Production process of high-thickness low-temperature binder ceramic grinding wheel
Through the production process of high-thickness low-temperature bonded ceramic grinding wheels, the problems of hardness deviation and short service life of ceramic grinding wheels are solved, and efficient grinding, energy saving and environmental protection of ceramic grinding wheels are achieved. Small-sized grinding wheels are spliced to form large-sized grinding wheels, which reduces production costs. .
Patent Information
- Application Number
- CN202411026389.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-15
AI Technical Summary
The existing ceramic grinding wheel production process results in large hardness deviations of ceramic grinding wheels, inconsistent grinding quality, poor processing accuracy, and short service life.
The production process of high-thickness low-temperature bonded ceramic grinding wheels is adopted. By mixing the raw materials and adding low-temperature bonding agent and temporary bonding agent, ball milling and hot pressing are performed, and then sintered in a resistance furnace to form a ceramic grinding wheel with suitable hardness and toughness. And small-sized grinding wheels are spliced to form large-sized grinding wheels to reduce the scrap rate.
It improves the sharpness and service life of the ceramic grinding wheel, reduces the sintering temperature, has the advantages of energy saving and environmental protection, and realizes the convenient replacement of large-sized grinding wheels through the splicing of small-sized grinding wheels, reducing production costs.
Smart Images

Figure HDA0004968666320000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic grinding wheels, in particular to a production process of high-thickness low-temperature bonding agent ceramic grinding wheels. Background Art
[0002] Grinding wheels are an important part of the abrasive tool industry. The abrasive tool industry is becoming more and more important in mechanical production, and grinding wheels play an indispensable role. With the development of science and technology, new materials are growing, and mechanical processing is developing towards high quality, high precision, high efficiency, and automation. The application scope of ceramic grinding wheels is getting wider and wider, and the amount is increasing. However, the ceramic grinding wheels produced by the existing ceramic grinding wheel production process have large hardness deviations and uneven grinding quality, resulting in poor machining accuracy and short service life of ceramic grinding wheels. Therefore, we proposed a high-thickness low-temperature bond ceramic grinding wheel production process to solve the above-mentioned problems. Summary of the invention
[0003] The object of the present invention is to provide a production process for a high-thickness low-temperature bonded ceramic grinding wheel to solve the problems raised in the above-mentioned background technology.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] A production process for a high-thickness, low-temperature bonded vitrified grinding wheel comprises the following steps:
[0006] Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed;
[0007] Step 2: Add an appropriate amount of low-temperature binder raw material to the materials uniformly mixed in step 1, and place them in a ball mill to mix and grind them to form a uniform mixture;
[0008] Step 3: Fill the mixed material into the molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it;
[0009] Step 4: The dried ceramic grinding wheel is placed in a resistance furnace for sintering to give it the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacture of the ceramic grinding wheel;
[0010] Step 5: The manufactured ceramic grinding wheel uses a small-sized grinding wheel as the basic specification. The small-sized grinding wheel is used alone, or multiple small-sized grinding wheels are combined to form large-sized grinding wheels of different specifications for use. When the large-sized grinding wheel is partially damaged, the local small-sized grinding wheel can be replaced;
[0011] Or the ceramic grinding wheel can be directly formed into large size specifications for use at one time.
[0012] As a further solution of the present invention: in step 1, the raw materials are mixed and fully stirred by a mixer to ensure that the materials are evenly distributed. The raw materials include abrasives, temporary binders, and pore-forming agents. The abrasives include brown corundum abrasives, white corundum abrasives, and silicon carbide abrasives.
[0013] As a further solution of the present invention: in the step 2, an appropriate amount of low-temperature binder raw material is added to the material uniformly mixed in the step 1, and the material is placed in a ball mill for mixing and grinding to form a uniform mixture. The binder uses a ceramic binder composed of clay and feldspar borax.
[0014] As a further solution of the present invention: the temporary adhesive is polyvinyl alcohol.
[0015] As a further solution of the present invention: the pore-forming agent uses one or more organic substances selected from polytetrafluoroethylene, polyimide, and bismaleimide.
[0016] As a further solution of the present invention: in the step 2, an appropriate amount of binder raw material is added to the material uniformly mixed in the step 1, and the material is placed in a ball mill for mixing and grinding to form a uniform mixture, and the ball milling time is 65-90 minutes.
[0017] As a further solution of the present invention: in step three, the mixed material is filled into a molding mold, pressure is applied to preliminarily shape the material, and the molded grinding wheel is stored at room temperature for more than 48 hours to dry it. The hot pressing molding temperature is 330-350°C, the pressing pressure is 20-24MPa, and the pressing time is 75-90min.
[0018] As a further solution of the present invention: the ceramic grinding wheel dried in step 4 is placed in a resistance furnace for sintering to make it have the required hardness and toughness, and then the sintered grinding wheel is processed into a designed size to complete the manufacture of the ceramic grinding wheel. The sintering temperature is 750-900°C and the time is 18-25 hours.
[0019] As a further solution of the present invention: the ceramic grinding wheel is made of the following raw materials in mass fractions: abrasive: 45%-55%, binder: 25%-35%, temporary adhesive: 4%-6%, pore-forming agent: 13%-15%.
[0020] As a further solution of the present invention: the specification of the lower-sized grinding wheel manufactured in the step five is 600*200*305, the specification of the large-sized grinding wheel is 600*600*305 or 600*400*305, and the combination method of the small-sized grinding wheel is bonding, embedding or oblique splicing, wherein the oblique splicing is carried out after the grinding wheel is processed with an inclined surface.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] In the production process of high-thickness low-temperature bonded ceramic grinding wheels, the temporary binder can not only increase the strength of the semi-finished product, but also improve the sharpness of the prepared ceramic grinding wheel and increase the service life of the prepared ceramic grinding wheel; the binder can significantly reduce the sintering temperature of the prepared silicon carbide ceramic grinding wheel, so that the ceramic grinding wheel has suitable hardness, high grinding efficiency and long service life, can be fired at low temperature, and has the advantages of energy saving and environmental protection;
[0023] The present invention produces a small-sized grinding wheel as a basic specification, which can be used alone or by splicing multiple small-sized grinding wheels to form large-sized grinding wheels of different specifications, thereby reducing the problem of high scrap rate in direct production of large-sized grinding wheels. At the same time, the splicing of small-sized grinding wheels is also convenient for local replacement, thereby reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the production process of the high-thickness low-temperature bond ceramic grinding wheel of the present invention. DETAILED DESCRIPTION
[0025] Example 1
[0026] like Figure 1 As shown, a production process of a high-thickness low-temperature bonded ceramic grinding wheel comprises the following steps:
[0027] Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed;
[0028] Step 2: Add an appropriate amount of low-temperature binder raw material to the materials uniformly mixed in step 1, and place them in a ball mill to mix and grind them to form a uniform mixture;
[0029] Step 3: Fill the mixed material into the molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it;
[0030] Step 4: The dried ceramic grinding wheel is placed in a resistance furnace for sintering to give it the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacture of the ceramic grinding wheel;
[0031] Step 5: The manufactured ceramic grinding wheel uses a small-sized grinding wheel as the basic specification. The small-sized grinding wheel is used alone, or multiple small-sized grinding wheels are combined to form large-sized grinding wheels of different specifications for use. When the large-sized grinding wheel is partially damaged, the local small-sized grinding wheel can be replaced;
[0032] Or the ceramic grinding wheel can be directly formed into large size specifications for use at one time.
[0033] Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed. The raw materials include abrasives, temporary binders, and pore-forming agents. The abrasives include brown corundum abrasives, white corundum abrasives, and silicon carbide abrasives.
[0034] Step 2: Add an appropriate amount of low-temperature binder raw material to the material uniformly mixed in step 1, and place it in a ball mill for mixing and grinding to form a uniform mixture. The binder uses a ceramic binder composed of clay and feldspar borax; the temporary binder uses polyvinyl alcohol; the pore-forming agent uses one or more of polytetrafluoroethylene, polyimide, bismaleimide and various organic substances; Step 2: Add an appropriate amount of binder raw material to the material uniformly mixed in step 1, and place it in a ball mill for mixing and grinding to form a uniform mixture. The ball milling time is 65-90 minutes; Step 3: Fill the mixed material into a molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it. The molding method is hot pressing; Step 3: Fill the mixed material into a molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it. The temperature of hot pressing is 330-350°C, and the pressing pressure is 20-24MPa , the pressing time is 75-90min; in step 4, the dried ceramic grinding wheel is placed in a resistance furnace for sintering to give it the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacturing of the ceramic grinding wheel. The sintering temperature is 750°C and the time is 18-25 hours; the ceramic grinding wheel is made of the following raw materials by mass fraction: abrasive: 45%, binder: 25%, temporary binder: 4%, pore-forming agent: 13%; the specification of the lower size grinding wheel manufactured in step 5 is 600*200*3 05. The specifications of large-size grinding wheels are 600*600*305 or 600*400*305 or other specifications. The combination methods of small-size grinding wheels are bonding, inlaying or bevel splicing, etc., among which the bevel splicing should be carried out after the grinding wheel is processed with the bevel. If the large size 600*600*305 or 600*400*305 is directly formed, due to the use of proprietary low-temperature binder and organic temporary binder, the manufactured grinding wheel material has good fluidity, uniform structure, good hardness consistency, and cracks and imbalance problems in the product can be effectively controlled.
[0035] Example 2
[0036] like Figure 1 As shown, a production process of a high-thickness low-temperature bonded ceramic grinding wheel comprises the following steps:
[0037] Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed;
[0038] Step 2: Add an appropriate amount of low-temperature binder raw material to the materials uniformly mixed in step 1, and place them in a ball mill to mix and grind them to form a uniform mixture;
[0039] Step 3: Fill the mixed material into the molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it;
[0040] Step 4: The dried ceramic grinding wheel is placed in a resistance furnace for sintering to give it the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacture of the ceramic grinding wheel;
[0041] Step 5: The manufactured ceramic grinding wheel uses a small-sized grinding wheel as the basic specification. The small-sized grinding wheel is used alone, or multiple small-sized grinding wheels are combined to form large-sized grinding wheels of different specifications for use. When the large-sized grinding wheel is partially damaged, the local small-sized grinding wheel can be replaced;
[0042] Or the ceramic grinding wheel can be directly formed into large size specifications for use at one time.
[0043] Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed. The raw materials include abrasives, temporary binders, and pore-forming agents. The abrasives include brown corundum abrasives, white corundum abrasives, and silicon carbide abrasives.
[0044] Step 2: Add an appropriate amount of low-temperature binder raw material to the material uniformly mixed in step 1, and place it in a ball mill for mixing and grinding to form a uniform mixture. The binder uses a ceramic binder composed of clay and feldspar borax; the temporary binder uses polyvinyl alcohol; the pore-forming agent uses one or more of polytetrafluoroethylene, polyimide, bismaleimide and other organic substances; Step 2: Add an appropriate amount of binder raw material to the material uniformly mixed in step 1, and place it in a ball mill for mixing and grinding to form a uniform mixture. The ball milling time is 65-90 minutes; Step 3: Fill the mixed material into a molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it. The molding method is hot pressing; Step 3: Fill the mixed material into a molding mold, apply pressure to preliminarily shape the material, and place the molded sand wheel in a mold. The wheel is stored at room temperature for more than 48 hours to dry it. The temperature of hot pressing is 330-350℃, the pressing pressure is 20-24MPa, and the pressing time is 75-90min. Step 4: The dried ceramic grinding wheel is placed in a resistance furnace for sintering to make it have the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacturing of the ceramic grinding wheel. The sintering temperature is 900℃ and the time is 18-25 hours. The ceramic grinding wheel is made of the following raw materials by mass fraction: abrasive: 45%, binder: 25%, temporary binder: 4%, pore-forming agent: 13%; the specification of the lower size grinding wheel manufactured in step 5 is 600*200*305, the specification of the large size grinding wheel is 600*600*305 or 600*400*305 or other specifications, and the combination of the small size grinding wheel is bonding or inlaying or oblique splicing, wherein the oblique splicing is performed after the grinding wheel is processed with an inclined surface.
[0045] Example 3
[0046] like Figure 1 As shown, a production process of a high-thickness low-temperature bonded ceramic grinding wheel comprises the following steps:
[0047] Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed;
[0048] Step 2: Add an appropriate amount of low-temperature binder raw material to the materials uniformly mixed in step 1, and place them in a ball mill to mix and grind them to form a uniform mixture;
[0049] Step 3: Fill the mixed material into the molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it;
[0050] Step 4: The dried ceramic grinding wheel is placed in a resistance furnace for sintering to give it the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacture of the ceramic grinding wheel;
[0051] Step 5: The manufactured ceramic grinding wheel uses a small-sized grinding wheel as the basic specification. The small-sized grinding wheel is used alone, or multiple small-sized grinding wheels are combined to form large-sized grinding wheels of different specifications for use. When the large-sized grinding wheel is partially damaged, the local small-sized grinding wheel can be replaced;
[0052] Or the ceramic grinding wheel can be directly formed into large size specifications for use at one time.
[0053] Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed. The raw materials include abrasives, temporary binders, and pore-forming agents. The abrasives include brown corundum abrasives, white corundum abrasives, and silicon carbide abrasives.
[0054] Step 2: Add an appropriate amount of low-temperature binder raw material to the material uniformly mixed in step 1, and place it in a ball mill for mixing and grinding to form a uniform mixture. The binder uses a ceramic binder composed of clay and feldspar borax; the temporary binder uses polyvinyl alcohol; the pore-forming agent uses one or more of polytetrafluoroethylene, polyimide, bismaleimide and other organic substances; Step 2: Add an appropriate amount of binder raw material to the material uniformly mixed in step 1, and place it in a ball mill for mixing and grinding to form a uniform mixture. The ball milling time is 65-90 minutes; Step 3: Fill the mixed material into a molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it. The molding method is hot pressing; Step 3: Fill the mixed material into a molding mold, apply pressure to preliminarily shape the material, and place the molded sand wheel in a mold. The wheel is stored at room temperature for more than 48 hours to dry it. The temperature of hot pressing is 330-350℃, the pressing pressure is 20-24MPa, and the pressing time is 75-90min. The ceramic grinding wheel after step 4 is placed in a resistance furnace for sintering to make it have the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacture of the ceramic grinding wheel. The sintering temperature is 750℃ and the time is 18-25 hours. The ceramic grinding wheel is made of the following mass fractions of raw materials: abrasive: 55%, binder: 35%, temporary binder: 6%, pore-forming agent: 15%; the specification of the lower size grinding wheel manufactured in step 5 is 600*200*305, the specification of the large size grinding wheel is 600*600*305 or 600*400*305 or other specifications, and the combination of the small size grinding wheel is bonding or inlaying or oblique splicing, wherein the oblique splicing is performed after the grinding wheel is processed on the inclined surface.
[0055] Example 4
[0056] like Figure 1 As shown, a production process of a high-thickness low-temperature bonded ceramic grinding wheel comprises the following steps:
[0057] Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed;
[0058] Step 2: Add an appropriate amount of low-temperature binder raw material to the materials uniformly mixed in step 1, and place them in a ball mill to mix and grind them to form a uniform mixture;
[0059] Step 3: Fill the mixed material into the molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it;
[0060] Step 4: The dried ceramic grinding wheel is placed in a resistance furnace for sintering to give it the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacture of the ceramic grinding wheel;
[0061] Step 5: The manufactured ceramic grinding wheel uses a small-sized grinding wheel as the basic specification. The small-sized grinding wheel is used alone, or multiple small-sized grinding wheels are combined to form large-sized grinding wheels of different specifications for use. When the large-sized grinding wheel is partially damaged, the local small-sized grinding wheel can be replaced;
[0062] Or the ceramic grinding wheel can be directly formed into large size specifications for use at one time.
[0063] Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed. The raw materials include abrasives, temporary binders, and pore-forming agents. The abrasives include brown corundum abrasives, white corundum abrasives, and silicon carbide abrasives.
[0064] Step 2: Add an appropriate amount of low-temperature binder raw material to the material uniformly mixed in step 1, and place it in a ball mill for mixing and grinding to form a uniform mixture. The binder uses a ceramic binder composed of clay and feldspar borax; the temporary binder uses polyvinyl alcohol; the pore-forming agent uses one or more of polytetrafluoroethylene, polyimide, bismaleimide and other organic substances; Step 2: Add an appropriate amount of binder raw material to the material uniformly mixed in step 1, and place it in a ball mill for mixing and grinding to form a uniform mixture. The ball milling time is 65-90 minutes; Step 3: Fill the mixed material into a molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it. The molding method is hot pressing; Step 3: Fill the mixed material into a molding mold, apply pressure to preliminarily shape the material, and place the molded sand wheel in a mold. The wheel is stored at room temperature for more than 48 hours to dry it. The temperature of hot pressing is 330-350℃, the pressing pressure is 20-24MPa, and the pressing time is 75-90min. Step 4: The dried ceramic grinding wheel is placed in a resistance furnace for sintering to make it have the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacturing of the ceramic grinding wheel. The sintering temperature is 900℃ and the time is 18-25 hours. The ceramic grinding wheel is made of the following mass fractions of raw materials: abrasive: 55%, binder: 35%, temporary binder: 6%, pore-forming agent: 15%; the specification of the lower size grinding wheel manufactured in step 5 is 600*200*305, the specification of the large size grinding wheel is 600*600*305 or 600*400*305 or other specifications, and the combination of the small size grinding wheel is bonding or inlaying or oblique splicing, wherein the oblique splicing is performed after the grinding wheel is processed on the inclined surface.
[0065] Comparative Example 1
[0066] The same number of ceramic grinding wheels prepared in Example 1 and Example 2 were taken to test their hardness and flexural strength. The experimental results are shown in Table 1 below.
[0067] Table 1 Experimental results of grinding wheels in Example 1 and Example 2
[0068] parameter Example 1 Example 2 Hardness HDH 89.7 98.3 Flexural strength MPa 65.6 70.4
[0069] It can be seen from the above table that the hardness and flexural strength of the ceramic grinding wheel prepared by the production process of Example 2 are higher than those of the ceramic grinding wheel prepared by the production process of Example 1.
[0070] Comparative Example 2
[0071] The same number of ceramic grinding wheels prepared in Example 1 and Example 3 were taken to test their hardness and flexural strength. The experimental results are shown in Table 2 below.
[0072] Table 2 Experimental results of grinding wheels in Example 1 and Example 3
[0073] parameter Example 1 Example 3 Hardness HDH 89.7 81.9 Flexural strength MPa 65.6 60.5
[0074] It can be seen from the above table that the hardness and flexural strength of the ceramic grinding wheel prepared by the production process of Example 1 are higher than those of the ceramic grinding wheel prepared by the production process of Example 3.
[0075] Comparative Example 3
[0076] The same number of ceramic grinding wheels prepared in Example 1 and Example 4 were taken to test their hardness and flexural strength. The experimental results are shown in Table 3 below.
[0077] Table 3 Experimental results of grinding wheels in Example 1 and Example 4
[0078] parameter Example 1 Example 4 Hardness HDH 89.7 106.8 Flexural strength MPa 65.6 77.4
[0079] It can be seen from the above table that the hardness and flexural strength of the ceramic grinding wheel prepared by the production process of Example 4 are higher than those of the ceramic grinding wheel prepared by the production process of Example 1.
[0080] Comparative Example 4
[0081] The same number of ceramic grinding wheels prepared in Example 2 and Example 3 were taken to test their hardness and flexural strength. The experimental results are shown in Table 4 below.
[0082] Table 4 Experimental results of grinding wheels in Example 2 and Example 3
[0083] parameter Example 2 Example 3 Hardness HDH 98.3 81.9 Flexural strength MPa 70.4 60.5
[0084] It can be seen from the above table that the hardness and flexural strength of the ceramic grinding wheel prepared by the production process of Example 2 are higher than those of the ceramic grinding wheel prepared by the production process of Example 3.
[0085] Comparative Example 5
[0086] The same number of ceramic grinding wheels prepared in Example 2 and Example 4 were taken to test their hardness and flexural strength. The experimental results are shown in Table 5 below.
[0087] Table 5 Experimental results of grinding wheels in Example 2 and Example 4
[0088] parameter Example 2 Example 4 Hardness HDH 98.3 106.8 Flexural strength MPa 70.4 77.4
[0089] It can be seen from the above table that the hardness and flexural strength of the ceramic grinding wheel prepared by the production process of Example 4 are higher than those of the ceramic grinding wheel prepared by the production process of Example 2.
[0090] Comparative Example 6
[0091] The same number of ceramic grinding wheels prepared in Example 3 and Example 4 were taken to test their hardness and flexural strength. The experimental results are shown in Table 6 below.
[0092] Table 6 Experimental results of grinding wheels in Example 3 and Example 4
[0093] parameter Example 3 Example 4 Hardness HDH 81.9 106.8 Flexural strength MPa 60.5 77.4
[0094] It can be seen from the above table that the hardness and flexural strength of the ceramic grinding wheel prepared by the production process of Example 4 are higher than those of the ceramic grinding wheel prepared by the production process of Example 3.
[0095] According to the experimental results of Comparative Examples 1, 2, 3, 4, 5 and 6, the ceramic grinding wheel produced by the production process of Example 4 has the best hardness and flexural strength and the longest service life.
[0096] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A production process for high-thickness low-temperature bonded ceramic grinding wheels, characterized in that: The following steps are involved: Step 1: Mix the raw materials and stir them thoroughly in a mixer to ensure that the materials are evenly distributed; Step 2: Add an appropriate amount of low-temperature binder raw material to the materials uniformly mixed in step 1, and place them in a ball mill to mix and grind them to form a uniform mixture; Step 3: Fill the mixed material into the molding mold, apply pressure to preliminarily shape the material, and store the molded grinding wheel at room temperature for more than 48 hours to dry it; Step 4: The dried ceramic grinding wheel is placed in a resistance furnace for sintering to give it the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacture of the ceramic grinding wheel; Step 5: The manufactured ceramic grinding wheel uses a small-sized grinding wheel as the basic specification. The small-sized grinding wheel is used alone, or multiple small-sized grinding wheels are combined to form large-sized grinding wheels of different specifications for use. When the large-sized grinding wheel is partially damaged, the local small-sized grinding wheel can be replaced; Or the ceramic grinding wheel can be directly formed into large size specifications for use at one time.
2. A high-thickness low-temperature bond vitrified grinding wheel production process according to claim 1, characterized in that: In the step 1, the raw materials are mixed and fully stirred by a mixer to ensure that the materials are evenly distributed. The raw materials include abrasives, temporary binders, and pore-forming agents. The abrasives include brown corundum abrasives, white corundum abrasives, and silicon carbide abrasives.
3. A high-thickness low-temperature bond vitrified grinding wheel production process according to claim 2, characterized in that: The second step is to add an appropriate amount of low-temperature binder raw material to the material uniformly mixed in the first step, and place it in a ball mill for mixing and grinding to form a uniform mixture. The binder uses a ceramic binder composed of clay and feldspar borax.
4. A high-thickness low-temperature bond vitrified grinding wheel production process according to claim 2, characterized in that: The temporary adhesive is polyvinyl alcohol.
5. The production process of a high-thickness low-temperature bonded ceramic grinding wheel according to claim 2, characterized in that: The pore-forming agent is one or more organic substances selected from polytetrafluoroethylene, polyimide, and bismaleimide.
6. The production process of a high-thickness low-temperature bonded ceramic grinding wheel according to claim 1, characterized in that: The second step is to add a proper amount of binder raw material to the material uniformly mixed in the first step, and place it in a ball mill for mixing and grinding to form a uniform mixture. The ball milling time is 65-90 minutes.
7. Fill the material into the forming mold and apply pressure to preliminarily shape the material. The production process of a high-thickness low-temperature bond ceramic grinding wheel according to claim 1 is characterized in that: In the step three, the mixed material is filled into the molding die, and pressure is applied to preliminarily shape the material. The molded grinding wheel is stored at room temperature for more than 48 hours to dry it. The hot pressing molding temperature is 330-350° C., the pressing pressure is 20-24 MPa, and the pressing time is 75-90 min.
8. The production process of a high-thickness low-temperature bonded ceramic grinding wheel according to claim 1, characterized in that: The ceramic grinding wheel after drying in step 4 is placed in a resistance furnace for sintering to make it have the required hardness and toughness, and then the sintered grinding wheel is processed into the designed size to complete the manufacture of the ceramic grinding wheel. The sintering temperature is 750-900° C. and the time is 18-25 hours.
9. The production process of a high-thickness low-temperature bonded ceramic grinding wheel according to claim 3, characterized in that: The ceramic grinding wheel is made of the following raw materials in mass fractions: abrasive: 45%-55%, bonding agent: 25%-35%, temporary bonding agent: 4%-6%, and pore-forming agent: 13%-15%.
10. The production process of a high-thickness low-temperature bond vitrified grinding wheel according to claim 1, characterized in that: The specification of the lower-sized grinding wheel manufactured in the step five is 600*200*305, the specification of the large-sized grinding wheel is 600*600*305 or 600*400*305, and the combination method of the small-sized grinding wheel is bonding, embedding or oblique splicing, wherein the oblique splicing is performed after the grinding wheel is processed with an inclined surface.
Citation Information
Patent Citations
High-thickness grinding wheel
CN107378806A
Special ceramic bond end face grinding wheel for accurate grinding of compressor slip sheet and preparation method
CN112025565A
Preparation method of high-thickness low-temperature binder grinding needle ceramic grinding tool
CN117549226A
Superhard ceramic grinding wheel for grinding double end faces of metal ceramic cutter and preparation method of superhard ceramic grinding wheel
CN117601030A
Low-temperature ceramic bond