Transparent high-barrier film and preparation method thereof
Through the combined structure of alumina-plated base layer, barrier coating layer and polyurethane protective layer, combined with modified nanoparticles and functional additives, the deficiencies in barrier performance and mechanical properties of traditional films are solved, achieving high transparency and good gas Barrier and mechanical strength film suitable for packaging needs in many fields.
Patent Information
- Application Number
- CN202410990072.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult for traditional films to meet high transparency, excellent gas barrier properties and good mechanical properties at the same time. Moreover, the adhesion between the barrier layer and the substrate and the flexibility and wear resistance of the film are insufficient, making it difficult to improve barrier properties while maintaining cost-effectiveness.
It adopts a combined structure of plated aluminum oxide base layer, barrier coating layer and polyurethane protective layer. The barrier coating liquid contains functional additives such as modified nanoparticles, polyvinyl alcohol and polyvinylidene chloride, and is pre-treated and refined through glow discharge. Coating technology ensures layer uniformity and adhesion.
Significantly enhances the barrier capability against oxygen and water vapor, extends the shelf life of packaged items, and improves the wear resistance, flexibility and mechanical strength of the film. It is suitable for food, medicine and electronic product packaging, meeting the requirements of high performance and environmental protection. demand for packaging materials.
Smart Images

Figure CN118772475A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging materials, and in particular to a transparent high-barrier film and a preparation method thereof. Background Art
[0002] In the field of packaging materials, especially food, medicine and high-end electronic product packaging, there are extremely high requirements for the barrier properties of film materials. Traditional film materials often find it difficult to simultaneously meet the requirements of high transparency, excellent gas barrier properties and good mechanical properties. As consumers pay more and more attention to product preservation, safety and packaging sustainability, the market urgently needs a new type of film material that can effectively isolate harmful substances such as oxygen and water vapor while maintaining high transparency and good physical properties.
[0003] In the prior art, although there have been some attempts to improve the barrier properties of films by adding inorganic fillers or using specific polymers, these methods often have many limitations. For example, the addition of inorganic fillers may cause the transparency of the film to decrease, while the use of specific polymers may increase costs or reduce the processing performance of the film. In addition, how to ensure good adhesion between the barrier layer and the substrate, and how to maintain the flexibility and wear resistance of the film while improving the barrier performance are also key issues that need to be urgently resolved in the industry. Therefore, the development of a new type of transparent high-barrier film that can maintain high transparency while having excellent gas barrier properties and good mechanical strength, and has good processing performance and environmental adaptability has become an important direction of current materials science research. Summary of the invention
[0004] The main purpose of the present invention is to provide a transparent high-barrier film and a preparation method thereof, which can effectively solve the problems in the background technology.
[0005] To achieve the above object, the technical solution adopted by the present invention is: A transparent high-barrier film, comprising a base layer in the middle, barrier coating layers are arranged on both upper and lower end surfaces of the base layer, and a protective layer is arranged on the side of the barrier coating layer opposite to the base layer; The thickness of the base layer is 35-75 μm, the thickness of the barrier coating layer is 25-45% of the thickness of the base layer, and the thickness of the protective layer is 3-8% of the thickness of the base layer; The base layer is an aluminum oxide film; The protective layer is a polyurethane film; The barrier coating liquid comprises the following raw materials by weight: 20-30 parts of 11,3,3-tetramethylguanidine, 5-10 parts of xylene, 30-40 parts of 3-chloropropyltrimethoxysilane, 5-10 parts of wetting agent, 5-10 parts of curing agent, 5-10 parts of organic solvent, 30-50 parts of polyvinylidene chloride solution, 10-20 parts of polyvinylidene chloride solution, and 4-7 parts of modified nanoparticles; the solid content of the second protective coating liquid is 10-12%.
[0006] Preferably, the modified nanoparticles include the following raw materials by weight: 30-50 parts of azobisisobutyronitrile, 20-30 parts of silicon dioxide, 20-30 parts of zinc oxide, 10-20 parts of divinylbenzene, 8-12 parts of sodium p-styrene sulfonate, 15-25 parts of chitosan, 6-8 parts of trifluoromethanesulfonic acid, 10-14 parts of titanate coupling agent, 20-28 parts of methanol, 20-28 parts of chlorophyllide, 10-20 parts of clove essential oil, 10-18 parts of terminal epoxy silicone oil, and 8-14 parts of anionic emulsifier.
[0007] Preferably, the polyvinyl alcohol solution comprises powdered polyvinyl alcohol and deionized water, and the solid content of the polyvinyl alcohol solution is 10-18%; the solid content of the polyvinylidene chloride solution is 38-42%.
[0008] Preferably, the curing agent is melamine curing agent; the wetting agent is sulfosuccinate surfactant; and the organic solvent is ethanol.
[0009] Preferably, the anionic emulsifier is one or more of oleic acid and pure sodium lauryl sulfate; and the titanate coupling agent is KR-TTS.
[0010] Preferably, the preparation method of the barrier coating liquid is: S1: Preparation of nanocarriers: S2: preparing emulsion; S3: setting the reaction temperature to 19-24°C and the pressure to 0.01-0.2MPa, placing the nanocarrier in the emulsion for ultrasonic dispersion for 30-60min, and filtering to obtain modified nanoparticles; S4: Synthetic barrier coating fluid.
[0011] Preferably, in S1, preparing the nanocarrier specifically comprises the following steps: S101: Mix 11,3,3-tetramethylguanidine and xylene at 80-100°C, stir and react for 50-70 minutes, add 3-chloropropyltrimethoxysilane, stir and react for 1-2 hours, and filter and wash to obtain material A; S102: placing material A under a pressure of 80-90 mmHg for vacuum distillation, and taking the fraction obtained under a temperature of 125-140° C. as solution A; S103: placing solution A at 95-105°C and 0.8-1.3 MPa under stirring for 18-24 hours, evaporating the solvent to obtain material B; S104: Place azobisisobutyronitrile in tetrahydrofuran at 25-35°C and stir to dissolve, then add silicon dioxide, zinc oxide, divinylbenzene, and sodium p-styrene sulfonate in sequence, and stir at 100-150 r / min for 30-60 min to obtain solution B: S105: placing chitosan in a hydrochloric acid solution and stirring to dissolve, to obtain a solution C; S106: Add solution C and ethanol to material B and mill at a ball milling speed of 500-600 r / min for 30-40 min, add concentrated sulfuric acid and stir to react for 8-12 h, filter, wash and dry to obtain material C; S107: Place material C in toluene at a constant temperature of 85-95°C and stir to react for 3-5h, add trifluoromethanesulfonic acid at a dropping speed of 1-3ml / min, and stir to react for 20-30min while adding. After the addition is completed, continue to stir to react at a stirring speed of 100-200r / min for 1-3h, add titanate coupling agent and continue to stir to react for 1-2h, filter, wash, and vacuum dry to obtain the nanocarrier.
[0012] Preferably, in S2, preparing the emulsion specifically comprises the following steps: S201: Mix methanol and chlorophyllin acid to obtain a water-based solution; mix clove essential oil and epoxy-terminated silicone oil to obtain an oil-based solution; S202: Pour the water-based solution into the oil-based solution, add an anionic emulsifier, and stir at a high speed of 2000-2200 r / min for 10-15 minutes to obtain an emulsion.
[0013] In S4, synthesizing the barrier coating liquid specifically includes the following steps: S401: placing powdered polyvinyl alcohol in deionized water and stirring to dissolve to obtain a polyvinyl alcohol solution, wherein the solid content of the polyvinyl alcohol solution is 10-18%; S402: adding a wetting agent, a polyvinyl alcohol solution, a polyvinylidene chloride solution, a curing agent, an organic solvent, and modified nanoparticles into deionized water in sequence while stirring for 40-50 minutes to obtain a barrier coating solution.
[0014] The present invention also discloses a method for preparing a transparent high-barrier film, comprising the following steps: A: The film surface is pretreated by glow discharge, the film coil is treated by active oxygen plasma, vacuumed, introduced with high-purity oxygen, quenched, the film is flattened by a guide roller, and then rolled into a coil to obtain the base layer; B: Apply the barrier coating liquid to the surface of the substrate at 100-120°C and let it react for 3-5 hours; C: A protective layer is coated on the side of the barrier coating layer opposite to the base layer by online coating, and then rolled up after drying to obtain a transparent high-barrier film.
[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The transparent high-barrier film provided by the present invention adopts an aluminum oxide-plated base layer, which significantly enhances the barrier ability of the film to gases such as oxygen and water vapor, effectively prolonging the shelf life and stability of the items in the package. The design of the barrier coating layer further enhances the barrier efficiency of the film, making it perform well in high-humidity or oxygen-sensitive application environments. The introduction of the polyurethane protective layer not only improves the wear resistance and scratch resistance of the film, but also enhances its flexibility and chemical corrosion resistance, making the film less susceptible to damage during packaging and transportation, and maintaining good appearance and functionality. In addition, the proportional design of the thickness of each layer ensures that the film has good mechanical strength and cost-effectiveness while maintaining high barrier properties, meeting the diversified needs of industrial production and application.
[0016] 2. The transparent high-barrier film provided by the present invention is suitable for multiple fields such as food packaging, pharmaceutical packaging, and electronic product protection due to its excellent comprehensive performance, meeting the market's growing demand for high-performance, environmentally friendly packaging materials.
[0017] 3. In the preparation method of the present invention, the fine formula of the barrier coating layer contains a variety of functional additives, such as polyvinyl alcohol, polyvinylidene chloride, modified nanoparticles, etc. This innovative design significantly improves the comprehensive performance of the film. The synergistic effect of PVA and PVDC not only enhances the film's barrier ability to gas and moisture, but also optimizes its heat sealing performance and printability; and the addition of modified nanoparticles further strengthens the film's microstructure, improves its mechanical strength and chemical resistance, and at the same time greatly improves its compatibility and dispersibility with the matrix material, effectively avoiding particle agglomeration, ensuring the uniformity of the film's microstructure, and thus optimizing the overall performance.
[0018] 4. In the preparation method of the present invention, the activity of the film surface is improved by glow discharge pretreatment, which promotes the firm adhesion of the subsequent coating layer, while the precise temperature and pressure control and the application of ultrasonic dispersion, ball milling and other technologies ensure the uniformity of the coating layer and the high-quality production of the film. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The figure is a schematic diagram of the composition structure of a transparent high barrier film of the present invention.
[0020] In the figure: 1, base layer; 2, barrier coating layer; 3, protective layer. DETAILED DESCRIPTION
[0021] Example like Figure 1 As shown, a transparent high barrier film comprises a base layer 1 in the middle, barrier coating layers 2 are arranged on both upper and lower end surfaces of the base layer 1, and a protective layer 3 is arranged on the side of the barrier coating layer 2 opposite to the base layer 1; The thickness of the base layer 1 is 35-75 μm, the thickness of the barrier coating layer 2 is 25-45% of the thickness of the base layer 1, and the thickness of the protective layer 3 is 3-8% of the thickness of the base layer 1; The base layer 1 is an aluminum oxide film; The protective layer 3 is a polyurethane film.
[0022] In this embodiment, the barrier coating liquid includes the following raw materials by weight: 20-30 parts of 11,3,3-tetramethylguanidine, 5-10 parts of xylene, 30-40 parts of 3-chloropropyltrimethoxysilane, 5-10 parts of wetting agent, 5-10 parts of curing agent, 5-10 parts of organic solvent, 30-50 parts of polyvinyl alcohol solution, 10-20 parts of polyvinylidene chloride solution, and 4-7 parts of modified nanoparticles; the solid content of the second protective coating liquid is 10-12%; the modified nanoparticles include the following raw materials by weight: 30-50 parts of azobisisobutyronitrile, 20-30 parts of silicon dioxide, 20-30 parts of zinc oxide, 10-20 parts of divinylbenzene, 8 parts of sodium p-styrene sulfonate, and 10-20 parts of sodium styrene sulfonate. -12 parts, chitosan 15-25 parts, trifluoromethanesulfonic acid 6-8 parts, titanate coupling agent 10-14 parts, methanol 20-28 parts, chlorophyllide ketone acid 20-28 parts, clove essential oil 10-20 parts, end epoxy silicone oil 10-18 parts, anionic emulsifier 8-14 parts; the polyvinyl alcohol solution comprises powdered polyvinyl alcohol and deionized water, and the solid content of the polyvinyl alcohol solution is 10-18%; the solid content of the polyvinylidene chloride solution is 38-42%; the curing agent is melamine curing agent; the wetting agent is a sulfosuccinate surfactant; the organic solvent is ethanol; the anionic emulsifier is one or more of oleic acid and pure sodium lauryl sulfate; the titanate coupling agent is KR-TTS.
[0023] In this embodiment, the preparation method of the barrier coating liquid is: S1: Preparation of nanocarriers: The preparation of the nanocarrier specifically comprises the following steps: S101: Mix 11,3,3-tetramethylguanidine and xylene at 80-100°C, stir and react for 50-70 minutes, add 3-chloropropyltrimethoxysilane, stir and react for 1-2 hours, and filter and wash to obtain material A; S102: placing material A under a pressure of 80-90 mmHg for vacuum distillation, and taking the fraction obtained under a temperature of 125-140° C. as solution A; S103: placing solution A at 95-105°C and 0.8-1.3 MPa under stirring for 18-24 hours, evaporating the solvent to obtain material B; S104: Place azobisisobutyronitrile in tetrahydrofuran at 25-35°C and stir to dissolve, then add silicon dioxide, zinc oxide, divinylbenzene, and sodium p-styrene sulfonate in sequence, and stir at 100-150 r / min for 30-60 min to obtain solution B: S105: placing chitosan in a hydrochloric acid solution and stirring to dissolve, to obtain a solution C; S106: Add solution C and ethanol to material B and mill at a ball milling speed of 500-600 r / min for 30-40 min, add concentrated sulfuric acid and stir to react for 8-12 h, filter, wash and dry to obtain material C; S107: Place material C in toluene at a constant temperature of 85-95°C and stir to react for 3-5h, add trifluoromethanesulfonic acid at a dropping speed of 1-3ml / min, and stir to react for 20-30min while adding. After the addition is completed, continue to stir to react at a stirring speed of 100-200r / min for 1-3h, add titanate coupling agent and continue to stir to react for 1-2h, filter, wash, and vacuum dry to obtain the nanocarrier.
[0024] S2: preparing emulsion; Wherein, preparing the emulsion specifically comprises the following steps: S201: Mix methanol and chlorophyllin acid to obtain a water-based solution; mix clove essential oil and epoxy-terminated silicone oil to obtain an oil-based solution; S202: Pour the water-based solution into the oil-based solution, add an anionic emulsifier, and stir at a high speed of 2000-2200 r / min for 10-15 minutes to obtain an emulsion.
[0025] S3: setting the reaction temperature to 19-24°C and the pressure to 0.01-0.2MPa, placing the nanocarrier in the emulsion for ultrasonic dispersion for 30-60min, and filtering to obtain modified nanoparticles; S4: Synthetic barrier coating fluid.
[0026] The synthesis of the barrier coating liquid specifically includes the following steps: S401: placing powdered polyvinyl alcohol in deionized water and stirring to dissolve to obtain a polyvinyl alcohol solution, wherein the solid content of the polyvinyl alcohol solution is 10-18%; S402: adding a wetting agent, a polyvinyl alcohol solution, a polyvinylidene chloride solution, a curing agent, an organic solvent, and modified nanoparticles into deionized water in sequence while stirring for 40-50 minutes to obtain a barrier coating solution.
[0027] The transparent high-barrier film provided by the present invention adopts an aluminum oxide-plated base layer 1, which significantly enhances the film's barrier ability to gases such as oxygen and water vapor, effectively prolonging the shelf life and stability of the items in the package. The design of the barrier coating layer 2 further enhances the barrier efficiency of the film, making it perform well in high-humidity or oxygen-sensitive application environments. The introduction of the polyurethane protective layer 3 not only improves the film's wear resistance and scratch resistance, but also enhances its flexibility and chemical corrosion resistance, making the film less susceptible to damage during packaging and transportation, and maintaining good appearance and functionality. In addition, the proportional design of the thickness of each layer ensures that the film has good mechanical strength and cost-effectiveness while maintaining high barrier properties, meeting the diversified needs of industrial production and application; due to its excellent comprehensive performance, it is suitable for food packaging, pharmaceutical packaging, electronic product protection and other fields, meeting the market's growing demand for high-performance, environmentally friendly packaging materials.
[0028] The present invention also discloses a method for preparing a transparent high-barrier film, comprising the following steps: A: The film surface is pretreated by glow discharge, the film coil is treated by active oxygen plasma, vacuumed, introduced with high-purity oxygen, quenched, the film is flattened by a guide roller, and then rolled into a coil to obtain a base layer 1; B: Apply the barrier coating liquid to the surface of the substrate layer 1 at 100-120°C and allow to react for 3-5 hours; C: A protective layer 3 is coated on the side of the barrier coating layer 2 opposite to the base layer 1 by online coating, and then rolled up after drying to obtain a transparent high-barrier film.
[0029] The preparation method provided by the present invention comprises a fine formula of the barrier coating layer 2, which comprises a variety of functional additives, such as polyvinyl alcohol, polyvinylidene chloride, modified nanoparticles, etc. This innovative design significantly improves the comprehensive performance of the film. The synergistic effect of PVA and PVDC not only enhances the gas and moisture barrier ability of the film, but also optimizes its heat sealing performance and printability. The addition of modified nanoparticles further strengthens the microstructure of the film, improves its mechanical strength and chemical resistance, and greatly improves its compatibility and dispersibility with the matrix material, effectively avoids particle agglomeration, ensures the uniformity of the film microstructure, and further optimizes the overall performance. The activity of the film surface is enhanced by glow discharge pretreatment, which promotes the firm adhesion of the subsequent coating layer. The precise temperature and pressure control and the application of ultrasonic dispersion, ball milling and other technologies ensure the uniformity of the coating layer and the high-quality production of the film.
[0030] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A transparent high barrier film, characterized in that: It comprises a base layer (1) in the middle, the upper and lower end surfaces of the base layer (1) are both provided with a barrier coating layer (2), and the side of the barrier coating layer (2) opposite to the base layer (1) is both provided with a protective layer (3); The thickness of the base layer (1) is 35-75 μm, the thickness of the barrier coating layer (2) is 25-45% of the thickness of the base layer (1), and the thickness of the protective layer (3) is 3-8% of the thickness of the base layer (1); The base layer (1) is an aluminum oxide film; The protective layer (3) is a polyurethane film; The barrier coating liquid comprises the following raw materials by weight: 20-30 parts of 11,3,3-tetramethylguanidine, 5-10 parts of xylene, 30-40 parts of 3-chloropropyltrimethoxysilane, 5-10 parts of wetting agent, 5-10 parts of curing agent, 5-10 parts of organic solvent, 30-50 parts of polyvinyl alcohol solution, 10-20 parts of polyvinylidene chloride solution, and 4-7 parts of modified nanoparticles; The solid content of the second protective coating liquid is 10-12%.
2. A transparent high barrier film according to claim 1, characterized in that: The modified nanoparticles include the following raw materials by weight: 30-50 parts of azobisisobutyronitrile, 20-30 parts of silicon dioxide, 20-30 parts of zinc oxide, 10-20 parts of divinylbenzene, 8-12 parts of sodium p-styrene sulfonate, 15-25 parts of chitosan, 6-8 parts of trifluoromethanesulfonic acid, 10-14 parts of titanate coupling agent, 20-28 parts of methanol, 20-28 parts of chlorophyll keto acid, 10-20 parts of clove essential oil, 10-18 parts of terminal epoxy silicone oil, and 8-14 parts of anionic emulsifier.
3. A transparent high barrier film according to claim 1, characterized in that: The polyvinyl alcohol solution comprises powdered polyvinyl alcohol and deionized water, and the solid content of the polyvinyl alcohol solution is 10-18%; the solid content of the polyvinylidene chloride solution is 38-42%.
4. A transparent high barrier film according to claim 1, characterized in that: The curing agent is melamine curing agent; the wetting agent is sulfosuccinate surfactant; and the organic solvent is ethanol.
5. The transparent high barrier film according to claim 1, characterized in that: The anionic emulsifier is one or more of oleic acid and pure sodium lauryl sulfate; the titanate coupling agent is KR-TTS.
6. The transparent high barrier film according to claim 1, characterized in that: The preparation method of the barrier coating liquid is: S1: Preparation of nanocarriers: S2: preparing emulsion; S3: setting the reaction temperature to 19-24°C and the pressure to 0.01-0.2MPa, placing the nanocarrier in the emulsion for ultrasonic dispersion for 30-60min, and filtering to obtain modified nanoparticles; S4: Synthetic barrier coating fluid.
7. A transparent high barrier film according to claim 6, characterized in that: In S1, preparing the nanocarrier specifically comprises the following steps: S101: Mix 11,3,3-tetramethylguanidine and xylene at 80-100°C, stir and react for 50-70 minutes, add 3-chloropropyltrimethoxysilane, stir and react for 1-2 hours, and filter and wash to obtain material A; S102: placing material A under a pressure of 80-90 mmHg for vacuum distillation, and taking the fraction obtained under a temperature of 125-140° C. as solution A; S103: placing solution A at 95-105°C and 0.8-1.3 MPa under stirring for 18-24 hours, evaporating the solvent to obtain material B; S104: Place azobisisobutyronitrile in tetrahydrofuran at 25-35°C and stir to dissolve, then add silicon dioxide, zinc oxide, divinylbenzene, and sodium p-styrene sulfonate in sequence, and stir at 100-150 r / min for 30-60 min to obtain solution B: S105: placing chitosan in a hydrochloric acid solution and stirring to dissolve, to obtain a solution C; S106: Add solution C and ethanol to material B and mill at a ball milling speed of 500-600 r / min for 30-40 min, add concentrated sulfuric acid and stir to react for 8-12 h, filter, wash and dry to obtain material C; S107: Place material C in toluene at a constant temperature of 85-95°C and stir to react for 3-5h, add trifluoromethanesulfonic acid at a dropping speed of 1-3ml / min, and stir to react for 20-30min while adding. After the addition is completed, continue to stir to react at a stirring speed of 100-200r / min for 1-3h, add titanate coupling agent and continue to stir to react for 1-2h, filter, wash, and vacuum dry to obtain the nanocarrier.
8. The transparent high barrier film according to claim 6, characterized in that: In said S2, preparing the emulsion specifically comprises the following steps: S201: Mix methanol and chlorophyllin acid to obtain a water-based solution; mix clove essential oil and epoxy-terminated silicone oil to obtain an oil-based solution; S202: Pour the water-based solution into the oil-based solution, add an anionic emulsifier, and stir at a high speed of 2000-2200 r / min for 10-15 minutes to obtain an emulsion.
9. The transparent high barrier film according to claim 6, characterized in that: In S4, synthesizing the barrier coating liquid specifically includes the following steps: S401: placing powdered polyvinyl alcohol in deionized water and stirring to dissolve to obtain a polyvinyl alcohol solution, wherein the solid content of the polyvinyl alcohol solution is 10-18%; S402: adding a wetting agent, a polyvinyl alcohol solution, a polyvinylidene chloride solution, a curing agent, an organic solvent, and modified nanoparticles into deionized water in sequence while stirring for 40-50 minutes to obtain a barrier coating solution.
10. A method for preparing a transparent high barrier film according to any one of claims 1 to 9, characterized in that: The following steps are involved: A: Glow discharge pretreatment is performed on the film surface, active oxygen plasma treatment is performed on the film coil, vacuuming is performed, high-purity oxygen is introduced, and the film is quenched. After the film is flattened by a guide roller, it is rolled into a coil to obtain a base layer (1); B: coating the barrier coating liquid onto the surface of the substrate layer (1) at 100-120°C and allowing to react for 3-5 hours; C: A protective layer (3) is coated on the side of the barrier coating layer (2) opposite to the base layer (1) by online coating, and the film is dried and rolled up to obtain a transparent high-barrier film.
Citation Information
Cited By
Vacuum bag film with high barrier property
CN120697405A