislocations, so more serious dislocation pileups and stress concentration are likely to occur inside the steel wire with a high degree of crystallization, thereby reducing the torsional toughness of the steel wire. Delamination cracks appear in the early stage of torsion, causing the steel wire to delaminate and break prematurely after being twisted for 7-9 turns. In actual production, the steel wire is required to have good torsional toughness, so it is of great significance to effectively inhibit the occurrence of cementite crystallization during the drawing process. Summary of the invention
[0004] One of the purposes of the present invention is to provide a pearlite steel wire drawing process and a drawing system, so as to effectively solve the problem in the existing high-strength pearlite steel wire drawing production process that the temperature increase easily leads to the crystallization of cementite lamellae inside the steel wire, thereby reducing the torsional toughness of the steel wire.
[0005] Another object of the present invention is to provide a pearlite steel wire, thereby solving the problem of relatively low torsional toughness of existing high-strength pearlite steel wire.
[0006] In order to achieve the above object, the technical solution provided by the present invention is:
[0007] The present invention provides a pearlite steel wire drawing process, comprising:
[0008] Before the steel wire drawing production, start the spray cooling unit in advance to spray water on the drawing die and steel wire;
[0009] During the wire drawing process, the wire exit die temperature and the last die temperature are monitored in real time, and the spray flow rate L of the spray liquid is regulated according to the following formula (unit: mL / s):
[0010] When the mold temperature T1>T0, control the spray flow rate
[0011] When the mold temperature T1<T0, control the spray flow rate
[0012] Among them, T1 is the wire exit die temperature during the drawing process, T2 is the die temperature of the last pass N; T0 is the set cooling target temperature; ε1, ε2, …, ε N are the true strain variables of the steel wire in each drawing pass; a and b are initialization constants, and when the drawing die and steel wire are sprayed with water before the steel wire drawing production, the spraying is carried out at a flow rate of a.
[0013] In the traditional steel wire production process, the surface temperature of the steel wire increases due to the thermal effect during the drawing process, and the temperature will continue to rise and remain for a period of time when it passes through the drawing die continuously. Therefore, the instantaneous temperature of the steel wire passing through the drawing die is relatively high. At this time, due to the increase in temperature, the amorphous cementite in the microstructure of the steel wire will gradually crystallize. Compared with the amorphous cementite lamellae, the crystallized cementite has more serious blockage of dislocations, which will cause stress concentration inside the steel wire, thereby reducing the torsional toughness of the steel wire.
[0014] In view of the above phenomenon, the present invention proposes a pearlite steel wire drawing process, which monitors the steel wire demolding temperature and the mold temperature of the last pass in real time, and regulates the spray flow rate L of the spray liquid according to the monitored temperature, thereby effectively suppressing the crystallization of cementite lamellae during the drawing process, solving the technical problem that the traditional steel wire drawing production process easily leads to the deterioration of the torsional toughness of the steel wire, significantly improving the torsional toughness of the steel wire, and thus helping to reduce the risk of delamination and fracture of the steel wire.
[0015] Specifically, if the die exit temperature T1>T0°C, the spray flow rate of the spray liquid is increased until the die exit temperature T1 meets the requirement of the set cooling target temperature. At this time, the nozzle flow rate L is kept constant to suppress the temperature rise effect during the wire drawing process. If the die exit temperature T1<T0°C, the spray flow rate of the spray liquid can be reduced. The degree of reduction in the flow rate of the spray liquid must ensure that the temperature rise effect during the wire drawing process can be effectively suppressed (i.e., it does not exceed the set cooling target temperature).
[0016] Furthermore, the initialization constants a and b are calculated according to the following formula:
[0017]
[0018]
[0019] In the above formula, t1 is the on-site room temperature, t2 is the temperature of the coolant, γ% is the carbon content in the steel wire, φ0 is the initial wire rod diameter, unit: mm; φ Nis the wire diameter of the Nth pass; V is the wire drawing speed, in mm / s, and the control accuracy of the wire drawing speed V is ±5%.
[0020] Furthermore, the cooling target temperature T0 is set to 148-153°C. Combining the recrystallization temperature of high carbon steel and the daily production experience of steel wire, it is found that when the temperature upper limit is exceeded, the cementite in the internal microstructure of the steel wire will undergo a more serious crystallization phenomenon, so the cooling target temperature T0 is controlled to 148-153°C.
[0021] Furthermore, the method also includes: drying the steel wire after being drawn out of the mold, thereby effectively reducing the risk of rusting of the steel wire during storage.
[0022] The present invention also provides a pearlite steel wire drawing system, comprising:
[0023] Drawing die, used for drawing steel wire;
[0024] Spray cooling unit, used for spray cooling of drawing dies and steel wires;
[0025] The first temperature measuring unit and the second temperature measuring unit are used to monitor the temperature of the drawing die and the steel wire after being ejected from the die in real time, respectively; and
[0026] The control unit is used to control the spray flow rate L of the spray liquid according to the temperatures measured by the first temperature measuring unit and the second temperature measuring unit. The specific control method is as follows:
[0027] When the mold temperature T1>T0, control the spray flow rate
[0028] When the mold temperature T1<T0, control the spray flow rate
[0029] Among them, T1 is the wire exit die temperature during the drawing process, T2 is the die temperature of the last pass N; T0 is the set cooling target temperature; ε1, ε2, …, ε N are the true strain variables of the steel wire in each drawing pass; a and b are initialization constants, and when the drawing die and steel wire are sprayed with water before the steel wire drawing production, the spraying is carried out at a flow rate of a.
[0030] Furthermore, the spray cooling unit includes a spray pipe and a spray head installed on the spray pipe, wherein the spray direction of the spray head is toward the drawing die and the steel wire.
[0031] Furthermore, the spray pipe is provided with a plurality of nozzles, and the spray pipe is connected to the water inlet pipe through a water pump; the water pump and the first temperature measuring unit and the second temperature measuring unit are all connected to the control unit. The temperatures measured by the first temperature measuring unit and the second temperature measuring unit are fed back to the control unit, and then the pressure of the water pump is controlled and adjusted by the control unit to adjust the spray flow rate.
[0032] Furthermore, the spray cooling unit also includes a water tank, which is located below the drawing die and is used to collect and recycle the falling spray water, and a filter is provided above the water tank. The spray liquid used for spray cooling naturally falls into the water tank, and the iron filings generated during the drawing process are filtered through the filter to avoid pipe clogging. At the same time, the water that falls into the water tank and is filtered can be collected and recycled in subsequent production.
[0033] Furthermore, the system also includes a drying unit, which is used to dry the steel wire after being drawn out of the die.
[0034] The present invention also provides a pearlite steel wire, which is drawn by any of the above-mentioned drawing methods or any of the drawing systems, thereby effectively suppressing the crystallization of cementite during the drawing process. The torsional toughness of the pearlite steel wire is effectively improved compared with the steel wire produced by the traditional drawing process.
[0035] In summary, the technical solution provided by the present invention can achieve the following beneficial effects compared with the prior art:
[0036] (1) The present invention monitors the wire ejection temperature and the drawing die temperature in real time during the wire drawing process, and regulates the spray flow rate of the spray liquid of the spray cooling unit according to the wire ejection temperature, thereby effectively avoiding excessive temperature during the wire drawing process and inhibiting the occurrence of cementite lamellar crystallization, while also helping to save water.
[0037] (2) The pearlite steel wire drawing system of the present invention comprises: a drawing die, a spray cooling unit, a first temperature measuring unit and a second temperature measuring unit, and a control unit, wherein the first temperature measuring unit and the second temperature measuring unit are respectively used to monitor the temperature of the drawing die and the steel wire after being ejected from the die in real time and feed back the temperature to the control unit, and the control unit regulates the flow rate of the spray liquid of the spray cooling unit according to the fed-back temperature, thereby effectively suppressing the occurrence of cementite lamellar crystallization, improving the torsional toughness of the steel wire, and reducing the occurrence of stratification of the steel wire in the torsion test, which is beneficial to ensure the normal production and use of the steel wire.
[0038] (3) The drawing system of the present invention has a simple structure and only needs to be slightly modified on the basis of the traditional drawing system. It is fully compatible with most existing high-strength steel wire drawing production processes, and realizes the regulation of the temperature effect during the steel wire drawing process. It has important guiding significance for the optimization and upgrading of the steel wire drawing process, and improves the steel wire productivity and product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 is a schematic structural diagram of a drawing system according to an embodiment of the present invention;
[0040] Among them: 1. water tank; 2. water pump; 3. spray pipe; 4. nozzle; 5. support beam; 6. second temperature measuring unit; 7. drying unit; 8. filter; 9. drain outlet; 10. control unit; 11. first temperature measuring unit; 12. steel wire; 13. drawing die; 14. water inlet pipe;
[0041] Figure 2 is a TEM microstructure diagram of the steel wire when the die-out temperature is high in Example 1 of the present invention;
[0042] Figure 3 is a torsional layered fracture diagram of the steel wire when the die-out temperature is high in Example 1 of the present invention;
[0043] Figure 4 is a TEM microstructure diagram of the steel wire when the die-out temperature is stabilized at 153° C. in Example 1 of the present invention;
[0044] Figure 5 This is a torsional cross-sectional view of the steel wire when the die-out temperature is stabilized at 153° C. in Example 1 of the present invention;
[0045] Figure 6 is a TEM microstructure diagram of the steel wire when the ejection temperature is 148° C. in Example 2 of the present invention;
[0046] Figure 7 is a torsional cross-section diagram of the steel wire when the die-out temperature is 148° C. in Example 2 of the present invention;
[0047] Figure 8 is a TEM microstructure diagram of the steel wire when the die-out temperature is high in Example 3 of the present invention;
[0048] Fig. 9 is a torsional layered fracture diagram of the steel wire when the die-out temperature is high in Example 3 of the present invention;
[0049] Fig.10 is a TEM microstructure diagram of the steel wire when the die-out temperature is stabilized at 152° C. in Example 3 of the present invention;
[0050] Fig.11 It is a torsional cross-section diagram of the steel wire when the die temperature is stabilized at 152° C. in Example 3 of the present invention. DETAILED DESCRIPTION
[0051] The present invention provides a drawing process for high-strength pearlite steel wire, comprising:
[0052] Before the steel wire drawing production, start the spray cooling unit in advance to spray cool the drawing die and steel wire;
[0053] During the wire drawing process, the wire exit die temperature and the last die temperature are monitored in real time, and the spray flow rate L of the spray liquid is regulated according to the following formula (unit: mL / s):
[0054] When the mold temperature T1>T0, control the spray flow rate
[0055] When the mold temperature T1<T0, control the spray flow rate
[0056] Among them, T1 is the wire die exit temperature during the drawing process, T2 is the die temperature of the last pass N; T0 is the set cooling target temperature, which is 145±5℃; ε1, ε2, …, ε N are the true strain of the steel wire in each drawing pass; a and b are initialization constants.
[0057] Specifically, before the steel wire drawing production, the spray cooling unit is turned on in advance, and the initialization constants a and b are calculated, and the spraying is continued for 2-5 minutes at the speed of a, and then the steel wire drawing production is started. The parameters of the steel wire drawing process include: the carbon content γ% in the high-strength steel wire (usually between 0.70% and 1.10%), the initial wire rod diameter φ0 (unit: mm), and the drawing pass N, and the wire diameters φ1, φ2, φ3, ... φ N and the corresponding true response variables ε0, ε1, ε2, ... N , wire drawing speed V, control accuracy ±5%.
[0058] Furthermore, the initialization constants a and b are calculated according to the following formula:
[0059]
[0060]
[0061] In the above formula, t1 is the on-site room temperature, t2 is the temperature of the coolant, and t1 and t2 are measured on-site; γ% is the carbon content in the steel wire, φ0 is the initial wire rod diameter, in mm; φ N is the wire diameter of the Nth pass; V is the wire drawing speed, the unit is mm / s, and V is the wire drawing speed.
[0062] According to the recrystallization temperature of high carbon steel and the daily production experience of steel wire, when the steel wire ejection temperature is higher than 150°C, the cementite in the internal microstructure of the steel wire will undergo a more serious crystallization phenomenon. Therefore, the cooling target temperature T0 is set to 150°C in the present invention. If the ejection temperature T1>150°C, the control system of the spray cooling unit quickly increases the water pump pressure and speeds up the nozzle flow rate through negative feedback until the ejection temperature T1<150°C, and keeps the nozzle flow rate L constant to suppress the temperature rise effect during the wire drawing process. If the ejection temperature T1<150°C, the control system of the spray cooling unit reduces the water pump pressure and slows down the nozzle flow rate through positive feedback, which can effectively suppress the temperature rise effect during the wire drawing process and also help save spray water.
[0063] The microstructure of the steel wire after drawing in the present application was observed using a transmission electron microscope, and it can be seen that the crystallization phenomenon of cementite lamellae in its microstructure has been significantly suppressed; at the same time, the steel wire prepared by drawing in the present invention was subjected to a torsion test, and no delamination cracks or delamination fractures were observed, and the torsional toughness was good, thereby proving the feasibility and reliability of the method of the present invention.
[0064] In order to further understand the content of the present invention, the present invention is now described in detail in conjunction with the accompanying drawings and embodiments. It should be noted that the following embodiments are only described by taking the production of 82B steel wire as an example, and the composition (mass percentage content) of the 82B steel wire is: C 0.82%, Si 0.22%, Mn 0.69%, Cr 0.19%, and the balance is Fe, but it is actually not limited to the drawing production of this specific high-strength pearlite steel wire. The main composition range of the applicable high-strength pearlite steel wire is: C 0.70-1.10%, Si 0.10-1.20%, Cr 0.01-1.00%, Ni 0.00-0.50%, other micro-alloying elements Nb, V, Ti, etc. 0.00-1.50%, and the balance is Fe.
[0065] Example 1
[0066] In this example, the initial diameter of the 82B strip is φ0 = 7.2 mm. After three passes of drawing, the diameter is reduced to 6.4 mm, 5.3 mm, and 4 mm, respectively. The corresponding drawing strains are ε1 = 0.24, ε2 = 0.61, ε3 = 1.18, and the drawing speed is 100 mm / s. Through microstructural observation, the microstructure is lamellar pearlite. The chemical composition of 82B steel wire is C: 0.82%, Mn: 0.69%, Si: 0.20%, S: 0.01%, and the remainder is impurity elements.
[0067] The specific steps of the steel wire drawing process in this embodiment are as follows:
[0068] Step 1: After measuring the on-site room temperature t1 = 25°C, water temperature t2 = 10°C, and pulling speed V = 100 mm / s, the initial spray speed a = 30 ml / s is calculated.
[0069] Step 2: Turn on the spray cooling unit and spray cool the mold and steel wire for 2 minutes at the spray speed of step 1.
[0070] Step 3: Start the wire drawing process, monitor the drawing die and wire exit temperature, and find that the die temperature reaches 352°C and the wire exit temperature reaches 303°C. At this time, the control unit controls the water pressure to increase quickly, and the spraying speed is increased, and the die temperature and wire exit temperature are significantly reduced. Finally, the spraying speed reaches 96ml / s, the wire die temperature drops to 186°C, and the wire exit temperature drops to 153°C.
[0071] Step 4: After the steel wire is dried by the drying unit, the finished drawn steel wire is collected.
[0072] When the temperature drops and does not stabilize, the front half of the steel wire is cut and its microstructure is observed (such as Figure 2 as shown) and torsion test (as Figure 3 As shown in the figure, it can be seen that the cementite crystallization phenomenon is obvious and the fracture morphology is a layered fracture, which proves that the temperature rise effect of wire drawing will cause the cementite crystallization in the microstructure, thereby destroying the torsional toughness of the steel wire.
[0073] When the temperature drops and stabilizes, the second half of the steel wire is cut and its microstructure is observed (e.g. Figure 4 as shown) and torsion test (as Figure 5 As shown), it was found that the cementite crystallization phenomenon was not obvious and the fracture morphology was a flat fracture, which proved that the example of the present invention can effectively inhibit the crystallization phenomenon of cementite lamellae during steel wire drawing and improve the torsional toughness of the steel wire.
[0074] Example 2
[0075] In this example, the 82B strip has an initial diameter of 3.2 mm, and is drawn in three passes to reduce the diameter to 3.0 mm, 2.7 mm, and 2.4 mm, respectively. The corresponding drawing strains are ε1 = 0.18, ε2 = 0.46, ε3 = 0.87, and the drawing speed is 80 mm / s. Through microstructural observation, the microstructure is lamellar pearlite. The chemical composition of 82B steel wire is C: 0.82%, Mn: 0.69%, Si: 0.20%, S: 0.01%, and the remainder is impurity elements.
[0076] The specific steps of the steel wire drawing process in this embodiment are as follows:
[0077] Step 1: After measuring the on-site room temperature t1 = 30°C, water temperature t2 = 10°C, and pulling speed V = 80 mm / s, the initial spray speed a = 27 ml / s is calculated.
[0078] Step 2: Turn on the spray cooling unit and spray cool the mold and steel wire for 3 minutes at the spray speed of step 1.
[0079] Step 3, start the steel wire drawing process, observe the mold temperature measuring device and the steel wire ejection temperature, and find that the mold temperature reaches 163°C and the steel wire ejection temperature reaches 128°C. At this time, the control unit sends a command to the water pump to reduce the water pressure, slow down the spraying speed, and reduce the water consumption. Finally, the spray rate reaches 16ml / s, the steel wire mold temperature drops to 173°C, and the steel wire ejection temperature drops to 148°C. If the water pressure continues to be reduced, the steel wire ejection temperature will exceed 150°C, proving that the control method of the present invention example is effective.
[0080] Step 4: After the steel wire is dried by the drying unit, the finished drawn steel wire is collected.
[0081] The rear section of the steel wire after the temperature has been reduced and stabilized is cut and its microstructure is observed (such as Figure 6 as shown) and torsion test (as Figure 7 As shown), the results show that the cementite crystallization phenomenon is not obvious, and the fracture morphology is a flat fracture, which proves that the crystallization phenomenon of the example of the present invention has been suppressed and cooling water has been saved to a certain extent.
[0082] Example 3
[0083] In this example, the 82B strip has an initial diameter of 9.0 mm, and is drawn in three passes to reduce the diameter to 7.6 mm, 6.0 mm, and 4.8 mm, respectively. The corresponding drawing strains are ε1 = 0.34, ε2 = 0.81, ε3 = 1.26, and the drawing speed is 100 mm / s. Through microstructural observation, the microstructure is lamellar pearlite. The chemical composition of 82B steel wire is C: 0.82%, Mn: 0.69%, Si: 0.20%, S: 0.01%, and the remainder is impurity elements.
[0084] Drawing system diagram of steel wire in this embodiment Figure 1 As shown, it includes:
[0085] A drawing die 13, used for drawing the steel wire;
[0086] Spray cooling unit, used for spray cooling of drawing dies and steel wires;
[0087] The first temperature measuring unit 11 and the second temperature measuring unit 6 are used to monitor the temperature of the drawing die 13 and the steel wire 12 after being ejected from the die in real time, respectively; and
[0088] The control unit 10 is used to control the spray flow rate L of the spray liquid according to the temperatures measured by the first temperature measuring unit 11 and the second temperature measuring unit 6. The specific control method is as follows:
[0089] When the mold temperature T1>T0, control the spray flow rate
[0090] When the mold temperature T1<T0, control the spray flow rate
[0091] Among them, T1 is the wire exit die temperature during the drawing process, T2 is the die temperature of the last pass N; T0 is the set cooling target temperature; ε1, ε2, …, ε N are the true strains of the steel wire in each drawing pass; a and b are initialization constants, and when the drawing die and steel wire are sprayed with water before the steel wire drawing production, the spraying is performed at a flow rate of a.
[0092] Specifically, the spray cooling unit in this embodiment includes a spray pipe 3 and a spray head 4 installed on the spray pipe, wherein the spray direction of the spray head 4 is toward the drawing die 13 and the steel wire 12. Furthermore, the spray pipe 3 is provided with a plurality of spray heads 4, such as 4, 5 or 6, which can be installed according to actual needs, and the spray pipe is connected to the water inlet pipe 14 through the water pump 2.
[0093] In this embodiment, the water pump 2 and the first temperature measuring unit 11 and the second temperature measuring unit 6 are all connected to the control unit 10. The temperatures measured by the first temperature measuring unit and the second temperature measuring unit are fed back to the control unit 10, and then the pressure of the water pump is adjusted by the control unit to adjust the spray flow rate.
[0094] As a further improvement of this embodiment, the spray cooling unit further includes a water tank 1, which is located below the drawing die and is used to collect and recycle the falling spray water, and a filter screen 8 is provided above the water tank. The spray liquid used for spray cooling naturally falls into the water tank 1, and the iron filings generated during the drawing process are filtered through the filter screen 8 to avoid pipe clogging. The water that falls into the water tank 1 and is filtered is discharged and collected through the drain port 9, and can be recycled in subsequent production, which is conducive to saving water.
[0095] Furthermore, the system further comprises a drying unit 7, which is used to dry the steel wire after being drawn out of the die. Specifically, in this embodiment, the drying unit 7 can directly adopt a fan, and the drying unit 7 and the second temperature measuring unit 6 can be installed through the support beam 5.
[0096] The specific steps of the steel wire drawing process in this embodiment are as follows:
[0097] Step 1: Statistically, the room temperature t1 = 25°C, the water temperature t2 = 10°C, and the pulling speed V = 100 mm / s, and the initial spraying speed a = 33 ml / s is calculated.
[0098] Step 2: Turn on the spray cooling unit and spray cool the mold and steel wire for 4 minutes at the spray speed of step 1.
[0099] Step 3: Start the wire drawing process, observe the mold temperature measuring device and the wire exit temperature, and find that the mold temperature reaches 358°C and the wire exit temperature reaches 306°C. At this time, the control unit sends a command to the water pump to quickly increase the water pressure and increase the spraying speed, and the mold temperature and wire exit temperature are significantly reduced. Finally, the spraying speed reaches 99ml / s, the wire mold temperature drops to 186°C, and the wire exit temperature drops to 152°C.
[0100] Step 4: After the steel wire is dried by the drying device, the finished drawn steel wire is collected.
[0101] When the temperature drops and does not stabilize, the front half of the steel wire is cut and its microstructure is observed (such as Figure 8 as shown) and torsion test (as Fig. 9 The results show that the cementite crystallization phenomenon is obvious and the fracture morphology is a layered fracture, which proves that the temperature rise effect of wire drawing will cause the cementite crystallization in the microstructure, thereby destroying the torsional toughness of the steel wire.
[0102] Step 6: When the temperature drops and stabilizes, cut the second half of the steel wire and observe its microstructure (such as Fig.10 as shown) and torsion test (as Fig.11 As shown), the results show that the cementite crystallization phenomenon is not obvious and the fracture morphology is a flat fracture, which proves that the example of the present invention can effectively inhibit the crystallization phenomenon of cementite lamellae during steel wire drawing and improve the torsional toughness of the steel wire.
[0103] In summary, when the pearlite steel wire passes through the drawing die, the large drawing strain causes the die surface and the steel wire surface temperature to rise, resulting in the crystallization of the nano-cementite lamellae under the thermal effect, which deteriorates the torsional toughness of the steel wire. In the present invention, a water spray cooling unit is introduced during the steel wire drawing process, and the spray speed during the steel wire drawing process is adjusted, so as to effectively reduce the temperature rise effect during the drawing process, inhibit the cementite crystallization phenomenon during the drawing process, thereby effectively avoiding the occurrence of torsional stratification phenomenon and improving the torsional toughness of the steel wire.
[0104] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.
Claims
1. A pearlite steel wire drawing process, characterized in that: include: Before the steel wire drawing production, start the spray cooling unit in advance to spray water on the drawing die and steel wire; During the wire drawing process, the wire die temperature and the last die temperature are monitored in real time, and the spray flow rate L of the spray liquid is adjusted according to the following formula, in mL / s, until the die temperature T1=T0 is met, and the spray flow rate L remains unchanged: When the mold temperature is greater than T0, control the spray flow rate When the mold temperature T1<T0, control the spray flow rate Among them, T1 is the wire exit die temperature during the drawing process, T2 is the die temperature of the last pass N; T0 is the set cooling target temperature; ε1, ε2, …, ε N are the true strain variables of the steel wire in each drawing pass; a and b are initialization constants, and when the drawing die and steel wire are sprayed with water before the steel wire drawing production, the spraying is carried out at a flow rate of a.
2. The pearlite steel wire drawing process according to claim 1, characterized in that: The initialization constants a and b are calculated according to the following formula: In the above formula, t1 is the on-site room temperature, t2 is the temperature of the coolant, γ% is the carbon content in the steel wire, φ0 is the initial wire rod diameter, unit: mm; φ N is the wire diameter of the Nth pass; V is the wire drawing speed, in mm / s.
3. The pearlite steel wire drawing process according to claim 2, characterized in that: Set the cooling target temperature T0 to 148-153°C.
4. The pearlite steel wire drawing process according to any one of claims 1 to 3, characterized in that: Also includes: The steel wire is dried after being drawn out of the mold.
5. A pearlite steel wire drawing system, characterized in that: include: A drawing die (13) for drawing the steel wire (12); A spray cooling unit, used for spray cooling the drawing die (13) and the steel wire (12); The first temperature measuring unit (11) and the second temperature measuring unit (6) are used to respectively monitor the temperature of the drawing die (13) and the steel wire (12) after being ejected from the die in real time; as well as The control unit (10) is used to control the spray flow rate L of the spray liquid according to the temperatures measured by the first temperature measuring unit (11) and the second temperature measuring unit (6). The specific control method is as follows: When the mold temperature T1>T0, control the spray flow rate When the mold temperature T1<T0, control the spray flow rate Among them, T 01 is the wire exit die temperature during the drawing process, T2 is the die temperature of the last pass N; T0 is the set cooling target temperature; ε1, ε2, …, ε N are the true strain variables of the steel wire in each drawing pass; a and b are initialization constants, and when the drawing die and steel wire are sprayed with water before the steel wire drawing production, the spraying is carried out at a flow rate of a.
6. The pearlite steel wire drawing system according to claim 5, characterized in that: The spray cooling unit comprises a spray pipe (3) and a spray head (4) installed on the spray pipe (3), wherein the spray direction of the spray head (4) is toward the drawing die (13) and the steel wire (12).
7. The pearlite steel wire drawing system according to claim 6, characterized in that: The spray pipe (3) is provided with a plurality of spray heads (4), and the spray pipe (3) is connected to a water inlet pipe (14) via a water pump (2); the water pump (2) and the first temperature measuring unit (11) and the second temperature measuring unit (6) are all connected to a control unit (10).
8. The pearlite steel wire drawing system according to claim 6 or 7, characterized in that: The spray cooling unit further comprises a water tank (1), which is located below the drawing die (13) and is used to collect and recycle the falling spray water, and a filter screen (8) is provided above the water tank (1).
9. The pearlite steel wire drawing system according to any one of claims 5 to 7, characterized in that: The system also comprises a drying unit (7), which is used to dry the steel wire (12) after being drawn out of the die.
10. A pearlite steel wire, characterized in that: The pearlite steel wire is drawn by the drawing method according to any one of claims 1 to 4 or the drawing system according to any one of claims 5 to 9.
Citation Information
Patent Citations
Automatic temperature control cooling water tank
CN202316608U
Cooling system of metal wire drawing machine
CN212442592U
Method and apparatus for cooling drawn wire
GB1576820A
Device for wire-drawing extremely fine wire and method for washing extremely fine wire
JP1993138244A
Water flow control method of wire rod
KR1020010010808A