Sintering method of yellow tungsten titanium oxide target material and yellow tungsten titanium oxide target material
Through the two-stage temperature-raising sintering method, the problem in the existing technology that the tungsten titanium oxide target material is not completely converted into tungsten trioxide is solved, and a high-density, low-resistance yellow tungsten titanium oxide target material is prepared, ensuring the quality and performance of the film. .
Patent Information
- Application Number
- CN202410751332.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-12
AI Technical Summary
It is difficult to prepare high-density yellow tungsten oxide and titanium targets with the existing technology, resulting in not all tungsten oxide being converted into tungsten trioxide, affecting the quality of the film.
A two-stage heating sintering method is adopted. The first stage is heated to 800℃ at a heating rate of 0.5-1℃/min, and then to 1150℃-1200℃ at a heating rate of 2-3℃/min, and continues to pass through the high temperature stage. Oxygen, the oxygen flow rate is 40-60L/min, and the short holding time is controlled to ensure the density and low resistance of the target material.
Successfully prepared tungsten titanium oxide targets that are all yellow and have low resistance, ensuring target quality, avoiding deactivation of tungsten trioxide and changes in tungsten price, increasing density and reducing resistance.
Smart Images

Figure CN118771886A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of target material preparation, and in particular to a sintering method of a yellow tungsten titanium oxide target material and the yellow tungsten titanium oxide target material. Background Art
[0002] Target materials are basic consumables in the magnetron sputtering process. Not only are they used in large quantities, but the quality of the target materials also plays a crucial role in determining the performance of the film. Target materials have a wide range of applications, mainly including optical targets, targets for display films, targets for semiconductors, targets for recording media, and superconducting targets, among which targets for semiconductors, targets for displays, and targets for recording media are the three most widely used targets.
[0003] In order to improve the film preparation rate and ensure the growth quality of the film, the sputtering target material must meet certain index requirements; in recent years, flat panel display technologies such as liquid crystal display, active organic light-emitting diode display and flexible display have developed rapidly, and the importance of thin film transistors (TFTs) as core components is self-evident; among them, TFTs based on oxide semiconductors have attracted widespread attention for their advantages such as higher mobility, good electrical uniformity, high visible light transmittance, lower preparation temperature, and lower cost.
[0004] The application of tungsten oxide in chemistry, mechanical sensors, selective catalysis, electrochemical industry and environmental engineering has attracted widespread attention. 3 ) is an n-type semiconductor with a wide direct band gap (3.2eV), very high chemical stability and high conductivity, as well as the ability to withstand high temperatures. Studies have shown that crystalline WO 3 It has high chemical stability against dissolution during the anodic oxidation process and can be used as a promising electrode material for wastewater treatment. 3 The photoactive crystalline structure of the film makes it suitable for application as UV photodetector.
[0005] In order to prepare high-quality WO 3 The existing technology generally prepares thin films by sputtering a tungsten-titanium oxide target, and one of the key technical points in preparing thin films is the quality of the target.
[0006] Prior art 1: Chinese patent application 201710218606.6 discloses a preparation process of a high-purity, low-density tungsten oxide target and a tungsten oxide target, the preparation steps of which include: 1) briquetting: pressing the tungsten oxide raw material powder into a plate-shaped block by a molding machine or a cold isostatic press; 2) calcining: placing the block obtained in step 1) in an oxygen atmosphere furnace for calcining; 3) crushing: crushing the calcined block in step 2), and the crushed powder is sieved through a 50-200 mesh sieve; 4) granulation and pressing: adding a molding agent to the crushed powder in step 3), mixing evenly, and putting it into a mold and pressing it with a molding machine to obtain a blank; 5) sintering: placing the blank obtained in step 4) in an oxygen atmosphere sintering furnace for sintering to obtain the tungsten oxide target.
[0007] Prior art 1 is to prepare a high-purity but low-density tungsten oxide target for preparing high-quality tungsten oxide electrochromic thin films. It is a better technical solution. The sintering process is recorded in paragraph 0028 of its specification: "5) Sintering: Place the blank obtained in step 4) into an oxygen atmosphere sintering furnace and sinter for 1-5 hours at 800-1200°C and an oxygen flow rate of 30L / min to obtain the high-purity and low-density tungsten oxide target of the present invention." However, when this technical solution was used to prepare a high-density tungsten oxide titanium target, it was found that the tungsten oxide in the prepared tungsten oxide titanium target was not yellow tungsten oxide, indicating that the tungsten oxide in the prepared target was not completely converted into tungsten trioxide.
[0008] Therefore, the technical problem to be solved by the present invention is: how to prepare a yellow tungsten titanium oxide target material for preparing WO 3 film. Summary of the invention
[0009] One of the purposes of the present invention is to provide a sintering method for a yellow tungsten titanium oxide target material. The tungsten titanium oxide target materials sintered by the sintering method have a yellow appearance and uniform color, and low resistance, which effectively ensures the quality of the produced tungsten titanium oxide target materials.
[0010] Another object of the present invention is to provide a yellow tungsten titanium oxide target material, which is yellow and uniform in color and can meet the downstream quality requirements for the tungsten titanium oxide target material.
[0011] To achieve the above object, the present invention provides a sintering method for a yellow tungsten oxide titanium target, comprising the following steps:
[0012] Step 1: Heat the tungsten oxide titanium target blank to 800°C at a heating rate of 0.5-1°C / min, and continuously supply oxygen during the process, with an oxygen flow rate of 15-20L / min;
[0013] Step 2: Heat from 800°C to 1150°C-1200°C at a heating rate of 2-3°C / min, and keep warm for 1-3h. During the process, oxygen is continuously supplied at an oxygen flow rate of 40-60L / min.
[0014] In the technical solution of the present invention, the tungsten oxide titanium target blank can be prepared by existing technology, such as tungsten oxide titanium target blanks prepared by existing processes such as cold isostatic pressing and hot isostatic pressing, and the sintering method of the yellow tungsten oxide titanium target material of the present invention can be used to sinter the tungsten oxide titanium target blank into a yellow tungsten oxide titanium target material.
[0015] Preferably, the titanium tungsten oxide target blank is prepared by the following steps:
[0016] Step a: preparing tungsten oxide-doped titanium oxide powder;
[0017] Step b: performing compression molding and cold isostatic pressing on tungsten oxide-doped titanium oxide powder to obtain a tungsten oxide titanium target blank.
[0018] Specifically, the cold isostatic pressing step is as follows: after the die is pressed, it is placed in a soft package film and sealed; the sealed soft package film is placed in a cold isostatic press and immersed in a liquid pressure medium; the high-pressure liquid injected by a high-pressure pump is pressed at a pressure of 360MPa-400MPa to obtain a target embryo.
[0019] Furthermore, the step a specifically comprises the following steps:
[0020] Step a1: Weigh tungsten oxide powder and titanium oxide powder at a molar ratio of 90-94.8:10-5.2;
[0021] Step a2: Pre-dispersing the titanium oxide powder with pure water and a first dispersant, and then grinding to obtain a first slurry;
[0022] Step a3: adding tungsten oxide powder and a second dispersant to the first slurry for pre-dispersion, and then grinding to obtain a second slurry;
[0023] Step a4: adding a binder to the second slurry for pre-dispersion, and then grinding to obtain a third slurry;
[0024] Step a5: spray granulate the third slurry to obtain tungsten oxide-doped titanium oxide powder.
[0025] Furthermore, the specific operation of step a2 is: adding titanium oxide powder, pure water and a first dispersant into a mixing barrel and pre-dispersing them at a speed of 60-200 r / min for 20-40 minutes, and then grinding them into a sander at a grinding speed of 1200-1800 r / min for 10-22 hours to obtain a first slurry with a solid content of 60-70%; wherein the first dispersant accounts for 1-5% of the total mass of the added titanium oxide powder, pure water and the first dispersant.
[0026] Furthermore, the specific operation of step a3 is: add tungsten oxide powder and the second dispersant to the first slurry and pre-disperse at a speed of 60-200r / min for 20-40min, then grind it into a sander at a grinding speed of 1200-1800r / min for 8-15h to obtain a second slurry with a solid content of 60-70%; wherein the second dispersant accounts for 1-15% of the total mass of the added tungsten oxide powder and the second dispersant.
[0027] Furthermore, the specific operation of step a4 is: adding a binder to the second slurry and pre-dispersing it at a speed of 60-200r / min for 20-40min, and then grinding it in a sander at a grinding speed of 1200-1800r / min for 2-4h to obtain a third slurry; wherein the binder accounts for 5-15% of the total mass of the added tungsten oxide powder, titanium oxide powder and binder.
[0028] Furthermore, the binder is at least one of polyvinyl alcohol and polyvinyl butyral, or a mixture of polyvinyl alcohol and polyethylene glycol.
[0029] Furthermore, the first dispersant and the second dispersant are one of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate and sodium hexadecylbenzene sulfonate.
[0030] Furthermore, the specific operation of step a5 is: injecting the third slurry into a spray drying tower for spray granulation, and then mixing and screening in sequence to obtain tungsten oxide-doped titanium oxide powder; wherein the air outlet temperature is 70-85° C., and the atomizer frequency is 120 Hz.
[0031] A yellow tungsten titanium oxide target material is prepared by adopting the sintering method of the yellow tungsten titanium oxide target material.
[0032] Beneficial Effects
[0033] Compared with the prior art, the present invention has at least the following advantages:
[0034] (1) The present invention discloses a sintering method for a yellow tungsten oxide titanium target material, which adopts a two-stage heating method. In the first heating stage, a lower heating rate and a lower oxygen flow rate are used to improve the density of the target material; in the second heating stage, a higher heating rate and a higher oxygen flow rate are used to avoid the deactivation of tungsten trioxide and cause a change in the price of tungsten.
[0035] (2) The present invention adopts a higher heating rate and a higher oxygen flow rate in the second heating stage to sinter the tungsten oxide titanium target while controlling a shorter holding time, which can effectively avoid the deactivation of tungsten trioxide caused by too long holding time, resulting in a change in the price of tungsten. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The present invention is further described below in conjunction with the accompanying drawings and embodiments;
[0037] Figure 1 This is a product appearance diagram of Embodiment 3 of the present invention;
[0038] Figure 2 This is a product appearance diagram of Comparative Example 1 of the present invention;
[0039] Figure 3 This is the appearance diagram of the product of Comparative Example 2 of the present invention;
[0040] Figure 4 It is the product appearance picture of comparative example 5 of the present invention. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with the embodiments, but it does not constitute any limitation to the present invention. Any limited number of modifications made within the scope of the claims of the present invention are still within the scope of the claims of the present invention.
[0042] In order to explain the technical content of the present invention in detail, further description is given below in conjunction with the implementation modes.
[0043] In the following examples and comparative examples, the titanium tungsten oxide target blanks are prepared by the following steps:
[0044] Step a1: Weigh tungsten oxide powder and titanium oxide powder in a molar ratio of 90:10;
[0045] Step a2: adding titanium oxide powder, pure water and polyvinyl pyrrolidone into a mixing barrel and pre-dispersing them at a speed of 100 r / min for 30 minutes, and then grinding them into a grinder at a grinding speed of 1500 r / min for 12 hours to obtain a first slurry with a solid content of 70%; wherein the polyvinyl pyrrolidone accounts for 4% of the total mass of the added titanium oxide powder, pure water and polyvinyl pyrrolidone;
[0046] Step a3: Add tungsten oxide powder and polyvinyl pyrrolidone to the first slurry and pre-disperse at a speed of 100 r / min for 30 minutes, then grind in a sander at a grinding speed of 1500 r / min for 8 hours to obtain a second slurry with a solid content of 65%; wherein the polyvinyl pyrrolidone accounts for 4% of the total mass of the added tungsten oxide powder and polyvinyl pyrrolidone;
[0047] Step a4: Add polyvinyl alcohol to the second slurry and pre-disperse it at a speed of 100 r / min for 30 minutes, then grind it in a sander at a grinding speed of 1500 r / min for 2 hours to obtain a third slurry; wherein the polyvinyl alcohol accounts for 10% of the total mass of the added tungsten oxide powder, titanium oxide powder and polyvinyl alcohol;
[0048] Step a5: injecting the third slurry into a spray drying tower for spray granulation, and then mixing and sieving in sequence to obtain tungsten oxide-doped titanium oxide powder; wherein the air outlet temperature is 75° C. and the atomizer frequency is 120 Hz;
[0049] Step b: performing compression molding and cold isostatic pressing on tungsten oxide-doped titanium oxide powder to obtain a tungsten oxide titanium target blank.
[0050] Specifically, the cold isostatic pressing step is as follows: after the die is pressed, it is placed in a soft package film and sealed; the sealed soft package film is placed in a cold isostatic press and immersed in a liquid pressure medium; the high-pressure liquid injected by a high-pressure pump is pressed at a pressure of 360MPa-400MPa to obtain a target embryo.
[0051] It should be noted that the tungsten oxide doped titanium oxide powder and the tungsten oxide titanium target blank of the present invention can not only be prepared by the above steps, but also can be prepared by other existing technologies; the tungsten oxide titanium target blank prepared by other existing technologies can be used to prepare yellow tungsten oxide titanium target material by the sintering method of the present invention.
[0052] Example 1
[0053] A yellow tungsten titanium oxide target is sintered by the following steps:
[0054] Step 1: The tungsten oxide titanium target blank is heated to 800°C at a heating rate of 0.5°C / min, and oxygen is continuously supplied during the process, with an oxygen flow rate of 15L / min;
[0055] Step 2: Heat the temperature from 800°C to 1150°C at a heating rate of 3°C / min, and keep it warm for 2 hours to obtain a yellow tungsten titanium oxide target. Oxygen is continuously supplied during the process, and the oxygen flow rate is 40L / min.
[0056] Example 2
[0057] A yellow tungsten titanium oxide target is sintered by the following steps:
[0058] Step 1: The tungsten oxide titanium target blank is heated to 800°C at a heating rate of 0.5°C / min, and oxygen is continuously supplied during the process, with an oxygen flow rate of 15L / min;
[0059] Step 2: Heat the temperature from 800°C to 1200°C at a heating rate of 2°C / min, and keep it warm for 2 hours to obtain a yellow tungsten oxide titanium target. Oxygen is continuously supplied during the process, and the oxygen flow rate is 60L / min.
[0060] Example 3
[0061] A yellow tungsten titanium oxide target is sintered by the following steps:
[0062] Step 1: Heat the tungsten oxide titanium target blank to 800°C at a heating rate of 1°C / min, and continuously supply oxygen during the process with an oxygen flow rate of 15L / min;
[0063] Step 2: Heat the temperature from 800°C to 1180°C at a heating rate of 3°C / min and keep it warm for 3 hours to obtain a yellow tungsten titanium oxide target. Oxygen is continuously supplied during the process with an oxygen flow rate of 55 L / min.
[0064] Example 4
[0065] A yellow tungsten titanium oxide target is sintered by the following steps:
[0066] Step 1: The tungsten oxide titanium target blank is heated to 800°C at a heating rate of 1°C / min, and oxygen is continuously supplied during the process, with an oxygen flow rate of 20L / min;
[0067] Step 2: Heat the temperature from 800°C to 1180°C at a heating rate of 3°C / min and keep it warm for 3 hours to obtain a yellow tungsten titanium oxide target. Oxygen is continuously supplied during the process with an oxygen flow rate of 55 L / min.
[0068] Example 5
[0069] A yellow tungsten titanium oxide target is sintered by the following steps:
[0070] Step 1: The tungsten oxide titanium target blank is heated to 800°C at a heating rate of 1°C / min, and oxygen is continuously supplied during the process, with an oxygen flow rate of 20L / min;
[0071] Step 2: Heat the temperature from 800°C to 1180°C at a heating rate of 3°C / min and keep it warm for 3 hours to obtain a yellow tungsten titanium oxide target. Oxygen is continuously supplied during the process with an oxygen flow rate of 40 L / min.
[0072] Comparative Example 1
[0073] A yellow tungsten titanium oxide target is sintered by the following steps:
[0074] Step 1: Heat the tungsten oxide titanium target blank to 1180°C at a heating rate of 1°C / min, and keep it warm for 3 hours to obtain a yellow tungsten oxide titanium target. Oxygen is continuously supplied during the process, and the oxygen flow rate is 55L / min.
[0075] Comparative Example 2
[0076] It is generally the same as Example 3, except that the insulation time of step 2 is 5 hours.
[0077] Comparative Example 3
[0078] It is generally the same as Example 3, except that the heating rate of step 1 is 3°C / min.
[0079] Comparative Example 4
[0080] It is generally the same as Example 3, except that the heating rate of step 2 is 0.5°C / min.
[0081] Comparative Example 5
[0082] It is generally the same as Example 3, except that the oxygen flow rate in step 2 is 20 L / min.
[0083] Comparative Example 6
[0084] It is generally the same as Example 3, except that the oxygen flow rate in step 1 is 30 L / min.
[0085] Performance Testing
[0086] Test method:
[0087] Density measurement is obtained by Archimedes displacement method.
[0088] The resistance is measured by four-probe measurement.
[0089] The targets prepared in Examples 1-5 and Comparative Examples 1-6 were tested according to the above test method. The results are shown in Table 1 and Attached Figure 1-4 As shown, Figure 1 This is the product picture of Example 3. Figure 2 The product diagram of comparative example 1, Figure 3 This is the product picture of Comparative Example 2. Figure 4 This is the product picture of Comparative Example 5;
[0090] Table 1 Target performance data obtained from Examples 1-5 and Comparative Examples 1-6
[0091] <![CDATA[Target density g / cm 3 > Resistance mΩ·cm Target appearance Example 1 6.71 1.4663 The target material is yellow and uniform in color Example 2 6.74 1.4386 The target material is yellow and uniform in color Example 3 6.79 1.3892 The target material is yellow and uniform in color Example 4 6.82 1.2940 The target material is yellow and uniform in color Example 5 6.80 1.3048 The target material is yellow and uniform in color Comparative Example 1 6.26 1.569 The target is light yellow but has some green spots Comparative Example 2 6.76 686.358 The target material is dark green in color Comparative Example 3 6.14 1.6973 The target is yellow Comparative Example 4 6.73 639.4897 The target material is dark green in color Comparative Example 5 6.77 796.359 The target material is dark green with black spots Comparative Example 6 6.32 1.6984 The target is light yellow but has some green spots
[0092] According to the results in Table 1, we can see that:
[0093] According to Examples 1-5, the tungsten oxide titanium target sintered by the sintering method of the present invention can effectively ensure that the components in the target are all yellow tungsten oxide, ensure the valence state of tungsten, and effectively increase the density of the target and reduce the resistance of the target.
[0094] According to Comparative Example 1, failure to adopt the two-stage temperature increase sintering method of the present invention will lead to the appearance of some green spots in the target material, that is, the valence state of tungsten changes, thus affecting the quality of the target material. It is speculated that this is caused by too low density of the target material in the early stage of sintering. In Comparative Example 1, too much oxygen is introduced in the early stage of sintering, which affects the densification process and causes oxygen vacancies in the target material, thereby increasing the probability of tungsten valence state changes.
[0095] According to the data comparison between Example 3 and Comparative Example 2, when the holding time is too long, the tungsten oxide in the tungsten oxide titanium target will be deactivated and the valence state of tungsten will change. The tungsten oxide grains in the target produced are not yellow tungsten trioxide grains.
[0096] According to the data comparison between Example 3 and Comparative Example 3, when the heating rate of step 1 is too fast, the density of the target material will decrease significantly.
[0097] According to the data comparison between Example 3 and Comparative Example 4, when the heating rate in step 2 is too slow, the tungsten oxide in the tungsten oxide titanium target will be inactivated and the valence state of tungsten will change. The tungsten oxide grains in the target produced are not yellow tungsten trioxide grains. The possible reason is that heating too fast will reduce the density of the target, affecting the densification process of the target, thereby increasing the probability of tungsten valence change.
[0098] According to the data comparison of Example 3 and Comparative Examples 5 and 6, it can be seen that when the oxygen flow rate of step 1 and the oxygen flow rate of step 2 are not within the scope of the technical solution of the present invention, the target materials produced are not yellow tungsten titanium oxide targets. The reason is that when the oxygen flow rate of step 2 is less than the scope of this solution, the target material is not sintered in an oxygen-rich atmosphere during the high temperature stage, which causes the target material to lose oxygen and affects the color of the target material; when the oxygen flow rate of step 1 is less than the scope of this solution, it also affects the color of the target material. When it is greater than the scope of this solution, the density of the target material will be reduced. The reason is that the oxygen flow rate is too high, and the gas and other substances inside the target material cannot be well escaped, and remain inside the target material, affecting the densification process, thereby increasing the probability of changes in the tungsten valence state.
[0099] The embodiments presented herein are only embodiments selected according to the combination of all possible embodiments. The appended claims should not be limited by the embodiments describing the present invention. Some numerical ranges used in the claims include sub-ranges therein, and the changes in these ranges should also be covered by the appended claims.
Claims
1. A sintering method for a yellow tungsten titanium oxide target, characterized in that: The steps include: Step 1: Heat the tungsten oxide titanium target blank to 800°C at a heating rate of 0.5-1°C / min, and continuously supply oxygen during the process, with an oxygen flow rate of 15-20L / min; Step 2: Heat from 800°C to 1150°C-1200°C at a heating rate of 2-3°C / min, and keep warm for 1-3h. During the process, oxygen is continuously supplied at an oxygen flow rate of 40-60L / min.
2. The sintering method of yellow tungsten oxide titanium target according to claim 1, characterized in that: The titanium tungsten oxide target blank is prepared by the following steps: Step a: preparing tungsten oxide-doped titanium oxide powder; Step b: performing compression molding and cold isostatic pressing on tungsten oxide-doped titanium oxide powder to obtain a tungsten oxide titanium target blank.
3. The sintering method of the yellow tungsten oxide titanium target according to claim 2, characterized in that: The step a specifically comprises the following steps: Step a1: Weigh tungsten oxide powder and titanium oxide powder at a molar ratio of 90-94.8:10-5.2; Step a2: Pre-dispersing the titanium oxide powder with pure water and a first dispersant, and then grinding to obtain a first slurry; Step a3: adding tungsten oxide powder and a second dispersant to the first slurry for pre-dispersion, and then grinding to obtain a second slurry; Step a4: adding a binder to the second slurry for pre-dispersion, and then grinding to obtain a third slurry; Step a5: spray granulate the third slurry to obtain tungsten oxide-doped titanium oxide powder.
4. The sintering method of the yellow tungsten oxide titanium target according to claim 3, characterized in that: The specific operation of step a2 is: adding titanium oxide powder, pure water and a first dispersant into a mixing barrel and pre-dispersing them at a speed of 60-200 r / min for 20-40 minutes, and then grinding them into a sander at a grinding speed of 1200-1800 r / min for 10-22 hours to obtain a first slurry with a solid content of 60-70%; wherein the first dispersant accounts for 1-5% of the total mass of the added titanium oxide powder, pure water and the first dispersant.
5. The sintering method of yellow tungsten oxide titanium target according to claim 3, characterized in that: The specific operation of step a3 is: add tungsten oxide powder and the second dispersant to the first slurry and pre-disperse at a speed of 60-200 r / min for 20-40 minutes, then grind it into a sander at a grinding speed of 1200-1800 r / min for 8-15 hours to obtain a second slurry with a solid content of 60-70%; wherein the second dispersant accounts for 1-15% of the total mass of the added tungsten oxide powder and the second dispersant.
6. The sintering method of yellow tungsten oxide titanium target according to claim 3, characterized in that: The specific operation of step a4 is: adding a binder to the second slurry and pre-dispersing it at a speed of 60-200 r / min for 20-40 minutes, then grinding it in a sander at a grinding speed of 1200-1800 r / min for 2-4 hours to obtain a third slurry; wherein the binder accounts for 5-15% of the total mass of the added tungsten oxide powder, titanium oxide powder and binder.
7. The sintering method of the yellow tungsten oxide titanium target according to claim 6, characterized in that: The binder is at least one of polyvinyl alcohol and polyvinyl butyral or a mixture of polyvinyl alcohol and polyethylene glycol.
8. The sintering method of the yellow tungsten oxide titanium target according to any one of claims 3 to 5, characterized in that: The first dispersant and the second dispersant are one of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate and sodium hexadecylbenzene sulfonate.
9. The sintering method of yellow tungsten oxide titanium target according to claim 3, characterized in that: The specific operation of step a5 is: injecting the third slurry into a spray drying tower for spray granulation, and then mixing and sieving in sequence to obtain tungsten oxide-doped titanium oxide powder; wherein the air outlet temperature is 70-85° C., and the atomizer frequency is 120 Hz.
10. A yellow tungsten titanium oxide target, characterized in that: The yellow tungsten oxide titanium target is prepared by the sintering method of any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation technology of tungsten oxide target material with high purity and low density and tungsten oxide target material
CN106977202A
Gas sensitive element based on tungsten oxide / titanium oxide core-shell nanowires and preparation method of gas sensitive element
CN107402241A
Aerosol-assisted synthesis of crystalline tungsten bronze particles
WO2022035631A1
Method for preparing ultrafine tungsten carbide powder by means of one-step carbonization of tungsten oxide
WO2023065457A1