Vacuum induction electrode casting liquid cooling mold, design method and application thereof

By designing a spiral water pipeline and filling the air gap with helium in vacuum induction electrode casting, the problems of slow solidification speed and pollution in the vacuum induction melting process are solved, and efficient sequential solidification and high-quality casting are achieved.

CN118768550APending Publication Date: 2024-10-15ZHEJIANG UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410696809.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The vacuum induction melting process has a slow solidification and crystallization speed inside large-sized ingots, resulting in coarse microstructure, severe element segregation, and deep shrinkage holes in the ingots, which affects the yield rate. The crucible is prone to oxidation and pollution, and the molten steel has poor desulfurization and dephosphorization capabilities, which limits its use. As the final smelting link for large alloy ingots.

Method used

Design a liquid-cooled mold for vacuum induction electrode casting, using spiral water pipes and helium filling into the air gap to adjust the cooling rate of the casting, change the heat transfer mode from radiation heat transfer to convection heat transfer, increase the solidification speed, and Through the combination of cooling water and helium, the mold structure is optimized to reduce shrinkage porosity and shrinkage cavities.

Benefits of technology

It achieves efficient sequential solidification, reduces shrinkage porosity and shrinkage cavities of the ingot, improves casting quality, simplifies the subsequent demoulding process, and facilitates the production of high-quality large steel ingots.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768550A_ABST
    Figure CN118768550A_ABST
Patent Text Reader

Abstract

The invention relates to a vacuum induction electrode casting liquid cooling mold, a design method and application thereof. A base is arranged at the bottom of a matched mold, and a riser is formed in the top of the matched mold; a water pipeline is arranged on the inner wall of the matched mold, and a water inlet passage and a water outlet passage are respectively arranged on the mold matched with an opening of the water pipeline; defining a target casting, establishing and simplifying a thermal model in a casting mold filling process, calculating total heat absorbed by a mold and total heat of convective heat transfer of cooling water, setting a loss heat correction coefficient and a proportionality coefficient, and obtaining an optimal solution according to a casting modulus, a casting hot spot volume, a configuration cooling water volume and a mold modulus; molten steel is injected into the mold, the dead head is closed, liquid is guided into the mold from the water inlet channel at a preset speed, when the surface layer of the casting is solidified, helium is injected from the air gap at a preset speed, and the vacuum environment between the casting and the mold is destroyed. Cast ingot shrinkage porosity and shrinkage cavities are effectively reduced, and the heat transfer efficiency and the solidification speed are improved; large steel ingots with excellent casting quality are simply and effectively produced, and demolding is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal casting and casting of other materials using the same process or equipment, and in particular to a vacuum induction electrode casting liquid cooling mold, a design method and an application thereof. Background Art

[0002] Vacuum induction melting (VIM) is the first technological process for the production of nickel-based high-temperature alloys. It uses alternating current to act on an induction coil under vacuum conditions to generate an alternating magnetic field. The alternating magnetic field induces alternating current "eddy current" on the charge. The charge is heated and melted by the "eddy current" and a series of physical and chemical reactions such as electromagnetic stirring, vacuum deoxidation, denitrogenation, dehydrogenation, volatilization of impurity elements, and control of the action between the melt and the crucible are used to smelt an alloy ingot with accurate chemical composition and high purity.

[0003] The VIM smelting process also has many shortcomings, mainly manifested as follows: (1) The solidification and crystallization rate inside the large-sized ingot is slow, which makes the microstructure of the alloy ingot coarse and the elements in different parts are seriously segregated; (2) The shrinkage cavity of the ingot is deep, which affects the yield rate; (3) The crucible is prone to oxidation after steelmaking, which pollutes the alloy; (4) The alloy melt reacts with the refractory material of the crucible, causing secondary pollution; (5) The ability of molten steel to directly desulfurize and dephosphorize is poor.

[0004] In general, due to the influence of solidification defects and the limitation of impurity removal ability, VIM cannot be used as the final smelting link of large alloy ingots, but it can efficiently purify molten steel and control the initial alloy element content to the greatest extent. Therefore, at present, high-quality medium and large IN718 alloys use VIM as the first smelting process without exception, and use VIM ingots as electrode ingots for secondary smelting. In on-site casting, the electrode ingots obtained in the vacuum induction link have many problems such as large shrinkage and shrinkage cavities and element segregation. Since the ingots often need to be used as electrode rods in the subsequent vacuum consumable link, the defects of the ingots will affect the process quality of the subsequent links.

[0005] Therefore, there is an urgent need to redesign the casting mold and heat transfer control method. Summary of the invention

[0006] The invention solves the problems existing in the prior art and provides a vacuum induction electrode casting liquid cooling mold, a design method and an application thereof.

[0007] The technical solution adopted by the present invention is a vacuum induction electrode casting liquid cooling mold, including a mold, a base is provided at the bottom of the mold, and a riser is provided at the top of the mold; a water pipeline is arranged on the inner wall of the mold, and a water inlet passage and a water outlet passage are respectively provided on the mold to cooperate with the opening of the water pipeline.

[0008] Preferably, the water pipeline is a spiral water pipeline, the water inlet passage is arranged corresponding to the opening of the spiral water pipeline at the bottom of the mold, and the water outlet passage is arranged corresponding to the opening of the spiral water pipeline at the top of the mold.

[0009] Preferably, the pitch of the spiral water pipeline gradually increases from bottom to top.

[0010] Preferably, the thread diameter of the spiral water pipeline gradually increases from bottom to top.

[0011] Preferably, the mold is a hollow frustum, and the outer diameter of the mold gradually increases from top to bottom.

[0012] Preferably, a plurality of hanging parts are distributed on the outer wall of the mold.

[0013] Preferably, a bottom pad brick is provided in conjunction with the base, and the bottom pad brick is embedded in the top of the base.

[0014] Preferably, a concave surface is provided on the top of the bottom pad brick facing downwards, and the outer edge of the concave surface is disposed under the outer wall of the mold.

[0015] A method for designing a vacuum induction electrode casting liquid cooling mold, the method comprising the following steps:

[0016] S1 defines the target casting according to The casting modulus M, the mold constant B, n is a constant, V represents the casting volume, and A represents the surface area of ​​the casting in contact with the mold;

[0017] S2 establishes the thermal model of the casting filling process, Q c =ρ c V c (cLiquidΔTLiquid+cSolidΔTSolid+L), where ρ c is the density of the molten metal, V c is the casting volume, c 液 and c 固 are the constant pressure specific heat capacity of liquid alloy and solid alloy, ΔT 液 is the difference between the pouring temperature and the solidification temperature, ΔT 固 is the temperature difference from solidification temperature to casting mold, L is the latent heat of melting per unit mass;

[0018] Simplified Q c Q c =ρ c Vc (C c ΔT c +L), where C c is the average value of the specific heat capacity of liquid alloy and solid alloy at constant pressure, ΔT c It is the difference between pouring temperature and mold temperature;

[0019] S3 calculates the total heat Q absorbed by the mold m And the total heat of cooling water heat exchange Q cw ,

[0020] Q m =c m ρ m V m ΔT m

[0021] Q cw =c cw ρ cw V cw ΔT cw

[0022] Among them, c m is the specific heat capacity of the mold, ρ m is the density of the mold, V m is the mold volume, ΔT m is the difference between the maximum temperature and the initial temperature of the mold wall, c cw is the specific heat capacity of cooling water, ρ cw is the density of cooling water, V cw is the volume of cooling water required, ΔT cw is the water temperature difference at the pipe openings of the water inlet and outlet;

[0023] S4 is based on A represents the surface area of ​​the casting in contact with the mold, M represents the surface area of ​​the casting in contact with the mold. c 、M m Denoting the modulus of the casting and the mold, we obtain,

[0024]

[0025] Let the heat loss correction factor k1 satisfy k1Q c =Q m =Q cw ,get,

[0026]

[0027] Let the proportionality coefficient k2 satisfy V m =k2V c ,get,

[0028]

[0029] S5 obtains that the volume of cooling water is proportional to the casting modulus and the volume of the casting hot spot where the cooling water acts, and inversely proportional to the mold modulus; the larger the casting hot spot, the greater the required cooling amount, and the thicker the mold, the smaller the corresponding cooling water amount; according to the casting modulus and the volume of the casting hot spot, the cooling water volume and mold modulus are configured to obtain the optimal solution.

[0030] An application of the vacuum induction electrode casting liquid cooling mold is to inject molten steel into the mold, close the riser, and introduce liquid into the mold at a preset speed from the water inlet passage. When the surface layer of the casting solidifies, helium is filled into the air gap at a preset rate to destroy the vacuum environment between the casting and the mold.

[0031] The invention relates to a vacuum induction electrode casting liquid cooling mold, a design method and an application thereof, comprising a mold, wherein a base is provided at the bottom of the mold, and a riser is provided at the top of the mold; a water pipeline is arranged on the inner wall of the mold, and a water inlet passage and a water outlet passage are respectively provided on the mold in cooperation with the opening of the water pipeline; in the design, a target casting is defined, a thermal model of the casting filling process is established and simplified, the total heat absorbed by the mold and the total heat of the cooling water convection heat transfer are calculated, a loss heat correction coefficient and a proportional coefficient are set, and the cooling water volume and the mold modulus are configured according to the casting modulus and the volume of the casting hot node to obtain an optimal solution; the mold is used to inject molten steel into the mold, close the riser, introduce liquid into the mold from the water inlet passage at a preset speed, and when the surface layer of the casting solidifies, helium is filled into the air gap at a preset rate to destroy the vacuum environment between the casting and the mold.

[0032] The beneficial effects of the present invention are that the mold can achieve efficient and orderly adjustment of the cooling rate of the steel ingot at each part of the electrode mold, realize sequential solidification, effectively reduce the shrinkage and shrinkage cavity of the ingot, and the heat transfer mode of the steel ingot during the solidification process can be changed from radiation heat transfer to convection heat transfer by filling the air gap with helium, so as to improve the heat transfer efficiency and the solidification speed; it can simply and effectively produce large steel ingots with excellent casting quality, which is convenient for subsequent demolding. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the main view structure of the present invention;

[0034] Figure 2 for Figure 1 AA section view structural diagram;

[0035] Figure 3 It is a schematic diagram of the three-dimensional structure of the present invention;

[0036] Figure 4 It is a perspective structural schematic diagram of the mold of the present invention. DETAILED DESCRIPTION

[0037] The present invention is further described in detail below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto.

[0038] The present invention relates to a vacuum induction electrode casting liquid cooling mold, comprising a mold 1, a base 2 is provided at the bottom of the mold 1, and a riser 3 is provided at the top of the mold 1; a water pipeline 4 is arranged on the inner wall of the mold 1, and a water inlet passage 5 and a water outlet passage 6 are respectively provided on the mold to cooperate with the opening of the water pipeline 4.

[0039] The water pipeline 4 is a spiral water pipeline 4 , the water inlet passage 5 is arranged corresponding to the opening of the spiral water pipeline 4 at the bottom of the mold 1 , and the water outlet passage 6 is arranged corresponding to the opening of the spiral water pipeline 4 at the top of the mold 1 .

[0040] In the present invention, a spiral water pipe 4 is provided for water flow to pass through, cooling water is introduced through a water inlet passage 5 at the bottom of the mold 1, and is transported toward a water outlet passage 6 via the spiral water pipe. Effective cooling control is achieved by controlling the transport parameters of the cooling water passing through the spiral water pipe.

[0041] In the present invention, the mold 1 is arranged on the base 2 in an interlocking manner so as to be tightly fixed.

[0042] In the present invention, the water inlet passage 5 is generally located at the lower part of the mold 1 and the water outlet passage 6 is located at the upper part of the mold 1. The height range covered by the two is the cavity of the mold 1 or larger, so that it has a better liquid cooling effect; obviously, the openings of the water inlet passage 5 and the water outlet passage 6 are both located on the outer wall of the mold 1.

[0043] The pitch of the spiral water pipeline 4 gradually increases from bottom to top.

[0044] The thread diameter of the spiral water pipe 4 gradually increases from bottom to top.

[0045] The mold 1 is a hollow truncated cone, and the outer diameter of the mold 1 gradually increases from top to bottom.

[0046] In the present invention, the pitch of the spiral water pipeline 4 is gradually lengthened from bottom to top, and the thread diameter is also gradually increased from bottom to top, so that the volume of cooling water decreases from bottom to top, and the distance between the inner wall of the cavity and the liquid cooling condition increases from bottom to top. The stability of the mold 1 cavity is reduced from bottom to top due to the influence of liquid cooling, and the interface temperature difference decreases from bottom to top, so that the interface heat transfer coefficient decreases from bottom to top. Therefore, the solidification rate of the steel ingot in the mold 1 is controlled and adjusted with a gentle heat transfer change, and the cooling rate is controlled to achieve sequential solidification of the molten steel; under the structural limitation of this spiral water pipeline 4, the overall structure of the mold 1 is a hollow truncated cone, that is, the inner diameter of its internal cavity gradually increases from top to bottom; the structure of the cavity here is also conducive to the subsequent demolding step.

[0047] A plurality of hanging parts 7 are distributed on the outer wall of the mold 1 .

[0048] In the present invention, the hangers 7 are used to lift the mold 1 as a whole, and can also play the role of a counterweight. They are arranged in groups and in an even number, generally 4, that is, one group of hangers 7 is arranged at the same horizontal height on the upper part of the mold 1 in a symmetrical position with respect to the central axis of the mold 1, and the other group of hangers 7 is arranged at the same horizontal height on the lower part of the mold 1 in a symmetrical position with respect to the central axis of the mold 1, so as to achieve overall balance.

[0049] A bottom pad brick 8 is provided in conjunction with the base 2 , and the bottom pad brick 8 is embedded in the top of the base 2 .

[0050] The top of the bottom pad brick 8 is provided with a concave surface facing downwards, and the outer edge of the concave surface is disposed under the outer wall of the mold 1 .

[0051] In the present invention, in actual application, the bottom pad brick 8 is bowl-shaped and presents a concave surface. The top (edge) of the concave surface is against the mold 1, and the diameter of the bottom pad brick 8 is slightly larger than the diameter of the mold cavity. The setting of the bottom pad brick 8 here can avoid direct contact between the molten steel and the base 2, thereby extending the life of the base 2.

[0052] The present invention also relates to a design method for the vacuum induction electrode casting liquid cooling mold, which is analyzed in combination with the following steps.

[0053] S1 defines the target casting according to The casting modulus M, the casting constant B, n is a constant, V represents the casting volume, and A represents the surface area of ​​the casting in contact with the mold 1;

[0054] The relationship between the solidification time and the casting modulus of a simple casting satisfies equation (1):

[0055] t=BM n (1)

[0056] Where t is the solidification time in seconds, M is the casting modulus, n is a constant, usually 1.2 to 2, and B is the casting constant, which is related to the casting and mold material and satisfies formula (2).

[0057]

[0058] Where, T m T0 and T1 are the temperature at which the alloy begins to solidify and the initial temperature of mold 1, in K, respectively. c is the density of the molten metal, in kg / m 3 , L is the latent heat of melting per unit mass, in J / kg, k is the thermal conductivity of mold 1, in W / (m·K), c and c mare the constant-pressure specific heat capacities of mold 1 and metal, respectively, in J / (kg·K); ΔTliquid is the difference between the pouring temperature and the solidification temperature, in K; ρ is the density of mold 1, in kg / m3.

[0059] It can be seen from equations (1) and (2) that the solidification time t is not only related to the casting modulus, but also to the initial temperature T0 of mold 1. In the process of mass production, in order to ensure the stability of casting quality, it is necessary to ensure that the initial production conditions and solidification state of each casting are consistent, that is, the initial temperature of mold 1 and the solidification time of the casting should be equal. The main factor affecting the solidification time is the hot spot. Therefore, it is necessary to study the relationship between the modulus at the hot spot of the casting and the amount of cooling water.

[0060] The filling, solidification and cooling processes of castings are all accompanied by heat transfer, and the heat value can be calculated with the help of heat transfer principles.

[0061] S2 establishes a thermal model of the casting filling process, satisfying equation (3),

[0062] Q c =ρ c V c (cLiquidΔTLiquid+cSolidΔTSolid+L) (3)

[0063] Among them, ρ c is the density of the molten metal, V c is the casting volume, unit: m 3 , c 液 and c 固 are the constant pressure specific heat capacities of liquid alloy and solid alloy respectively, in J / (kg·K), ΔT liquid is the difference between the pouring temperature and the solidification temperature, in K, ΔT 固 is the temperature difference from the solidification temperature to the casting mold, in K, L is the latent heat of melting per unit mass, in J / kg;

[0064] Simplified Q c is formula (4),

[0065] Q c =ρ c V c (C c ΔT c +L) (4)

[0066] Among them, C c is the average value of the specific heat capacity of liquid alloy and solid alloy at constant pressure, in J / (kg·K), ΔT c It is the difference between pouring temperature and mold temperature, unit is K;

[0067] Most of the heat released by the alloy liquid is absorbed by the mold 1, so the heat transferred to the mold 1 can be calculated by the temperature change of the casting mold.

[0068] S3 uses equations (5) and (6) to calculate the total heat Q absorbed by mold 1 m And the total heat of cooling water heat exchange Q cw ,

[0069] Q m =c m ρ m V m ΔT m (5)

[0070] Q cw =c cw ρ cw V cw ΔT cw (6)

[0071] Among them, c m is the specific heat capacity of mold 1, in J / (kg·K), ρ m is the density of mold 1, in kg / m 3 , V m The volume of mold 1, in m 3 , ΔT m The difference between the maximum temperature and the initial temperature of the mold 1 wall, unit K, c cw is the specific heat capacity of cooling water, in J / (kg·K), ρ cw is the density of cooling water, in kg / m 3 , V cw is the volume of cooling water required, in m 3 , ΔT cw is the water temperature difference at the pipe openings of the water inlet passage 5 and the water outlet passage 6, in K;

[0072] S4 is based on A represents the surface area of ​​the casting in contact with the mold 1, M represents c 、M m Denoting the modulus of the casting and the mold, we obtain,

[0073]

[0074] Since mold 1 will naturally dissipate some heat to the outside while absorbing the heat released by the alloy liquid, this part of the lost heat is corrected by the empirical coefficient k1. The corrected total heat is equal to the heat absorbed by mold 1, that is, the heat required for water cooling, so that the lost heat correction coefficient k1 is satisfied.

[0075] QUR c =Q m =Q cw (8)

[0076] Substituting equations (4) to (7) into equation (8) yields equation (9):

[0077]

[0078] The wall thickness of mold 1 is determined based on the range of the heat-affected zone of the alloy liquid on the cavity. When the wall thickness of mold 1 increases to the maximum value of the heat-affected zone of the casting hot node, even if the wall thickness is increased, the solidification state of the casting will not be changed. Therefore, the proportional coefficient k2 is used to calculate the volume of the casting hot node and the volume of mold 1 corresponding to the economic wall thickness, so that the proportional coefficient k2 satisfies.

[0079] V m =k2V c (10)

[0080] We get formula (11):

[0081]

[0082] S5 obtains that the volume of cooling water is proportional to the casting modulus and the volume of the casting hot spot where the cooling water acts, and inversely proportional to the modulus of mold 1; the larger the casting hot spot, the greater the required cooling amount, and the thicker the mold 1, the smaller the corresponding cooling water amount; according to the casting modulus and the volume of the casting hot spot, the cooling water volume and the mold 1 modulus are configured to obtain the optimal solution.

[0083] According to the heat flux formula:

[0084]

[0085] In the formula, q is the heat flux density; : is the thermal conductivity of mold 1; Δ; is the temperature difference between the casting surface and the water-cooling surface of mold 1; < is the thickness between the casting surface and the water-cooling surface of mold 1.

[0086] It can be seen from the formula that the thickness of the casting surface and the water-cooled surface of mold 1 will affect the heat transfer of mold 1. A larger material thickness will hinder the conduction of heat, thereby reducing the heat flux density. In order to achieve sequential solidification of the casting, the diameter of the designed water pipe layout increases from bottom to top, so that the heat flux density decreases from bottom to top.

[0087] The constant parameters of water at 10℃, 15℃, and 20℃ are as follows:

[0088]

[0089] h=Nμ: / A

[0090]

[0091]

[0092] J K =μ / R

[0093] Where, h is the heat transfer coefficient between cooling water and mold 1; Nμ is the Noor index; Re is the Reynolds number; : is the heat transfer coefficient of water; Pr is the Planck constant; ρ is the density of water; u m is the average water flow velocity of the cross section; v is the kinematic viscosity; D is the diameter of the cooling water pipe; μ is the dynamic viscosity; a is the thermal conductivity.

[0094] In order to ensure that the heat transfer coefficient between the cooling water and the mold 1 is about 4000W / (m2·K), and to ensure the cooling effect, the cooling water flow effect should be turbulent, that is, the Reynolds number Re should be ≥10000, and the cooling water temperature is calculated at 20℃.

[0095] Give a specific example;

[0096] The basic dimensions of the currently designed mold 1 are HT200 gray cast iron hollow truncated cones with a height of 3250mm and a wall thickness of 140mm; the maximum outer contour dimensions of the cast casting are Φ420mm×3250mm, which is a large casting; the designed water pipe diameter is The flow rate is preset to 1m / s;

[0097] After calculation, the Reynolds number Re is about 19880, the Noor index Nμ is about 137.7, and the heat transfer coefficient is about 4124W / (m2·K), which meets the required requirements;

[0098] Riser feeding distance refers to the distance that riser 3 provides feeding effect to the feeding zone at the end of the casting during the solidification process of the casting. The effective feeding distance usually refers to the sum of the length of the feeding zone at the end of the casting and the feeding zone of riser 3 during the solidification process of the casting. For rod-shaped parts, the effective feeding distance is 25 to 30 times the square root of the thickness of the casting.

[0099] The casting is a rod-shaped casting with an upper diameter of 420mm, a lower diameter of 430mm, and a height of 3250mm. The upper 300mm is the riser 3 area. According to the formula, the shrinkage compensation distance of riser 3 is about 513-615mm. To ensure the casting quality, the minimum value of 500mm can be taken. To reduce the processing technology, the sequential solidification of the casting in this area can be achieved by the shrinkage compensation effect of riser 3, and the bottom of the water pipe layout area can be determined to be 2450mm.

[0100] The mold liquid cooling system mainly involves the determination of the following parameters: the diameter of the cooling water pipe, the distance between the water pipes, and the distance between the water pipe and the horizontal wall and side wall of the mold 1;

[0101] According to the principle of opening the cooling system, the distance between pipes is generally (2.5-4)D. In this embodiment, the distance between the bottom water pipes is 50mm, and the pitch of the spiral water pipe 4 increases by 1.5D, i.e. 30mm, for each turn. After 12 turns, the predetermined water pipe layout area is reached;

[0102] The distance from the cooling water channel to the cavity surface should not be too close or too far, generally (1.5~2.5)D. In this embodiment, the center distance of the bottom water pipe is 500mm, the distance from the cooling water channel to the cavity surface is 30mm, and the inner diameter of the spiral water pipe 4 increases by 3mm each turn. After 12 turns, it reaches the predetermined water pipe layout area.

[0103] In the present invention, since the mold 1 is a hollow truncated cone structure, its initial modulus condition is small at the top and large at the bottom, which is not conducive to sequential solidification. For the target casting, the electrode ingot of IN718 alloy is used to improve the quality of the electrode ingot and reduce shrinkage and shrinkage cavities. By controlling the target liquid cooling conditions, sequential solidification of the molten steel can be achieved.

[0104] The present invention also relates to an application of the vacuum induction electrode casting liquid cooling mold, which is used to inject molten steel into the mold 1, close the riser 3, and introduce liquid into the mold 1 at a preset speed from the water inlet passage 5. When the surface layer of the casting solidifies, helium is filled into the air gap at a preset rate to destroy the vacuum environment between the casting and the mold 1.

[0105] In the present invention, it has been widely verified that the increase of air gap has a weakening effect on the interface heat transfer coefficient. The heat transfer coefficient reaches the maximum value just before the air gap is generated. When the air gap begins to be generated, the heat transfer coefficient decreases rapidly. Later, as the air gap continues to increase, the rate of decrease of the heat transfer coefficient becomes slow and tends to be stable. In addition to the size of the air gap, the thermal properties of the gas in the air gap also have a great influence on the interface heat transfer coefficient. Helium is the only substance that cannot solidify under standard atmospheric pressure, and its chemical properties are very stable. It has the highest thermal conductivity and is very suitable as a gas medium for breaking vacuum in this application; the air gap refers to the gap between the casting and the inner wall of the mold 1 during the solidification process. In the actual operation process, helium is injected into the entire operation cabin and penetrates into the air gap between the casting and the mold 1 to complete the operation. This is easy for technicians in this field to understand.

[0106] The present invention provides an embodiment, in which molten steel is injected into the mold 1, the riser 3 is closed, and a 20°C liquid is introduced into the mold 1 from the water inlet passage 5 at a speed of 1 m / s. When the surface layer of the casting solidifies, helium is filled into the air gap at a rate of 50 ml / min to destroy the vacuum environment between the casting and the mold 1.

[0107] In the present invention, the application of the electrode mold involves the design of the solidification cooling method. The water pipeline 4 is used to cool the electrode mold. The vacuum environment between the steel ingot cooling and solidifying casting and the mold 1 is broken by filling helium into the air gap, so that the radiation heat exchange is converted into convection heat exchange, thereby accelerating the solidification rate.

[0108] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0109] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A vacuum induction electrode casting liquid cooling mold, comprising a mold, characterized in that: A base is provided at the bottom of the mold, and a riser is provided at the top of the mold; a water pipeline is arranged on the inner wall of the mold, and a water inlet passage and a water outlet passage are respectively provided on the mold to match the opening of the water pipeline.

2. A vacuum induction electrode casting liquid cooling mold according to claim 1, characterized in that: The water pipeline is a spiral water pipeline, the water inlet passage is arranged corresponding to the opening of the spiral water pipeline at the bottom of the mold, and the water outlet passage is arranged corresponding to the opening of the spiral water pipeline at the top of the mold.

3. A vacuum induction electrode casting liquid cooling mold according to claim 2, characterized in that: The pitch of the spiral water pipeline increases gradually from bottom to top.

4. A vacuum induction electrode casting liquid cooling mold according to claim 3, characterized in that: The thread diameter of the spiral water pipeline gradually increases from bottom to top.

5. A vacuum induction electrode casting liquid cooling mold according to claim 4, characterized in that: The mold is a hollow truncated cone, and the outer diameter of the mold increases gradually from top to bottom.

6. The vacuum induction electrode casting liquid cooling mold according to claim 1, characterized in that: A plurality of hanging parts are distributed on the outer wall of the mold.

7. The vacuum induction electrode casting liquid cooling mold according to claim 1, characterized in that: A bottom pad brick is provided in conjunction with the base, and the bottom pad brick is embedded in the top of the base.

8. A vacuum induction electrode casting liquid cooling mold according to claim 7, characterized in that: The top of the bottom pad brick is provided with a concave surface facing downwards, and the outer edge of the concave surface is abutted against the outer wall of the mold.

9. A method for designing a liquid-cooled mold for vacuum induction electrode casting according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: S1 defines the target casting according to The casting modulus M, the mold constant B, n is a constant, V represents the casting volume, A represents the surface area of ​​the casting in contact with the mold; S2 establishes a thermal model of the casting filling process, Q c =ρ c V c (cLiquidΔTLiquid+cSolidΔTSolid+L), where ρ c is the density of the molten metal, V c is the casting volume, c 液 and c 固 are the constant pressure specific heat capacity of liquid alloy and solid alloy, ΔT 液 is the difference between the pouring temperature and the solidification temperature, ΔT 固 is the temperature difference from the solidification temperature to the casting mold, L is the latent heat of melting per unit mass; simplified Q c Q c =ρ c V c (C c ΔT c +L), where C c is the average value of the specific heat capacity of liquid alloy and solid alloy at constant pressure, ΔT c It is the difference between pouring temperature and mold temperature; S3 calculates the total heat Q absorbed by the mold m And the total heat of cooling water heat exchange Q cw , Q m =c m ρ m 5 m ΔT m Q cw =c cw ρ cw 5 cw ΔT cw Among them, c m is the specific heat capacity of the mold, ρ m is the density of the mold, V m is the mold volume, ΔT m is the difference between the maximum temperature and the initial temperature of the mold wall, c cw is the specific heat capacity of cooling water, ρ cw is the density of cooling water, V cw is the volume of cooling water required, ΔT cw is the water temperature difference at the pipe openings of the water inlet and outlet; S4 is based on A represents the surface area of ​​the casting in contact with the mold, M represents the surface area of ​​the casting in contact with the mold. c 、M m Denoting the modulus of the casting and the mold, we obtain, Let the heat loss correction factor k1 satisfy k1Q c =Q m =Q cw ,get, Let the proportionality coefficient k2 satisfy V m =k2V c ,get, S5 obtains that the volume of cooling water is proportional to the casting modulus and the volume of the casting hot spot where the cooling water acts, and inversely proportional to the mold modulus; the larger the casting hot spot, the greater the required cooling amount, and the thicker the mold, the smaller the corresponding cooling water amount; according to the casting modulus and the volume of the casting hot spot, the cooling water volume and mold modulus are configured to obtain the optimal solution.

10. An application of a liquid-cooled mold for vacuum induction electrode casting according to any one of claims 1 to 8, characterized in that: It is used to inject molten steel into the mold, close the riser, and introduce liquid into the mold at a preset speed from the water inlet channel. When the surface of the casting solidifies, helium is filled into the air gap at a preset rate to destroy the vacuum environment between the casting and the mold.

Citation Information

Cited By

  • Casting device for forging lining plate

    CN119387573A