Preparation method of corn straw-based thermal-insulation foam concrete wall thermal-insulation material

CN118771818APending Publication Date: 2024-10-15BEIHUA UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410837282.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15

Smart Images

  • Figure CN118771818A_ABST
    Figure CN118771818A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a corn straw-based thermal insulation foam concrete wall thermal insulation material, and belongs to the technical field of thermal insulation materials. The thermal insulation material comprises the following raw materials in parts by mass: 30-40 parts of waterproof corn straw particles, 90-110 parts of 42.5 R Portland cement, 30-40 parts of quartz sand, 3-4 parts of a water reducing agent, 40-55 parts of water, 5-8 parts of a waterproof agent and 100-120 parts of foam. The modified waterproof corn straw particles are used as the raw material to be doped into the concrete and are mixed with the modified foam to prepare the thermal insulation material, so that the thermal insulation performance, the sound insulation performance and the tensile toughness of the thermal insulation material can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal insulation materials, and in particular relates to a method for preparing a corn stalk-based thermal insulation foam concrete wall insulation material. Background Art

[0002] Corn stalks are a natural renewable resource with abundant reserves and good thermal insulation, heat insulation, and sound insulation properties. However, since corn stalks are mainly composed of cellulose, hemicellulose, and lignin, they cannot react well with silicate cement and even reduce the strength of silicate cement paste, hindering the bonding strength of corn stalks as concrete filling aggregates. Summary of the invention

[0003] In order to solve the above technical problems, the present invention proposes a method for preparing a corn stalk-based thermal insulation foam concrete wall insulation material.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] A corn stalk-based thermal insulation foam concrete wall insulation material comprises the following raw materials in parts by mass: 30-40 parts of waterproof corn stalk particles, 90-110 parts of 42.5R Portland cement, 30-40 parts of quartz sand, 3-4 parts of water reducing agent, 40-55 parts of water, 5-8 parts of waterproofing agent and 100-120 parts of foam.

[0006] Furthermore, the method for preparing the waterproof corn stalk particles comprises the following steps:

[0007] The corn stalk particles and PC 32.5 silicate cement are mixed, and the obtained mixture is mixed with quartz sand for a second time to obtain a dry mix;

[0008] Add potassium methyl silicate into water and stir to obtain a waterproofing agent;

[0009] The waterproofing agent, hydroxypropyl methylcellulose thickener and water glass are mixed, stirred and allowed to stand for more than 6 hours (including 6 hours) to obtain a waterproof thickener;

[0010] The dry mix is ​​mixed with the waterproof thickener and stirred to obtain waterproof corn stalk particles.

[0011] Furthermore, in terms of mass fractions,

[0012] In the mixture, 10-15 parts of corn stalk particles and 10-15 parts of PC 32.5 silicate cement;

[0013] In the dry mix, the mixture comprises 20-25 parts and 10-15 parts of quartz sand;

[0014] The waterproofing agent contains 2-5 parts of potassium methyl silicate and 100-110 parts of water;

[0015] The waterproof thickener comprises 100-110 parts of waterproof agent, 0.7-1 parts of hydroxypropyl methylcellulose thickener, and 5-9 parts of water glass with a modulus of 2;

[0016] The waterproof corn stalk particles contain 100-120 parts of dry-mixed mixture and 60-80 parts of waterproof thickener.

[0017] Furthermore, the method for preparing the foam comprises the following steps:

[0018] The primary animal protein mixture, calcium hydroxide and sodium lauryl sulfate are mixed, crushed and sieved to obtain a medium animal protein mixture;

[0019] The intermediate animal protein mixture is added to water to carry out a first grafting reaction, filtered, gelatin is added to the obtained filtrate, and a second grafting reaction is continued to obtain a modified foaming agent mother solution;

[0020] The modified foaming agent mother solution is added into water and stirred, and foamed by a foaming machine to obtain foam.

[0021] Furthermore, in terms of mass fractions,

[0022] The intermediate animal protein mixture comprises 100-130 parts of primary animal protein mixture, 12-15 parts of calcium hydroxide, and 5-8 parts of sodium lauryl sulfate;

[0023] The modified foaming agent mother solution comprises 100-130 parts of a medium animal protein mixture, 500-600 parts of water, and 10-15 parts of gelatin;

[0024] The foam contains 20-30 parts of modified foaming agent mother solution and 700-800 parts of water.

[0025] Furthermore, the primary animal protein mixture is one or more of cattle horns, cattle hair, cattle hoof horns, pig hoof horns, pig hair and chicken hair;

[0026] The crushing and screening is through a 1mm square hole sieve;

[0027] The first grafting reaction was carried out in an autoclave at 120° C. for 4 hours;

[0028] The second grafting reaction was carried out in an autoclave at 120° C. for 1 hour.

[0029] The present invention also provides a method for preparing a corn stalk-based thermal insulation foam concrete wall insulation material, comprising the following steps:

[0030] Dry-mixing the waterproof corn stalk particles, 42.5R Portland cement and quartz sand to obtain a dry-mixed mixture;

[0031] mixing a water reducing agent, water, a waterproofing agent and the obtained dry mix to obtain a premix;

[0032] The foam and the premix are stirred and mixed, and after mixing, they are put into a mold for curing and forming to obtain the corn stalk-based thermal insulation foam concrete wall insulation material.

[0033] Compared with the prior art, the present invention has the following advantages and technical effects:

[0034] The present invention uses modified waterproof corn stalk particles as raw materials to mix into concrete, and at the same time mixes with modified foam to prepare thermal insulation materials, which can effectively improve the thermal insulation performance, sound insulation performance and tensile toughness of the thermal insulation materials. The thermal conductivity is 0.1-0.126 (w / (m·k)), the compressive strength is greater than 3.5MPa, and the bulk density is less than 1100kg / m 3 .

[0035] The invention uses corn stalks as raw materials, which can not only improve the utilization rate of renewable resources and reduce the burden of corn stalks, a renewable resource, on the environment, but also produce a masonry thermal insulation material, improve the performance of the thermal insulation material, and is a green and environmentally friendly building material. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0037] Figure 1 This is a sample picture prepared in Example 1. DETAILED DESCRIPTION

[0038] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0039] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0040] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0041] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0042] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0043] The "room temperature" in the present invention refers to 20-30°C unless otherwise specified.

[0044] The "parts" described in the present invention, unless otherwise specified, refer to parts by mass.

[0045] The raw materials used in the present invention are all purchased from the market.

[0046] The invention provides a corn stalk-based thermal insulation foam concrete wall insulation material, comprising the following raw materials in parts by weight: 30-40 parts of waterproof corn stalk particles, 90-110 parts of 42.5R Portland cement, 30-40 parts of quartz sand, 3-4 parts of water reducer, 40-55 parts of water (tap water, the same below), 5-8 parts of waterproof agent and 100-120 parts of foam. Preferably, the material comprises 30 parts of waterproof corn stalk particles, 90 parts of 42.5R Portland cement, 30 parts of quartz sand, 3 parts of water reducer, 40 parts of water, 5 parts of waterproof agent and 100 parts of foam.

[0047] The present invention limits the amount of waterproof corn straw particles in the thermal insulation material to 30-40 parts. When the amount is less than 30 parts, it is found that it is not very economical, because under the same material ratio, there is still a lot of surplus foamed silicate cement, the gap between waterproof straw particles is too large, and the bulk density of corn straw-based thermal insulation foam concrete is relatively large, greater than 1200kg / m 3 , and the utilization rate of corn straw is not high; when the dosage is greater than 40 parts, it is found that the gap between the waterproof granular straw is too small, resulting in the puncture of the bubbles in the foam concrete after mixing, and when the dosage is greater than 40 parts, the compressive strength decreases significantly and cannot meet 3.5MPa.

[0048] The present invention limits the amount of 42.5R silicate cement to 90-110 parts. If the amount is too small, it is difficult to ensure the material yield and the strength decreases significantly. When the amount is greater than 110 parts, the economic efficiency is poor.

[0049] The present invention limits the quartz sand to 30-40 parts. When the quartz sand content is less than 30 parts, the grading of quartz and waterproof corn stalk particles is not good, and discontinuous grading may occur. When the quartz sand content is greater than 40 parts, due to the excessive quartz sand content, the quartz sand self-weight is too large, and serious material stratification and uneven quality will occur in the foam concrete.

[0050] The present invention limits the water reducer to 3-4 parts. Too little water reducer will have no effect, while too much water reducer will affect the hydration strength of silicate cement.

[0051] The present invention limits the amount of water to 40-55 parts. Water is an important reaction reagent for preparing foamed concrete. The amount of water seriously affects the strength of foamed concrete. If the amount of water is too small, the cement slurry is difficult to have working properties, such as fluidity. If the amount of water is too large, the durability of the cement will also be affected.

[0052] The present invention limits the waterproofing agent to 5-8 parts. When the waterproofing agent dosage is less than 5 parts, it cannot achieve waterproofing effect, and the water absorption rate of the treated material is too large. When the waterproofing agent dosage is greater than 8 parts, silicate cement is prone to alkali precipitation and the like, which affects the strength.

[0053] The present invention limits the foam content to 100-120 parts. When the foam content is less than 100 parts, the foam concrete has a larger bulk density, poorer self-compacting fluidity, and a larger thermal conductivity. When the foam content is greater than 120 parts, the durability and strength of the foam concrete are lower.

[0054] In the following preferred embodiments of the present invention, the method for preparing the waterproof corn stalk particles comprises the following steps:

[0055] 1) Add 10-15 parts of corn stalk particles and 10-15 parts of PC 32.5 silicate cement into a mixer and mix for 1 minute to allow the silicate cement to fully wrap the surface of the corn stalk to prepare a mixture of corn stalk and silicate cement;

[0056] 2) mixing 20-25 parts of the mixture with 10-15 parts of quartz sand having a mud content of less than 1% for a second time to obtain a dry mix;

[0057] 3) taking 2-5 parts of potassium methyl silicate and 100-110 parts of water and stirring them, and determining the stirring time according to the total mass ratio of water to ensure that the potassium methyl silicate can be fully dissolved in tap water to obtain a waterproofing agent;

[0058] 4) mixing 100-110 parts of the waterproofing agent with 0.7-1 parts of hydroxypropyl methylcellulose thickener and 5-9 parts of water glass with a modulus of 2, stirring them fully with a high-speed stirrer, and letting the stirred solution stand for more than 8 hours to prepare a waterproof thickener;

[0059] 5) 100-120 parts of the dry mix obtained in step 2) and 60-80 parts of the waterproof thickener obtained in step 4) are placed in a drum mixer and stirred to obtain waterproof corn stalk particles.

[0060] Corn stalks are natural polymer materials with strong water absorption. At the same time, corn stalks themselves also contain a large amount of lignin. Excessive water absorption will cause the stalks to compete with silicate cement for water for hydration reaction. Because corn stalks have reversible water absorption, while absorbing and releasing water, they will bring out lignin. Lignin is an important retarder for silicate cement, which will cause silicate cement to set slowly or never set for life, and the strength will drop significantly. Therefore, improving the waterproofness of corn stalks is an important technical means to solve the problem of corn stalks as filling materials.

[0061] In the following preferred embodiments of the present invention, the method for preparing the foam comprises the following steps:

[0062] 1) taking ox horns, ox hair, ox hoof horns, pig hoof horns, pig hair and chicken hair, mixing them in a random proportion (the proportion does not affect the final foam performance, and in order to ensure uniformity, the mixing proportions in the following embodiments of the present invention are the same), and drying the mixed materials in a dryer at 50° C. for more than 8 hours to prepare a primary animal protein mixture;

[0063] 2) 100-130 parts of the primary animal protein mixture, 12-15 parts of calcium hydroxide and 5-8 parts of sodium lauryl sulfate are mixed, and the mixture is put into a ball mill for pulverization. After pulverization, the particles are sieved with a 1 mm square hole sieve to prepare a secondary animal protein mixture;

[0064] 3) adding 100-130 parts of the intermediate animal protein mixture to 500-600 parts of water, reacting in an autoclave at 120° C. for 4 hours to perform a first grafting reaction, filtering the mixed solution with a filter screen, adding 10-15 parts of gelatin to the filtered mixed solution, and then performing a grafting reaction in an autoclave at 120° C. for 1 hour to prepare a modified foaming agent mother solution;

[0065] 4) Add 20-30 parts of the modified foaming agent mother solution into 700-800 parts of water and stir at a low speed to ensure that the foaming mother solution is fully mixed with tap water, and then foam the mixed solution with a high-pressure foaming machine to obtain foam.

[0066] The foam mother liquor prepared by the present invention has the characteristics of strong foam stabilization performance and high concentration. The foam stabilizer is added to the foaming agent mentioned in the invention, which has strong foam stabilization performance, strong water retention and puncture resistance, and can well ensure that the foam will not be punctured by irregular particles of corn stalks during stirring. In addition, the foaming mother liquor has a high concentration. In the present invention, a small amount of foaming mother liquor (20-30 parts) can be diluted with 700-800 parts of water, so that foam cement slurry that meets the requirements can be prepared by a high-pressure foaming machine.

[0067] In the following preferred embodiments of the present invention, the quartz sand is quartz sand with a mud content of less than 1% and a particle size of 0.145-3 mm.

[0068] In the following preferred embodiments of the present invention, the water reducer is a naphthalene-based water reducer.

[0069] The method for preparing the corn stalk-based thermal insulation foam concrete wall insulation material comprises the following steps:

[0070] 1) dry-mixing waterproof corn stalk particles, 42.5R Portland cement and quartz sand to obtain a dry-mixed mixture;

[0071] 2) mixing a water reducing agent, water and a waterproofing agent, and then mixing the mixture with the obtained dry mix to obtain a concrete mixture;

[0072] 3) Add 100-120 parts of foam into the concrete mixture for mixing, then put it into a masonry material mold or cast it on site according to the wall form, and cure it to form a corn straw-based thermal insulation foam concrete wall insulation material.

[0073] The technical solution of the present invention is further illustrated by the following embodiments.

[0074] Example 1

[0075] Corn stalk-based thermal insulation foam concrete wall insulation material includes the following raw materials in parts by mass: 30 parts of waterproof corn stalk particles, 90 parts of 42.5R silicate cement, 30 parts of quartz sand, 3 parts of water reducing agent, 40 parts of water, 5 parts of waterproofing agent and 100 parts of foam.

[0076] A method for preparing a corn stalk-based thermal insulation foam concrete wall insulation material comprises the following steps:

[0077] Step S1, preparation of waterproof corn stalk particles:

[0078] 1) Use a 380V or 220V hay cutter to crush the corn stalks after autumn harvest, and sieve them with a spiral 3-5 cm square hole sieve or round hole sieve to control the particle size of the crushed stalks to between 3-5 cm;

[0079] 2) dry-mix 10 parts of corn stalk pellets with 12 parts of PC 32.5 Portland cement for 1 minute to prepare a corn stalk and Portland cement mixture;

[0080] 3) mixing 20 parts of the mixture with 10 parts of quartz sand having a mud content of less than 1% for a second time to obtain a dry mix;

[0081] 4) taking 3 parts of potassium methyl silicate and 100 parts of water and stirring them, and stirring them evenly to obtain a waterproofing agent;

[0082] 5) 100 parts of the waterproofing agent, 0.7 parts of hydroxypropyl methylcellulose thickener and 5 parts of water glass with a modulus of 2 were mixed, and the mixture was stirred thoroughly with a high-speed stirrer. The stirred solution was allowed to stand for 8 hours to prepare a waterproof thickener;

[0083] 6) putting 100 parts of the dry mix obtained in step 3) and 60 parts of the waterproof thickener obtained in step 5) into a drum mixer and stirring and mixing to obtain waterproof corn stalk particles;

[0084] Step S2, preparation of foam:

[0085] 1) taking ox horns, ox hair, ox hoof horns, pig hoof horns, pig hair and chicken hair, mixing them in random proportions, drying the mixed materials in a dryer at 50° C. for 8 hours, and then crushing them in a ball mill to a fineness modulus of less than 80 meshes, to prepare a primary animal protein mixture;

[0086] 2) 100 parts of the primary animal protein mixture, 12 parts of calcium hydroxide and 5 parts of sodium lauryl sulfate were put into a ball mill for grinding, and the particles after grinding were sieved with a 1 mm square hole sieve to prepare a medium animal protein mixture;

[0087] 3) adding 100 parts of the intermediate animal protein mixture to 500 parts of water, reacting in an autoclave at 120° C. for 4 hours to perform a first grafting reaction, filtering the mixed solution with a filter screen, adding 10 parts of gelatin to the filtered mixed solution, and then performing a grafting reaction in an autoclave at 120° C. for 1 hour to prepare a modified foaming agent mother solution;

[0088] 4) adding 20 parts of the modified foaming agent mother solution into 700 parts of water and stirring at a low speed to fully ensure that the foaming mother solution is mixed with tap water, and then foaming the mixed solution with a high-pressure foaming machine to obtain foam;

[0089] Step S3: Preparation of corn stalk-based thermal insulation foam concrete wall insulation material

[0090] 1) dry-mixing 30 parts of waterproof corn stalk particles, 90 parts of 42.5R Portland cement and 30 parts of quartz sand to obtain a dry-mixed mixture;

[0091] 2) mixing 3 parts of naphthalene-based water reducing agent, 40 parts of water and 5 parts of waterproofing agent, and then mixing with the obtained dry mix to obtain a concrete mixture;

[0092] 3) Add 100 parts of foam to the concrete mixture and mix, then put it into a masonry material mold or cast it on site according to the wall form, and cure it to form a corn stalk-based thermal insulation foam concrete wall insulation material (see Figure 1 ).

[0093] Example 2

[0094] The same as Example 1, except that step S1, the preparation of waterproof corn stalk particles is as follows:

[0095] 1) Use a 380V or 220V mower to crush the corn stalks after the autumn harvest, and control the particle size of the crushed stalks to between 3-5 cm;

[0096] 2) Mix 15 parts of corn stalk particles with 15 parts of PC32.5 Portland cement for 1 minute to prepare a mixture of corn stalk and Portland cement;

[0097] 3) mixing 25 parts of the mixture with 15 parts of quartz sand having a mud content of less than 1% for a second time to obtain a dry mix;

[0098] 4) taking 5 parts of potassium methyl silicate and stirring with 110 parts of water to obtain a waterproofing agent;

[0099] 5) 110 parts of the waterproofing agent, 1 part of the hydroxypropyl methylcellulose thickener and 8 parts of water glass with a modulus of 2 were mixed, and the mixture was stirred thoroughly with a high-speed stirrer. The stirred solution was allowed to stand for 6 hours to prepare a waterproof thickener;

[0100] 6) 110 parts of the dry mix obtained in step 3) and 80 parts of the waterproof thickener obtained in step 5) are placed in a drum mixer and stirred to obtain waterproof corn stalk particles.

[0101] Comparative Example 1

[0102] The same as Example 1, except that the corn stalk-based thermal insulation foam concrete wall insulation material includes the following raw materials in parts by weight: 20 parts of waterproof corn stalk particles, 120 parts of 42.5R Portland cement, 20 parts of quartz sand, 2 parts of water reducer, 50 parts of water, 4 parts of waterproofing agent and 100 parts of foam.

[0103] Performance Testing

[0104] The 28d compressive strength, apparent density and water absorption of the 100*100*100 cubic test blocks prepared in Examples 1-2 and Comparative Example 1 were tested according to JG / T 266-2011 standard; the thermal conductivity of 300*300*30 was tested according to GB / T 10294-2008 standard, as shown in Table 1.

[0105] Table 1 Performance test results of different products

[0106]

[0107] Comparative Example 2

[0108] The same as Example 1, except that, in step S1, the preparation of waterproof corn stalk particles is as follows:

[0109] 1) Use a 380V or 220V hay cutter to crush the corn stalks after autumn harvest, and sieve them with a spiral 3-5 cm square hole sieve or round hole sieve to control the particle size of the crushed stalks to between 3-5 cm;

[0110] 2) 10 parts of corn stalk pellets, 12 parts of PC 32.5 Portland cement and 10 parts of quartz sand with a mud content of less than 1% are mixed to obtain a dry mix;

[0111] 3) The dry mix was stirred with 100 parts of water to obtain corn stalk pellets.

[0112] The material prepared by this comparative example cannot be formed.

[0113] Comparative Example 3

[0114] The same as Example 1, except that step S2 is removed, and the foam is replaced by the foam concrete foaming agent produced by Henan Sitong Huajian Concrete Admixture Co., Ltd. and the concentrated high-efficiency cement reducing foaming agent produced by Leimo Chemical Products Co., Ltd.

[0115] The results show that the material prepared by this comparative example cannot be formed. The foaming agent of the present invention has good stability, large foaming amount, uniform foam size, and can resist the cracking of the formed foam caused by the adsorption of the natural pores of corn stalks, while the products of other manufacturers cannot resist the adsorption of corn stalks, resulting in the foam being unable to be formed and the strength being greatly reduced.

[0116] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A corn stalk-based thermal insulation foam concrete wall insulation material, characterized in that: The invention comprises the following raw materials in parts by weight: 30-40 parts of waterproof corn stalk particles, 90-110 parts of 42.5R silicate cement, 30-40 parts of quartz sand, 3-4 parts of water reducing agent, 40-55 parts of water, 5-8 parts of waterproofing agent and 100-120 parts of foam.

2. The corn stalk-based thermal insulation foam concrete wall insulation material according to claim 1, characterized in that: The method for preparing the waterproof corn stalk particles comprises the following steps: The corn stalk particles and PC 32.5 silicate cement are mixed, and the obtained mixture is mixed with quartz sand for a second time to obtain a dry mix; Add potassium methyl silicate into water and stir to obtain a waterproofing agent; The waterproofing agent, hydroxypropyl methylcellulose and water glass are mixed, stirred and allowed to stand to obtain a waterproof thickener; The dry mix is ​​mixed with the waterproof thickener and stirred to obtain waterproof corn stalk particles.

3. The corn stalk-based thermal insulation foam concrete wall insulation material according to claim 2, characterized in that: According to the mass fraction, In the mixture, 10-15 parts of corn stalk particles and 10-15 parts of PC 32.5 silicate cement; The dry mix comprises 20-25 parts of the mixture and 10-15 parts of quartz sand; The waterproofing agent contains 2-5 parts of potassium methyl silicate and 100-110 parts of water; The waterproof thickener comprises 100-110 parts of waterproof agent, 0.7-1 parts of hydroxypropyl methylcellulose thickener, and 5-9 parts of water glass with a modulus of 2; The waterproof corn stalk particles contain 100-120 parts of dry-mixed mixture and 60-80 parts of waterproof thickener.

4. The corn stalk-based thermal insulation foam concrete wall insulation material according to claim 1, characterized in that: The method for preparing the foam comprises the following steps: The primary animal protein mixture, calcium hydroxide and sodium lauryl sulfate are mixed, crushed and sieved to obtain a medium animal protein mixture; The intermediate animal protein mixture is added to water to carry out a first grafting reaction, filtered, gelatin is added to the obtained filtrate, and a second grafting reaction is continued to obtain a modified foaming agent mother solution; The modified foaming agent mother solution is added into water and stirred, and foamed by a foaming machine to obtain foam.

5. The corn stalk-based thermal insulation foam concrete wall insulation material according to claim 4, characterized in that: According to the mass fraction, The intermediate animal protein mixture comprises 100-130 parts of primary animal protein mixture, 12-15 parts of calcium hydroxide, and 5-8 parts of sodium lauryl sulfate; The modified foaming agent mother solution comprises 100-130 parts of a medium animal protein mixture, 500-600 parts of water, and 10-15 parts of gelatin; The foam contains 20-30 parts of modified foaming agent mother solution and 700-800 parts of water.

6. The corn stalk-based thermal insulation foam concrete wall insulation material according to claim 4, characterized in that: The primary animal protein mixture is one or more of cattle horns, cattle hair, cattle hoof horns, pig hoof horns, pig hair and chicken hair.

7. The corn stalk-based thermal insulation foam concrete wall insulation material according to claim 4, characterized in that: The crushing and screening is through a 1 mm square hole sieve.

8. The corn stalk-based thermal insulation foam concrete wall insulation material according to claim 4, characterized in that: The first grafting reaction was carried out in an autoclave at 120° C. for 4 hours.

9. The corn stalk-based thermal insulation foam concrete wall insulation material according to claim 4, characterized in that: The second grafting reaction was carried out in an autoclave at 120° C. for 1 hour to prepare a modified foaming agent mother solution.

10. A method for preparing the corn stalk-based thermal insulation foam concrete wall insulation material according to any one of claims 1 to 9, characterized in that: The following steps are involved: Dry-mixing the waterproof corn stalk particles, 42.5R Portland cement and quartz sand to obtain a dry-mixed mixture; mixing a water reducing agent, water, a waterproofing agent and the obtained dry mix to obtain a premix; The foam and the premix are stirred and mixed, and after mixing, they are put into a mold for curing and forming, so as to obtain the corn stalk-based thermal insulation foam concrete wall insulation material.

Citation Information

Patent Citations

  • Composite animal and vegetable protein foaming agent

    CN102964081A

  • Novel wall heat-insulating material and preparation process thereof

    CN108129108A

  • Lightweight foam concrete

    CN116120015A

  • Preparation method of corn straw thermal insulation concrete masonry material

    CN117383850A

  • Lignocellulose additive comprises wood shavings and / or plant stalks, and a mantle