Polishing method for large-caliber monopotassium phosphate crystal element
Through the combined use of hard metal synthetic polishing discs and oil-based polishing fluids, combined with vacuum adsorption pads and UV light stripping technology, the problem of surface shape accuracy control of large-diameter potassium dihydrogen phosphate crystal components is solved, and efficient surface shape is achieved. ization and stability improvement.
Patent Information
- Application Number
- CN202411128475.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-16
AI Technical Summary
It is difficult to achieve rapid convergence of surface shape accuracy and efficient processing of large-diameter potassium dihydrogen phosphate crystal components with existing technology. Especially when processing large-diameter ultra-thin crystal components, the clamping deformation of diamond flying cutting limits the control of flatness. Other polishing methods are not efficient enough.
Full-bore polishing using a hard metal synthetic polishing disc, combined with oil-based polishing fluid and vacuum adsorption pads, gradually improving the flatness of the crystal element through rapid and precise polishing steps, using UV light to peel off the tape to achieve non-destructive processing, and using displacement compensation turning and abrasive-free polishing further improve precision and efficiency.
It achieves full surface planarization of large-diameter crystal components, with a processing accuracy of less than 2 μm, improves processing efficiency and process stability, and is suitable for polishing large-diameter potassium dihydrogen phosphate crystal components that are easily hydrolyzable.
Smart Images

Figure CN118769032A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optical manufacturing, and in particular to a polishing method for a large-caliber potassium dihydrogen phosphate crystal element. Background Art
[0002] Functional crystal materials can realize the interaction and mutual conversion of energy forms such as electricity, magnetism, sound, light, force, and heat. They are a core material in the field of optoelectronics and are increasingly widely used in various fields. With the rapid development of optical technology, higher and higher requirements are placed on the processing quality and efficiency of functional crystal optical components. Nonlinear laser materials represented by potassium dihydrogen phosphate crystals (including KDP crystals, DKDP crystals, CLBO crystals, etc.) have material properties such as soft and brittle, easy to hydrolyze, and anisotropic, and are extremely difficult to process.
[0003] The existing high-power laser device mainly uses diamond flycutting for finishing of large-diameter ultra-thin potassium dihydrogen phosphate crystal components. However, diamond flycutting is limited by the deformation of clamping, and it is difficult to control the accuracy of crystal flatness. Other polishing methods have insufficient processing efficiency for large-diameter components and are applicable to small sizes. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a polishing method for a large-caliber potassium dihydrogen phosphate crystal element which can achieve rapid convergence of crystal surface accuracy.
[0005] The technical solution adopted by the present invention to solve the technical problem is: a polishing method for a large-caliber potassium dihydrogen phosphate crystal element, the method comprising the following steps:
[0006] 1) Prepare oil-based polishing liquid;
[0007] 2) A vacuum adsorption pad is attached to the surface of a substrate of the same size as the crystal element;
[0008] 3) A photosensitive adhesive tape is pasted on the back of the crystal element, the crystal element is adsorbed on a vacuum adsorption pad, and the crystal element and the substrate are integrally mounted on the tooling of the machine tool;
[0009] 4) Rapidly polish the processing surface of the crystal element to improve the flatness to within 10 μm. The rapid polishing parameters are: rotation speed 15-20 rpm, processing pressure 800-1200 Pa, abrasive particle size ≥ 1 μm, and processing time 20-40 min;
[0010] 5) After the rapid polishing is completed, lift the workpiece disc, remove the crystal element and the substrate from the polishing disc, and use UV light to irradiate the tape so that the crystal element and the photosensitive tape can be peeled off without damage;
[0011] 6) Turn over the crystal element and quickly polish it to improve the double-sided flatness to within 10μm;
[0012] 7) The processed surface of the crystal element is precision polished to improve the flatness to 2 μm. The precision polishing parameters are: rotation speed 3-5 rpm, processing pressure 200-600 Pa, abrasive particle size 0.3-1 μm, and processing time 10-20 min.
[0013] Furthermore, after the above step 7), there is a step 8): repeating the above steps 3)-7) to perform secondary iterative processing.
[0014] Furthermore, after the above step 8), there is a step 9): using a brush to thoroughly clean the polishing disc, and after the polishing disc and the polishing liquid supply circuit are dry, using pure anhydrous oil to perform abrasive-free polishing to further remove abrasive particles and impurities embedded on the surface of the crystal element.
[0015] Furthermore, before the above step 1), there is another step: before polishing, the polishing disc is turned into a slightly convex parabola by using a displacement compensation turning method, and the shape error between the actual shape of the slightly convex parabola and the theoretical surface is controlled within 2 microns.
[0016] Furthermore, after turning, square grid grooves are formed on the surface of the polishing disc, and the groove spacing is less than 6 mm.
[0017] Furthermore, in step 1), the oil-based polishing liquid is prepared by polishing oil and abrasive in a ratio of 100:5 to 100:1, and 0.1% by mass of an abrasive dispersant is added, and the water content is controlled in the range of 50ppm to 1000ppm.
[0018] Furthermore, in step 2), the flatness of the substrate is better than 0.2 μm or better than one tenth of the target accuracy of the crystal element.
[0019] Furthermore, in step 3), there is a sub-millimeter gap between the crystal element and the stopper, and the front end of the stopper is processed into an arc shape, so that the crystal element can adaptively float and pressurize.
[0020] Furthermore, in step 7), a composite oil filtration system is configured during the polishing process, with a filtration accuracy better than 1 μm, and large particles of impurities and moisture are filtered simultaneously.
[0021] Furthermore, the surface of the vacuum adsorption pad is grooved, and the polishing disc is a hard metal synthetic polishing disc.
[0022] The beneficial effects of the present invention are as follows: a full-aperture polishing method using a hard polishing disc is used to process a crystal element; during the polishing process, the entire surface of the crystal element is in contact with the polishing tool at the same time, so that the high points of the crystal element are subjected to great pressure, and material removal is relatively fast; the processing accuracy of the crystal element depends on the shape accuracy of the polishing disc, and rapid processing based on a rigid grinding method is achieved, the crystal surface shape accuracy converges rapidly, and finally the flattening of the entire surface is achieved; the flatness of a 300-600 mm aperture crystal element is better than 2 μm, and the processed surface shape is smooth, the processing efficiency is high, and the process stability is good; the crystal element can be widely used in the processing of optical elements of various specifications, and is particularly suitable for the polishing of large-aperture potassium dihydrogen phosphate-type easily hydrolyzed crystal elements. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a polishing schematic diagram of the present invention.
[0024] Figure 2 It is a schematic diagram of the flatness of the crystal element after polishing in Example 1.
[0025] Figure 3 It is a schematic diagram of the roughness of the crystal element after polishing in Example 1.
[0026] Figure 4 This is a schematic diagram of the initial flatness of the crystal element of Example 2.
[0027] Figure 5 It is a schematic diagram of the flatness of the crystal element after polishing in Example 2. DETAILED DESCRIPTION
[0028] like Figure 1 As shown, the adaptive polishing device adopted in the polishing method of large-caliber potassium dihydrogen phosphate crystals of the present invention includes a substrate 1, a workpiece disk 3, a connector 5, a stop hook 7, a stop block 8, a vacuum adsorption pad 10 and a polishing disk 12, wherein the upper end of the stop hook 7 is mounted on the workpiece disk 3 by screws, the stop block 8 is mounted on the lower end of the stop hook 7 by screws, the connector 5 is mounted at the center position of the workpiece disk 3 by screws, the crystal element 11 is arranged on the substrate 1 by the vacuum adsorption pad 10, the stop block 8 and the lower end of the stop hook 7 limit the position of the crystal element 11, the connector 5 is connected to the machine tool spindle, and the machine tool spindle drives the connector 5 to rotate during operation, thereby driving the workpiece disk and the crystal element 11 to complete the rotational motion.
[0029] It is best to use a flexible polytetrafluoroethylene block 8 as the above-mentioned block, and the front end of the block is processed into an arc shape to protect the side of the crystal element 11; the substrate 1 material can be made of high-quality aluminum with a thickness greater than 25 mm to maintain high structural rigidity and shape accuracy; the surface of the vacuum adsorption pad 10 is grooved so that the crystal element 11 and the vacuum adsorption pad 10 are in point contact, and the overall contact area is not greater than 40% to reduce the deformation of the crystal element 11; the polishing disk 12 uses a hard metal synthetic polishing disk; in order to increase the polishing pressure, a substrate connecting rod 4 and a weight plate can also be set, and multiple substrate connecting rods 4 pass through the workpiece disk 3 and are connected to the weight block.
[0030] The polishing method of large-caliber potassium dihydrogen phosphate crystals of the present invention comprises the following steps:
[0031] 1) Prepare oil-based polishing fluid: polishing oil and abrasive are prepared in a ratio of 100:5 to 100:1, and an abrasive dispersant with a mass fraction of about 0.1% is added. The abrasive dispersant can improve the suspension characteristics of the abrasive particles, and the water content is controlled in the range of 50ppm to 1000ppm. In precision polishing, a polishing fluid with a low water content and a fine-grained abrasive can be used; in rapid polishing, a polishing fluid with a high water content and a large-grained abrasive can be used to improve the reaction efficiency through micro-dissolution chemical action. Abrasives can generally be diamond, aluminum oxide, etc. The abrasive shape should be as spherical as possible to improve the quality of the processed surface;
[0032] 2) processing a substrate 1 of the same size as the crystal element 11, the flatness of the substrate 1 is better than 0.2 μm or better than one tenth of the target accuracy of the crystal element 11, and a layer of flexible vacuum adsorption pad 10 of the same thickness is attached to the surface of the substrate 1;
[0033] 3) Wipe both sides of the crystal element 11 to be processed with analytical grade organic solvents such as anhydrous ethanol, and stick a layer of photo-induced debonding protective tape on the back. Adsorb the crystal element 11 on the vacuum adsorption pad 10, and install the crystal element 11 and the substrate 1 as a whole on the tooling of the machine tool to achieve low-strain rapid clamping. There is a sub-millimeter gap between the crystal element 11 and the block 8, so that the crystal element 11 can adaptively float and be pressurized. The polishing pressure comes from the gravity of the crystal element 11 and the substrate 1. Each point of the crystal element 11 is evenly pressurized, and no edge collapse will occur during the processing;
[0034] 4) Rapidly polish the processed surface of the crystal element 11 to remove residual lines or deep defects from the previous stage and improve the flatness to within 10 μm. The rapid polishing parameters are: rotation speed 15-20 rpm, processing pressure 800-1200 Pa, abrasive particle size ≥ 1 μm, and processing time 20-40 min;
[0035] 5) After the rapid polishing is completed, lift the workpiece disk 3, remove the crystal element 11 and the substrate 1 as a whole from the polishing disk 12, and use UV light to irradiate the tape so that the crystal element 11 and the photosensitive tape are peeled off without damage, and then wipe the surface of the crystal element 11 with a soft and clean silk cloth;
[0036] 6) Turn over and quickly polish the crystal element 11 to improve the double-sided flatness to within 10 μm;
[0037] 7) Precision polishing is performed on the processing surface of the crystal element 11 to improve the flatness to about 2μm. The precision polishing parameters are: rotation speed 3-5rpm, processing pressure 200-600Pa, abrasive particle size 0.3-1μm, and processing time 10-20min. During the polishing process, a composite oil filtration system is configured with a filtration accuracy better than 1μm, which can simultaneously filter large particles of impurities and water;
[0038] 8) To improve the final processing accuracy, repeat the above steps 3)-7) to perform secondary iterative processing. Unlike conventional processing, no detection is required during the processing, the operation is simple, and the processing efficiency is high;
[0039] 9) Use a brush to thoroughly clean the polishing disc 12. After the polishing disc 12 and the polishing liquid supply circuit are dry, use pure anhydrous oil to perform abrasive-free polishing to further remove abrasive particles and impurities embedded on the surface of the crystal element 11 and improve the surface quality.
[0040] The present invention adopts a metal synthetic polishing disc as a polishing tool. Different from the flexible polishing pad of traditional optical processing, the polishing disc 12 is a rigid polishing tool. The processing accuracy of the crystal element 11 is mainly affected by the shape accuracy of the polishing disc 12, with high removal efficiency and less edge collapse effect. The polishing disc 12 will not deform during the processing, and the shape accuracy of the polishing tool can be maintained for a long time. The metal synthetic polishing disc has a low elastic modulus and a porosity of not less than 30%. The abrasive can be embedded in the polishing tool, which can not only allow the abrasive to be embedded in the polishing disc 12 to improve the removal efficiency, but also prevent the abrasive from pressing brittle cracks on the crystal element 11, and the processing surface quality is good. The metal synthetic polishing disc has oil resistance, which avoids the failure and degumming problems of traditional polyurethane, polishing cloth, asphalt disc, etc. under the erosion conditions of organic oil.
[0041] Before polishing, the present invention first uses a displacement compensation turning method to turn the polishing disk 12 to a specified shape, and combines non-contact precision detection of the polishing disk 12 to control the overall shape accuracy of the polishing disk 12 to within 2 microns. Then, an anhydrous polishing liquid is used to quickly polish the crystal element 11. By alternately turning over both sides, iterative convergence of the two large surfaces of the crystal element 11 can be achieved. In addition, the processing method has a large tolerance for the shape of the crystal entrance, and the processing process does not need to rely on precise detection of the crystal element 11.
[0042] In order to improve the precision convergence efficiency of the crystal element 11, the shape of the polishing disc 12 is preferably a micro-convex parabola, and the shape error between the actual shape of the micro-convex parabola and the theoretical curved surface is controlled within 2 microns. After turning, the surface of the polishing disc 12 is opened with square grooves, and the groove spacing is less than 6mm, which can improve the conveying capacity of the abrasive and reduce the non-uniform characteristics of the material removal. After a certain period of use, the polishing disc 12 needs to be turned again to remove the surface passivation layer, improve the processing efficiency, and restore the contour shape and surface processing characteristics.
[0043] Embodiment 1:
[0044] 1) Installing a synthetic tin polishing disc on a machine tool spindle, wherein the porosity of the polishing disc material is ≥30%, and the radius of the polishing disc 12 is equivalent to the caliber of the crystal element 11; combining non-contact precision detection of the polishing disc 12, a displacement compensation turning method is used to turn the polishing disc 12 into a convex parabola, wherein the difference between the high and low point height values of the parabola does not exceed 5 μm, and the shape error between the actual shape of the parabola and the theoretical curved surface is controlled within 2 microns; a 3mm diameter high-speed milling cutter is used for slotting, wherein the slot shape is a grid shape, the slot spacing is 6mm, and the slot depth is 5mm;
[0045] 2) Prepare oil-based polishing liquid: ① Polishing liquid for rapid polishing: polishing oil and abrasive are prepared in a ratio of 50:1, and abrasive dispersant with a mass fraction of 0.1% is processed, water content is 800ppm, and abrasive is 1μm aluminum oxide; ② Polishing liquid for precision polishing: polishing oil and abrasive are prepared in a ratio of 50:1, and abrasive dispersant with a mass fraction of 0.1% is processed, water content is 300ppm, and abrasive is 0.3μm aluminum oxide;
[0046] 3) Prepare an aluminum substrate 1 of 200 mm×200 mm×30 mm, the flatness of the substrate 1 is better than 0.1 μm, attach a vacuum adsorption pad 10 to the surface of the substrate 1, and grooves are cut on the surface of the vacuum adsorption pad 10 so that the vacuum adsorption pads 10 are evenly distributed in small squares;
[0047] 4) Roughly cut the 200mm×200mm×8mm crystal element 11 to be polished, the double-sided flatness of the crystal element 11 is less than 50μm, the double-sided of the crystal element 11 is wiped clean with anhydrous ethanol, and a layer of photo-induced debonding protective tape is pasted on the back. The crystal element 11 is adsorbed on the vacuum adsorption pad 10, and the crystal element 11 and the substrate 1 are integrally installed on the tooling of the machine tool, with a gap of 0.5mm between the crystal element 11 and the flexible polytetrafluoroethylene block 8, so that the crystal element 11 can be floated and pressurized;
[0048] 5) A weight block is installed on the lower surface of the workpiece disk 3. When the workpiece disk 3 descends, the weight block first slowly presses on the substrate 1, and then further descends, so that the stopper 8 is substantially flush with the crystal element 11. At this time, the conical surface of the substrate connecting rod 4 is separated from the inner hole of the workpiece disk 3, that is, the weight block is completely pressed on the substrate 1 by gravity;
[0049] 6) Rapidly polish the machined surface to remove residual lines or deep defects from the previous stage and improve the flatness to within 10 μm. The rapid polishing parameters are: speed 15 rpm, processing pressure 800 Pa, polishing liquid supply flow 200 ml / min, and processing time 30 min;
[0050] 7) After the rapid polishing is completed, the workpiece plate 3 is lifted, and the workpiece plate 3 drives the substrate connecting rod 4 to rise by several centimeters. The conical surface of the substrate connecting rod 4 is stuck in the inner hole of the workpiece plate 3, and then drives the weight block to rise until it leaves the substrate 1;
[0051] 8) Remove the crystal element 11 and the substrate 1 as a whole from the polishing plate 12, irradiate the tape with UV light to make the crystal element 11 and the photosensitive tape peel off without damage, and then wipe the surface of the crystal element 11 with a soft clean silk cloth;
[0052] 9) Repeat the above steps 4)-8) to complete the rapid polishing of the reverse side of the crystal element 11, so that the double-sided flatness is improved to within 10 μm;
[0053] 10) Remove the weight block and place the crystal element 11 into the tooling according to step 4);
[0054] 11) Perform precision polishing on the machined surface to improve the flatness to about 2 μm. The precision polishing parameters are: rotation speed 3 rpm, processing pressure 200 Pa, polishing liquid supply flow rate 150 ml / min, and processing time 20 min;
[0055] 12) Repeat steps 10)-11) to perform precision polishing on the other side of the crystal element 11;
[0056] 13) After precision polishing is completed, pure anhydrous oil is used for non-abrasive polishing to remove abrasive particles and impurities embedded on the surface of the crystal element 11. During the polishing process, an oil filtration system is configured with a filtration accuracy better than 1μm, and large particles of impurities and water are filtered simultaneously. The polishing parameters are: speed 10rpm, processing pressure 200Pa, polishing liquid supply flow 250ml / min, processing time 5min;
[0057] 14) After the double-sided polishing is completed, wipe the surface of the crystal element 11 with a soft and clean silk cloth, and inspect the crystal element 11: the flatness PV of the crystal element 11 reaches 728nm. Figure 2 As shown, there are no obvious defects on the surface, and the roughness Ra is within 2nm. Figure 3 shown.
[0058] Embodiment 2:
[0059] 1) Installing a synthetic tin polishing disc on a machine tool spindle, wherein the porosity of the polishing disc material is ≥30%, and the radius of the polishing disc 12 is equivalent to the caliber of the crystal element 11; combining non-contact precision detection of the polishing disc 12, a displacement compensation turning method is used to turn the polishing disc 12 into a convex parabola, wherein the difference between the high and low point height values of the parabola does not exceed 6 μm, and the shape error between the actual shape of the parabola and the theoretical curved surface is controlled within 2 microns; using a 5 mm diameter high-speed milling cutter for slotting, the slot shape is a grid shape, the slot spacing is 5 mm, and the slot depth is 5 mm;
[0060] 2) Prepare oil-based polishing liquid: ① Polishing liquid for rapid polishing: polishing oil and abrasive are prepared in a ratio of 100:5, and abrasive dispersant with a mass fraction of 0.1%, water content of 800ppm, and abrasive of 2μm aluminum oxide. ② Polishing liquid for precision polishing: polishing oil and abrasive are prepared in a ratio of 50:1, and abrasive dispersant with a mass fraction of 0.1%, water content of 300ppm, and abrasive of 0.3μm aluminum oxide is prepared;
[0061] 3) Prepare an aluminum substrate 1 of 400 mm×400 mm×30 mm, the flatness of the substrate 1 is better than 0.1 μm, attach a vacuum adsorption pad 10 to the surface of the substrate 1, and grooves are made on the surface of the vacuum adsorption pad 10 so that the vacuum adsorption pads 10 are evenly distributed in small squares;
[0062] 4) Wipe both sides of the crystal element 11 with anhydrous ethanol and apply a layer of photo-induced debonding protective tape on the back. Adsorb the crystal element 11 on the vacuum adsorption pad 10, and install the crystal element 11 and the substrate 1 as a whole on the tooling of the machine tool. There is a 0.2mm gap between the crystal element 11 and the flexible polytetrafluoroethylene block 8, so that the crystal element 11 can be floated and pressurized;
[0063] 5) A weight block is installed on the lower surface of the workpiece disk 3. When the workpiece disk 3 descends, the weight block first slowly presses on the substrate 1, and then further descends, so that the stopper 8 is substantially flush with the crystal element 11. At this time, the conical surface of the substrate connecting rod 4 is separated from the inner hole of the workpiece disk 3, that is, the weight block is completely pressed on the substrate 1 by gravity;
[0064] 6) Rapidly polish the machined surface to remove residual lines or deep defects from the previous stage and improve the flatness to within 10 μm. The rapid polishing parameters are: speed 20 rpm, processing pressure 1100 Pa, polishing liquid supply flow 400 ml / min, and processing time 40 min;
[0065] 7) After the rapid polishing is completed, the workpiece plate 3 is lifted, and the workpiece plate 3 drives the substrate connecting rod 4 to rise by several centimeters. The conical surface of the substrate connecting rod 4 is stuck in the inner hole of the workpiece plate 3, and then drives the weight block to rise until it leaves the substrate 1;
[0066] 8) Remove the crystal element 11 and the substrate 1 as a whole from the polishing plate 12, irradiate the tape with UV light to make the crystal element 11 and the photosensitive tape peel off without damage, and then wipe the surface of the crystal element 11 with a soft clean silk cloth;
[0067] 9) Repeat the above steps 4)-8) to complete the rapid polishing of the reverse side of the crystal element 11, so that the double-sided flatness is improved to within 10 μm;
[0068] 10) Remove the weight block and place the crystal element 11 into the tooling according to step 4);
[0069] 11) Perform precision polishing on the machined surface to improve the flatness to about 2 μm. The precision polishing parameters are: rotation speed 5 rpm, processing pressure 300 Pa, polishing liquid supply flow rate 150 ml / min, and processing time 20 min;
[0070] 12) Repeat steps 10)-11) to perform precision polishing on the other side of the crystal element 11;
[0071] 13) After precision polishing is completed, pure anhydrous oil is used for non-abrasive polishing to remove abrasive particles and impurities embedded on the surface of the crystal element 11. During the polishing process, an oil filtration system is configured with a filtration accuracy better than 1μm, and large particles of impurities and water are filtered simultaneously. The polishing parameters are: speed 10rpm, processing pressure 200Pa, polishing liquid supply flow 250ml / min, processing time 5min;
[0072] 14) After polishing, clean the surface of the crystal element 11 with a soft and clean silk cloth, and inspect the crystal element 11: the initial flatness PV of the large-diameter crystal element 11 is about 20μm. Figure 4 As shown in Figure 2, the flatness PV value after processing converges to within 2 μm, as shown in Figure 2. Figure 5 shown.
Claims
1. A method for polishing a large-caliber potassium dihydrogen phosphate crystal element, characterized in that: The method comprises the following steps: 1) Prepare oil-based polishing liquid; 2) attaching a vacuum adsorption pad (10) to the surface of a substrate (1) having the same size as the crystal element (11); 3) affixing a light-induced debonding protective tape to the back of the crystal element (11), adsorbing the crystal element (11) onto a vacuum adsorption pad (10), and integrally mounting the crystal element (11) and the substrate (1) onto a tooling of a machine tool; 4) Rapidly polishing the processed surface of the crystal element (11) to improve the flatness to within 10 μm, the rapid polishing parameters are: rotation speed 15-20 rpm, processing pressure 800-1200 Pa, abrasive particle size ≥ 1 μm, processing time 20-40 min; 5) After the rapid polishing is completed, the workpiece disk (3) is lifted, the crystal element (11) and the substrate (1) are removed from the polishing disk (12), and the tape is irradiated with UV light to allow the crystal element (11) and the photosensitive tape to be peeled off without damage; 6) Turning over and quickly polishing the crystal element (11) to improve the double-sided flatness to within 10 μm; 7) Precision polishing is performed on the processed surface of the crystal element (11) to improve the flatness to 2 μm. The precision polishing parameters are: rotation speed 3-5 rpm, processing pressure 200-600 Pa, abrasive particle size 0.3-1 μm, and processing time 10-20 min.
2. The polishing method of large-diameter potassium dihydrogen phosphate crystal element according to claim 1, characterized in that: After the above step 7), there is a step 8): repeat the above steps 3)-7) to perform secondary iterative processing.
3. The polishing method of large-caliber potassium dihydrogen phosphate crystal element according to claim 2, characterized in that: After the above step 8), there is also a step 9): using a brush to thoroughly clean the polishing disc (12), and after the polishing disc (12) and the polishing liquid supply circuit are dried, using pure anhydrous oil to perform abrasive-free polishing to further remove abrasive particles and impurities embedded on the surface of the crystal element (11).
4. The polishing method of large-caliber potassium dihydrogen phosphate crystal element according to claim 1, characterized in that: Before the above step 1), there is a further step: before polishing, the polishing disc (12) is first turned into a micro-convex paraboloid by using a displacement compensation turning method, and the shape error between the actual shape of the micro-convex paraboloid and the theoretical curved surface is controlled within 2 microns.
5. The polishing method of large-caliber potassium dihydrogen phosphate crystal element according to claim 4, characterized in that: After turning, the surface of the polishing disc (12) is provided with square grooves, and the groove spacing is less than 6 mm.
6. The polishing method of large-caliber potassium dihydrogen phosphate crystal element according to claim 1, characterized in that: Step 1) The oil-based polishing liquid is prepared by polishing oil and abrasive in a ratio of 100:5 to 100:1, and 0.1% by mass of an abrasive dispersant is added, and the water content is controlled within the range of 50ppm to 1000ppm.
7. The polishing method of large-caliber potassium dihydrogen phosphate crystal element according to claim 1, characterized in that: Step 2) The flatness of the substrate (1) is better than 0.2 μm or better than one tenth of the target accuracy of the crystal element (11).
8. The polishing method of large-caliber potassium dihydrogen phosphate crystal element according to claim 1, characterized in that: Step 3) There is a sub-millimeter gap between the crystal element (11) and the stopper (8), and the front end of the stopper (8) is processed into an arc shape, so that the crystal element (11) can adaptively float and pressurize.
9. The polishing method of large-caliber potassium dihydrogen phosphate crystal element according to claim 1, characterized in that: Step 7) A composite oil filtration system is configured during the polishing process, with a filtration accuracy better than 1 μm, and large particles of impurities and moisture are filtered simultaneously.
10. The polishing method of large-diameter potassium dihydrogen phosphate crystal element according to claim 1, characterized in that: The surface of the vacuum adsorption pad (10) is grooved, and the polishing disc (12) is a hard metal synthetic polishing disc.
Citation Information
Patent Citations
Optical machining grinding and fly-cutting combined machine tool body
CN103802003A
Displacement compensation turning method for metal tin plate
CN109676155A
Ultra-hard grinding disc and correction disc for annular polishing machine
CN110509170A
Floating pressurizing clamping device used for fast polishing of optical element and method of floating pressurizing clamping device
CN111113201A
Ultra-precise efficient polishing device and method suitable for large-size KDP crystals
CN114378704A
Cited By
Preparation method of slotting-free polishing disc
CN119635526A