Low-carbon early strength concrete and preparation method thereof

By using a formula of aluminate cement, ultra-fine steel slag powder, silica fume and modified carbon nanotubes, the shortcomings of existing low-carbon early-strength concrete in early strength and carbon reduction are solved, and low-carbon production and high-efficiency carbon dioxide are achieved. Mineralization improves the early strength and structural compactness of concrete.

CN118771801APending Publication Date: 2024-10-15CHINA STATE CONSTR READY MIXED CONCRETE CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410857550.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing low-carbon early-strength concrete has deficiencies in achieving early strength and reducing carbon emissions, resulting in large carbon emissions, and there are many factors that control early strength development and have a greater impact.

Method used

It uses a formula system of aluminate cement, ultra-fine steel slag powder, silica fume, fine sand and gravel aggregate and modified carbon nanotubes to promote carbon dioxide mineralization through the modified carbon nanotube catalyst, combining ultra-fine steel slag powder and silica fume. Together, it improves the early strength of concrete and the formation of carbonate minerals, reducing carbon emissions.

Benefits of technology

It achieves low-carbon production, improves the early strength of concrete and the efficiency of mineralizing carbon dioxide, reduces carbon emissions, and optimizes the structural density and mechanical properties of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004918451480000051
    Figure BDA0004918451480000051
Patent Text Reader

Abstract

The invention discloses low-carbon early strength concrete, which is prepared from the following raw materials in parts by weight: 260 to 300 parts of cement, 60 to 90 parts of steel slag powder, 780 to 880 parts of sand, 950 to 1100 parts of stone, 15 to 30 parts of silica fume, 8 to 16 parts of catalyst, 8 to 10 parts of water reducing agent and 160 to 170 parts of water. The catalyst is a modified carbon nanotube. According to the invention, a formula system based on the low-carbon raw material aluminate cement, the superfine steel slag powder, the silica fume, the high-quality sandstone aggregate and the catalyst is adopted, so that low-carbon production and carbon dioxide mineralization of the concrete can be effectively realized, and good working performance, early strength performance and the like are considered; the preparation method is simple, convenient to operate and suitable for popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a low-carbon early-strength concrete and a preparation method thereof. Background Art

[0002] As an important material widely used in civil engineering fields such as buildings, roads, and bridges, the large amount of carbon dioxide emissions generated during the production and use of concrete has become one of the main sources of global carbon emissions. The research and development of low-carbon concrete is particularly important.

[0003] At present, low-carbon early-strength concrete usually still uses silicate cement as the main cementitious material, and the early strength performance is usually achieved by ordinary silicate cement combined with an early-strength agent, but the early strength development is controlled by many factors and the carbon emissions are also large; in terms of carbon reduction, the main method is to add mineral admixtures, but the impact on the early strength development of concrete is also large. Further development of low-carbon early-strength concrete with fast coagulation and hardening, high early strength and good carbon reduction and carbon fixation effects has good social and economic benefits. Summary of the invention

[0004] The main purpose of the present invention is to provide a low-carbon early-strength concrete in view of the problems and shortcomings of the prior art. The invention adopts a formulation system based on low-carbon raw materials such as aluminate cement, ultrafine steel slag powder, silica fume, fine sand and gravel aggregate, and catalyst, which can effectively achieve low-carbon production and carbon dioxide mineralization of concrete, while taking into account good working performance and early strength performance; and the preparation method involved is relatively simple, easy to operate, and suitable for promotion and application.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A low-carbon early-strength concrete comprises raw materials and their weight proportions: 260-300 parts of cement, 60-90 parts of steel slag powder, 780-880 parts of sand, 950-1100 parts of stone, 15-30 parts of silica fume, 8-16 parts of catalyst, 8-10 parts of water reducer and 160-170 parts of water; the catalyst is modified carbon nanotubes.

[0007] In the above scheme, the modified carbon nanotubes are obtained by adding carbon nanotubes to acid solution, stirring and dispersing them evenly (magnetic stirring for 5 to 10 minutes), soaking (3 to 5 hours), centrifuging, and drying (60 to 80° C.); the rate and efficiency of mineralizing carbon dioxide in the concrete system can be effectively improved.

[0008] In the above solution, the average diameter of the carbon nanotubes is 5 to 10 nm, and the length is 4 to 10 um.

[0009] In the above scheme, the acid solution is also nitric acid or the like, and its concentration is 30-50 vol%.

[0010] In the above scheme, the cement is aluminate cement, CA-50 grade or above, with a specific surface area greater than 320m 2 / kg; compared with ordinary silicates, the resulting concrete system has lower carbon emissions.

[0011] In the above scheme, the steel slag powder is ultrafine steel slag powder, the iron content of which is 6-10%, the particles smaller than 30um are greater than 80%, the 28d activity index is greater than 95%, and the specific surface area is greater than 700m 2 / kg; in the concrete system, it can promote carbonization reaction and improve the concrete microstructure.

[0012] In the above scheme, the particle size of the silica fume is 0.1-0.3 μm; it has good filling efficiency, and its SiO2 content is greater than 90%, which is beneficial to enhance the mineralization effect of carbon dioxide.

[0013] In the above scheme, the fineness modulus of the sand is 2.5-2.8, and the sand is medium in the second zone; the stone is 5-25 mm continuously graded, the crushing value is ≤6%, and the needle-like content is less than 6%.

[0014] In the above scheme, the water reducing agent is a polycarboxylic acid water reducing agent, and the water reducing rate is 12-30%.

[0015] The above-mentioned method for preparing low-carbon early-strength concrete comprises the following steps:

[0016] 1) Weigh the raw materials according to the proportion, and the raw materials and their weight proportions include: 260-300 parts of cement, 60-90 parts of steel slag powder, 780-880 parts of sand, 950-1100 parts of stone, 15-30 parts of silica fume, 8-16 parts of catalyst, 8-10 parts of water reducer, and 160-170 parts of water;

[0017] 2) First, mix part of the water and the water reducer evenly to obtain a water reducer solution; add sand and stone into a mixer and perform preliminary stirring to obtain a sand and stone mixture;

[0018] 3) Add cement, steel slag powder and silica fume to the sand and gravel mixture, continue stirring and disperse evenly;

[0019] 4) During the mixing process, add the pre-prepared polycarboxylate water-reducing agent solution and stir for 2 to 3 minutes to improve the working performance of the concrete, then slowly add the remaining amount of water and continue stirring;

[0020] 5) Finally, add the catalyst, stir and disperse evenly to obtain a low-carbon early-strength concrete mixture;

[0021] 6) The obtained low-carbon early-strength concrete mixture is placed in a CO2 environment with a purity of >90 vol% for curing to obtain a low-carbon early-strength concrete specimen.

[0022] In the above scheme, the water consumption in step 2) accounts for 40-60% of the total water consumption.

[0023] The low-carbon concrete prepared according to the above scheme has an initial slump of more than 180 mm, with no loss of slump within 1.5 hours. Microscopic testing and analysis of the specimens after 28 days of standard curing found that its structure is relatively dense and contains stable carbonate minerals, with excellent mechanical properties and basically no shrinkage in strength.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1) The hydration products of aluminate cement will undergo a crystal phase transition under certain temperature and humidity conditions. This process will release AH3 gel and free water and form pores, causing strength shrinkage. The present invention further introduces ultrafine steel slag powder. Under the stimulation of free water and AH3 alkali, the hydration activity of the ultrafine steel slag powder is stimulated again. The generated hydration products can effectively fill the pores, increase the density of the structure, reduce the carbon dioxide penetration and emission caused by pores and cracks in the concrete, and can also play a beneficial effect of compensating for the strength shrinkage.

[0026] 2) Using modified carbon nanotube catalysts can reduce OH in concrete - The activation energy and contact area of ​​the reaction with CO2 enable the system to promote the formation of stable carbonates, further filling the harmful pores generated by the crystal phase transformation, and effectively mineralizing carbon dioxide while also optimizing the pore structure of the system; in addition, the interaction between the modified carbon nanotube catalyst and the iron ions in the ultrafine steel slag powder can promote the formation of new active sites, further promoting the improvement of carbon fixation efficiency;

[0027] 3) The introduced silica fume particles are small in size and highly dispersible, which can provide more reaction sites for carbon dioxide, thereby improving the mineralization effect of the concrete system on carbon dioxide.

[0028] 4) This system uses aluminate cement and ultrafine steel slag powder as the main cementitious materials from the concrete raw materials. From material production to concrete composition and then to the entire life cycle of concrete service, it has beneficial effects of carbon reduction, carbon sealing and carbon absorption to varying degrees compared with existing concrete formulas. DETAILED DESCRIPTION

[0029] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with examples. These descriptions are only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention.

[0030] In the following examples, the cement used is aluminate cement, Zhengzhou Jianai CA-50 grade, 45um square hole sieve residue is 6.9%, and the specific surface area is 348m2 / kg; ultra-fine steel slag powder has a particle size below 30um, accounting for 84.6%, and a specific surface area of ​​718m 2 / kg, the activity index was measured to be 99.8%; the silica ash came from Henan Yixiang New Material Technology Co., Ltd., its particle size was 0.1-0.3μm, and the SiO2 mass fraction was 92.1%.

[0031] The modified carbon nanotubes are prepared by adding carbon nanotubes to a 50 vol% nitric acid solution, stirring for 5 min at room temperature using a magnetic stirring device to disperse the carbon nanotubes, soaking for 3 h, centrifuging the suspension after the reaction, and drying the suspension at 60-80° C. The carbon nanotubes used are provided by Shenzhen Suiheng Technology Co., Ltd., with an average diameter of 8 nm and an average length of 6 um.

[0032] The sand used is quartz sand, with a fineness modulus of 2.6, medium sand in zone 2; the stone used is quartz stone, with a continuous gradation of 5 to 25 mm, a crushing value of ≤6%, a mud content of ≤0.5%, and a needle-like shape of 0.6%;

[0033] The polycarboxylate water-reducing agent used is manufactured by China Construction Western Construction New Materials Technology Co., Ltd. The model is ZJC-01, with a solid content of 9.8% and a concrete water reduction rate of 24%.

[0034] Example 1

[0035] A low-carbon early-strength concrete, the preparation method of which comprises the following steps:

[0036] 1) Weigh the raw materials, and the weight proportions of the raw materials are: 260 parts of aluminate cement, 90 parts of ultrafine steel slag powder, 25 parts of silica fume, 810 parts of quartz sand, 1000 parts of quartz stone, 8 parts of modified carbon nanotubes, 8 parts of polycarboxylate water reducer, and 162 parts of water;

[0037] 2) First, 50% of the total water consumption is mixed with the polycarboxylate water-reducing agent to form a polycarboxylate water-reducing agent aqueous solution; sand and stone are added into a mixer and initially stirred to obtain a sand and stone mixture;

[0038] 3) Add aluminate cement, ultrafine steel slag powder and silica fume to the sand and gravel mixture and stir for 3 minutes to evenly mix the powdery materials with the aggregate;

[0039] 4) adding the pre-prepared polycarboxylate water-reducing agent aqueous solution to the mixture obtained in step 3) to improve the working performance of the concrete, continuing to stir for 2 minutes, adding the remaining amount of water, and continuing to stir;

[0040] 5) Finally, the modified carbon nanotubes are evenly sprinkled into a mixer and stirred for 1 minute to obtain a low-carbon early-strength concrete mixture;

[0041] 6) The prepared low-carbon early-strength concrete mixture is placed in a CO2 environment with a purity of >90 vol% for curing (normal temperature and pressure, the same below), thereby obtaining a low-carbon early-strength concrete specimen.

[0042] Example 2

[0043] A low-carbon early-strength concrete, the preparation method of which is substantially the same as that of Example 1, except that: the raw materials and their weight proportions are: 280 parts of aluminate cement, 80 parts of ultrafine steel slag powder, 20 parts of silica fume, 800 parts of quartz sand, 1000 parts of quartz stone, 10 parts of modified carbon nanotubes, 8 parts of polycarboxylic acid water reducer, and 160 parts of water.

[0044] Example 3

[0045] A low-carbon early-strength concrete, the preparation method of which is substantially the same as that of Example 1, except that: the raw materials and their weight proportions are: 300 parts of aluminate cement, 60 parts of ultrafine steel slag powder, 30 parts of silica fume, 790 parts of quartz sand, 1000 parts of quartz stone, 14 parts of modified carbon nanotubes, 9 parts of polycarboxylate water reducer, and 165 parts of water.

[0046] Example 4

[0047] A low-carbon early-strength concrete, the preparation method of which is substantially the same as that of Example 1, except that: the raw materials and their weight proportions are: 300 parts of aluminate cement, 80 parts of ultrafine steel slag powder, 15 parts of silica fume, 790 parts of quartz sand, 1000 parts of quartz stone, 16 parts of modified carbon nanotubes, 10 parts of polycarboxylic acid water reducer, and 168 parts of water.

[0048] Comparative Example 1

[0049] A low-carbon early-strength concrete, the preparation method of which is substantially the same as that of Example 1, except that: the raw materials and their weight proportions are: 360 parts of aluminate cement, 20 parts of silica fume, 800 parts of quartz sand, 1000 parts of quartz stone, 10 parts of modified carbon nanotubes, 8 parts of polycarboxylic acid water reducer, and 160 parts of water.

[0050] Comparative Example 2

[0051] A low-carbon early-strength concrete, the preparation method of which is substantially the same as that of Example 1, except that: the raw materials and their weight proportions are: 280 parts of aluminate cement, 80 parts of ultrafine steel slag powder, 20 parts of silica fume, 800 parts of quartz sand, 1000 parts of quartz stone, 8 parts of polycarboxylic acid water reducer, and 160 parts of water.

[0052] Comparative Example 3

[0053] A low-carbon early-strength concrete, the preparation method of which is substantially the same as that of Example 1, except that: the raw materials and their weight proportions are: 280 parts of aluminate cement, 80 parts of ultrafine steel slag powder, 10 parts of modified carbon nanotubes, 800 parts of quartz sand, 1000 parts of quartz stone, 8 parts of polycarboxylic acid water reducer, and 160 parts of water.

[0054] Comparative Example 4

[0055] A low-carbon concrete, the preparation method of which is substantially the same as that of Example 1, except that: unmodified carbon nanotubes are directly used.

[0056] The concretes formed by Examples 1 to 4 and Comparative Examples 1 to 4 were respectively tested for working performance, mechanical properties and microscopic properties, specifically including: measuring the initial fluidity and expansion of the fresh concrete, molding the prepared concrete into a 150mm×150mm×150mm test mold for testing the compressive strength of the concrete, and performing compressive strength tests after curing for 1d, 3d, and 28d under standard curing conditions. At the same time, 3d, 28d pore structure and 28d XRD tests were performed, followed by analysis. The carbonate content of the 28d sample was determined by the gravimetric method. The experimental results indirectly characterized its carbon fixation effect. The specific detection data indicators are shown in Table 1 below.

[0057] Table 1 Performance test results of concrete obtained from examples and comparative examples

[0058]

[0059] It can be seen from the above test results that the working performance and mechanical properties of the concrete obtained by the present invention are relatively excellent, and the carbon fixation effect is better than that of conventional means. From the perspective of the concrete pore structure, the internal structure is relatively dense.

[0060] The present invention is not limited to the above-mentioned embodiments. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

Claims

1. A low-carbon early-strength concrete, characterized in that: The raw materials and their weight proportions include: 260-300 parts of cement, 60-90 parts of steel slag powder, 780-880 parts of sand, 950-1100 parts of stone, 15-30 parts of silica fume, 8-16 parts of catalyst, 8-10 parts of water reducer, and 160-170 parts of water; the catalyst is modified carbon nanotubes.

2. The low-carbon early-strength concrete according to claim 1, characterized in that: The modified carbon nanotubes are prepared by adding the carbon nanotubes into an acid solution, stirring and dispersing the carbon nanotubes uniformly, soaking the carbon nanotubes, centrifuging and drying the carbon nanotubes.

3. The low-carbon early-strength concrete according to claim 2, characterized in that: The average diameter of the carbon nanotubes is 5-10 nm, and the length is 4-10 um.

4. The low-carbon early-strength concrete according to claim 1, characterized in that: The cement is aluminate cement, CA-50 grade or above, with a specific surface area greater than 320m 2 / kg.

5. The low-carbon early-strength concrete according to claim 1, characterized in that: The steel slag powder is ultra-fine steel slag powder, with an iron content of 6-10%, more than 80% of particles smaller than 30um, a 28d activity index greater than 95%, and a specific surface area greater than 700m 2 / kg.

6. The low-carbon early-strength concrete according to claim 1, characterized in that: The particle size of the silica fume is 0.1-0.3 μm, and the SiO2 content thereof is greater than 90%.

7. The low-carbon early-strength concrete according to claim 1, characterized in that: The sand has a fineness modulus of 2.5 to 2.8, and is medium sand in the second zone; the stone is continuously graded from 5 to 25 mm, the crushing value is ≤6%, and the needle-like content is less than 6%.

8. The low-carbon early-strength concrete according to claim 1, characterized in that: The water reducing agent has a water reducing rate of 12 to 30%.

9. The method for preparing the low-carbon early-strength concrete according to any one of claims 1 to 8, comprising the following steps: 1) Weigh the raw materials according to the proportion, and the raw materials and their weight proportions include: 260-300 parts of cement, 60-90 parts of steel slag powder, 780-880 parts of sand, 950-1100 parts of stone, 15-30 parts of silica fume, 8-16 parts of catalyst, 8-10 parts of water reducer, 160-170 parts of water; 2) First, mix part of the water and the water reducer evenly to obtain a water reducer solution; add sand and stone into a mixer and perform preliminary stirring to obtain a sand and stone mixture; 3) Add cement, steel slag powder and silica fume to the sand and gravel mixture, continue stirring and disperse evenly; 4) During the mixing process, add the pre-prepared polycarboxylate water-reducing agent solution and stir for 2 to 3 minutes to improve the working performance of the concrete, then slowly add the remaining amount of water and continue stirring; 5) Finally, add the catalyst, stir and disperse evenly to obtain a low-carbon early-strength concrete mixture; 6) The obtained low-carbon early-strength concrete mixture is placed in a CO2 environment with a purity of >90 vol% for curing to obtain a low-carbon early-strength concrete specimen.

Citation Information

Patent Citations

  • Carbon nanotube modified sea sand cement mortar and preparation method thereof

    CN112811868A

  • Low-carbon quick-hardening early-strength concrete and preparation method thereof

    CN115490489A

  • Carbonizable balancing weight with steel slag as main component and preparation method of carbonizable balancing weight

    CN117964298A