High-performance plastic additive and preparation method thereof

By using a reasonable ratio of bio-based flame retardants and nanomaterials in plastic materials, the performance limitations and environmental issues of traditional plastic materials are solved, the preparation of high-performance plastic additives is achieved, and the flame retardancy and mechanical properties are significantly improved. and antistatic properties, meeting the needs of environmental protection and sustainable development.

CN118772489APending Publication Date: 2024-10-15NINGBO FUTIAN ENG PLASTIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410992134.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional plastic materials have limitations in flame retardancy, mechanical properties, weather resistance and antistatic properties, and existing additives may contain ingredients harmful to the environment and human body, making it difficult to meet the requirements of environmental protection and sustainable development.

Method used

A reasonable combination of bio-based flame retardants, nanosiloxane, epoxy-modified graphene, microencapsulated red phosphorus, metal organic frameworks, self-healing microcapsules, anti-UV agents, antibacterial agents and environmentally friendly plasticizers Ratio, high-performance plastic additives are prepared through efficient preparation processes to improve the comprehensive performance of plastic materials.

Benefits of technology

It significantly improves the flame retardancy, mechanical properties, weather resistance and antistatic properties of plastic materials, reduces environmental burden, complies with environmental protection regulations, extends product service life, and broadens the scope of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772489A_ABST
    Figure CN118772489A_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance plastic additive and a preparation method thereof, and particularly relates to the technical field of plastic additives, and the high-performance plastic additive specifically comprises the following components in parts by weight: 15-25 parts of a bio-based flame retardant, 5-10 parts of nano siloxane, 3-8 parts of epoxy group modified graphene, 5-10 parts of microencapsulated red phosphorus, 3-7 parts of a metal organic framework and 2-5 parts of self-repairing microcapsules. 1-3 parts of an anti-ultraviolet agent, 1-3 parts of an antibacterial agent, 1-2 parts of a compatibility accelerant and 1-2 parts of an environment-friendly plasticizer. According to the high-performance plastic additive disclosed by the invention, the unique bio-based flame retardant is combined with an advanced nano material, so that the flame retardance, mechanical strength and weather resistance of a plastic product are remarkably improved, meanwhile, the antistatic property is optimized, the environmental protection property and sustainability are ensured, and the high-performance plastic additive can be used for various plastic materials and has wide application prospects. The material has excellent comprehensive performance and a wide application range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of plastic additives, and more specifically, to a high-performance plastic additive and a preparation method thereof. Background Art

[0002] In modern society, plastic materials are widely used in many fields such as packaging, construction, automobiles, electronics, etc. due to their advantages such as lightness, durability and cost-effectiveness. However, traditional plastic materials have certain limitations in flame retardancy, mechanical properties, weather resistance and antistatic properties, which restricts their application scope and service life.

[0003] In order to overcome these limitations, it is usually necessary to add additives to plastics to improve their performance. The plastic additives available on the market can often only improve performance in a certain aspect, such as improving flame retardancy or enhancing mechanical strength, but have limited improvements in other aspects. In addition, some additives may contain ingredients that are harmful to the environment and human health, such as halogen compounds and certain heavy metals, which is contrary to the growing global environmental protection requirements.

[0004] With the improvement of environmental protection awareness and the implementation of relevant laws and regulations, it is necessary to develop new high-performance plastic additives that not only have excellent comprehensive performance but also meet the requirements of environmental protection and sustainable development. Therefore, the present invention provides a high-performance plastic additive and a preparation method thereof. By adopting a reasonable ratio of environmentally friendly bio-based flame retardants, nanomaterials and other additives, and an efficient preparation process, the performance of plastic materials is comprehensively improved, while meeting the needs of environmental protection and sustainability. Summary of the invention

[0005] In order to overcome the above defects of the prior art, the present invention provides a high-performance plastic additive and a preparation method thereof to solve the problems raised in the above background technology.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a high-performance plastic additive, specifically comprising the following ingredients and weight portions: 15-25 parts of bio-based flame retardant, 5-10 parts of nano-siloxane, 3-8 parts of epoxy group-modified graphene, 5-10 parts of microencapsulated red phosphorus, 3-7 parts of metal organic framework, 2-5 parts of self-healing microcapsules, 1-3 parts of UV inhibitor, 1-3 parts of antibacterial agent, 1-2 parts of compatibility promoter, and 1-2 parts of environmentally friendly plasticizer.

[0007] Preferably, the following ingredients and weight portions are specifically included: 20 parts of bio-based flame retardant, 8 parts of nano-siloxane, 5 parts of epoxy group-modified graphene, 8 parts of microencapsulated red phosphorus, 5 parts of metal organic framework, 3 parts of self-healing microcapsules, 2 parts of anti-ultraviolet agent, 2 parts of antibacterial agent, 1 part of compatibility promoter, and 1 part of environmentally friendly plasticizer.

[0008] Preferably, the bio-based flame retardant is modified cellulose nanocrystals, the nanosiloxane is used as a reinforcing agent and a water-repellent, the nanosiloxane is surface-modified using a silane coupling agent, the epoxy group-modified graphene is obtained by non-covalently functionalizing π-π interactions or ionic bonds to modify the epoxy group on the graphene surface, and the average particle size of the microencapsulated red phosphorus is between 1-10 μm.

[0009] Preferably, the metal organic framework is a zirconium-based metal organic framework, and heating or vacuum treatment is used to remove solvent molecules or impurities in the metal organic framework. The self-healing microcapsules contain monomers with double bonds as core materials and free radical initiators as wall materials. The anti-ultraviolet agent is a hindered amine light stabilizer, and the antibacterial agent is silver nanoparticles or zinc ion releasers.

[0010] Preferably, the compatibility promoter is maleic anhydride grafted polypropylene, and the environmentally friendly plasticizer is a non-phthalate plasticizer.

[0011] Preferably, the bio-based flame retardant uses any one of wood, cotton, hemp and straw as natural cellulose, which is pretreated by mechanical crushing, alkali treatment or acid treatment to remove impurities and lignin or hemicellulose, and then acid hydrolyzed at 122°C with 1.8% sulfuric acid or hydrochloric acid. After high-speed centrifugation and multiple washing with deionized water, flame retardant functional groups are introduced by grafting reaction, esterification and phosphorylation, specifically including phosphorus, nitrogen and sulfur elements, to obtain modified cellulose nanocrystals.

[0012] A preparation method for preparing the above-mentioned high-performance plastic additive, the method specifically comprises the following steps:

[0013] S1. Raw material preparation and pretreatment:

[0014] S1.1, using wood, cotton, hemp and straw as raw materials, mechanically crushing, alkali treatment to remove impurities and lignin, and then acid hydrolyzing with 1.8% sulfuric acid at 122°C for 2 hours, high-speed centrifugation and multiple washing, and then introducing phosphorus, nitrogen and sulfur elements as flame retardant functional groups through grafting reaction to obtain bio-based flame retardant;

[0015] S2.2, using 1wt% of silane coupling agent to stir the nano-siloxane at room temperature for 2h to obtain surface-modified nano-siloxane;

[0016] S3.3, using non-covalent functionalization to combine π-π interactions or ionic bonds to modify epoxy groups on the graphene surface to obtain epoxy group-modified graphene, with an epoxy compound concentration of 15 wt%, and reacting at room temperature for 1 h;

[0017] S4.4, preparing microencapsulated red phosphorus with an average particle size of 5 μm, coating red phosphorus particles by interfacial polymerization to obtain microencapsulated red phosphorus, wherein the wall material is 10 wt% polyurethane, the reaction temperature is 60°C, and the reaction time is 4 hours;

[0018] S5.5, heating the metal organic framework in a vacuum environment at 180° C. for 8 h to remove solvent molecules in the zirconium-based metal organic framework to obtain a metal organic framework;

[0019] S6.6. Prepare self-healing microcapsules by in-situ polymerization of a monomer having a double bond and a free radical initiator in a mass ratio of 5:1, wherein the monomer having a double bond is a core material, the free radical initiator is a wall material, the reaction temperature is 60°C, and the reaction time is 5h;

[0020] S2, mixing components, mixing the anti-ultraviolet agent and the antibacterial agent in a mixing ratio of 1:1 for 30 minutes to obtain a mixture 1, and mixing the compatibility promoter and the environmentally friendly plasticizer in a ratio of 1:1 for 30 minutes to obtain a mixture 2;

[0021] S3, raw material mixing and extrusion, adding the above-mentioned pretreated raw materials and mixture 1 and mixture 2 into a high-speed mixer and mixing them evenly, and then adding them into a twin-screw extruder for melt blending, the extrusion temperature is set to 200° C., and the screw speed is 400 r / min;

[0022] S4, cooling and granulation, extrude the molten plastic additive through the die head of the extruder, and use a cooling water tank for cooling, granulate with a pelletizer, the cooling water temperature is 20°C, the pelletizer speed is 200r / min, the pellet length is 3mm, and finally the final product is obtained after screening and packaging.

[0023] Preferably, the high-performance plastic additive is used to improve the flame retardancy, mechanical properties, weather resistance and antistatic properties of plastic materials.

[0024] Preferably, the plastic material is polyvinyl chloride, polyethylene, polypropylene and polyethylene terephthalate.

[0025] Technical effects and advantages of the present invention:

[0026] 1. The present invention significantly reduces the environmental burden of plastic products by using bio-based flame retardants and non-phthalate plasticizers, while improving the renewability and sustainability of materials. This not only helps to reduce dependence on fossil resources, but also complies with global environmental regulations and market demand for green products, and contributes to the sustainable development of the plastics industry.

[0027] 2. The plastic additive of the present invention performs well in improving the flame retardancy, mechanical properties, weather resistance and antistatic properties of plastic materials, thereby extending the service life of the product and reducing maintenance costs. This comprehensive improvement in performance enables plastic products to better adapt to various harsh environments and complex applications, and broadens the application scope of plastics in the fields of construction, automobiles, electronics, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is the overall flow chart of the present invention. DETAILED DESCRIPTION

[0029] Embodiment 1,

[0030] This embodiment provides a high-performance plastic additive for improving the flame retardancy, mechanical properties, weather resistance and antistatic properties of plastic materials. The plastic material is polyvinyl chloride, and specifically includes the following components and weight parts: 20 parts of bio-based flame retardant, 8 parts of nano-siloxane, 5 parts of epoxy group-modified graphene, 8 parts of microencapsulated red phosphorus, 5 parts of metal organic framework, 3 parts of self-repairing microcapsules, 2 parts of anti-ultraviolet agent, 2 parts of antibacterial agent, 1 part of compatibility promoter, and 1 part of environmentally friendly plasticizer;

[0031] In this embodiment, the bio-based flame retardant is a modified cellulose nanocrystal, which specifically uses any one of wood, cotton, hemp and straw as natural cellulose, is pretreated by mechanical crushing, alkali treatment or acid treatment to remove impurities and lignin or hemicellulose, and then acid hydrolyzed at 122° C. with 1.8% sulfuric acid or hydrochloric acid, and then centrifuged at high speed and washed multiple times with deionized water, and then flame retardant functional groups are introduced by grafting reaction, esterification and phosphorylation, specifically including phosphorus, nitrogen and sulfur elements, to obtain modified cellulose nanocrystals;

[0032] Nanosiloxane is used as a reinforcing agent and a water-proofing agent, and a silane coupling agent is used to modify the surface of the nanosiloxane;

[0033] Epoxy-modified graphene is obtained by modifying the epoxy group onto the graphene surface through non-covalent functionalization by π-π interaction or ionic bonding;

[0034] The average particle size of microencapsulated red phosphorus is between 1-10 μm;

[0035] The metal organic framework is a zirconium-based metal organic framework, and the solvent molecules or impurities in the metal organic framework are removed by heating or vacuum treatment;

[0036] The self-healing microcapsules contain a monomer with a double bond as a core material and a free radical initiator as a wall material;

[0037] The UV-resistant agent is a hindered amine light stabilizer, and the antimicrobial agent is silver nanoparticles or a zinc ion releaser;

[0038] The compatibility promoter is maleic anhydride grafted polypropylene, and the environmentally friendly plasticizer is a non-phthalate plasticizer.

[0039] This embodiment also provides a method for preparing the above-mentioned high-performance plastic additive, which comprises the following steps:

[0040] S1. Raw material preparation and pretreatment. Wood, cotton, hemp and straw are used as raw materials. They are mechanically crushed and treated with alkali to remove impurities and lignin. Then, they are acid-hydrolyzed with 1.8% sulfuric acid at 122°C for 2 hours. After high-speed centrifugation and multiple washings, phosphorus, nitrogen and sulfur elements are introduced as flame-retardant functional groups through grafting reaction to obtain bio-based flame retardants. This step prepares bio-based flame retardants with high-efficiency flame retardant properties to improve the flame retardancy of plastic materials.

[0041] The nano-siloxane was stirred at room temperature for 2 hours using 1wt% of a silane coupling agent to obtain a surface-modified nano-siloxane; the nano-siloxane was surface-modified using 1wt% of a silane coupling agent to improve its compatibility and dispersibility with a plastic matrix, which helped to improve the overall mechanical properties and waterproof properties of the plastic material.

[0042] Non-covalent functionalization is used to modify the graphene surface with epoxy groups through π-π interaction or ionic bonding to obtain epoxy-modified graphene with an epoxy compound concentration of 15wt% and a reaction time of 1h at room temperature. The epoxy groups are modified on the graphene surface through a non-covalent functionalization method, and π-π interaction or ionic bonding is utilized to enhance the dispersibility and compatibility of graphene in the plastic matrix, thereby further improving the mechanical properties and conductivity of the material.

[0043] Microencapsulated red phosphorus with an average particle size of 5 μm is prepared, and red phosphorus particles are coated by interfacial polymerization to obtain microencapsulated red phosphorus, wherein the wall material is 10wt% polyurethane, the reaction temperature is 60°C, and the reaction time is 4h; red phosphorus particles are coated by interfacial polymerization to prepare microencapsulated red phosphorus with an average particle size of 5 μm. This method can improve the stability and safety of red phosphorus while maintaining its excellent flame retardant properties.

[0044] The metal organic framework is heated to 180°C in a vacuum environment for 8 hours to remove the solvent molecules in the zirconium-based metal organic framework to obtain the metal organic framework; in order to activate the pores of the metal organic framework and enhance its gas adsorption and separation properties, it helps to improve the barrier properties of the plastic material.

[0045] Self-repairing microcapsules are prepared by in-situ polymerization of a monomer with a double bond and a free radical initiator in a mass ratio of 5:1, wherein the monomer with a double bond is the core material, the free radical initiator is the wall material, the reaction temperature is 60°C, and the reaction time is 5 hours. This type of microcapsule can release a repair agent when cracks appear in the plastic material, thereby realizing the self-repair function of the material and extending its service life.

[0046] Specifically, this step prepares and modifies the materials so that the plastic additives have excellent comprehensive properties to meet the needs of modern industry and applications for high-performance plastics.

[0047] S2. Component mixing: the anti-ultraviolet agent and the antibacterial agent are mixed in a mixing ratio of 1:1 for 30 minutes to obtain a mixture 1; the compatibility promoter and the environmentally friendly plasticizer are mixed in a ratio of 1:1 for 30 minutes to obtain a mixture 2.

[0048] In this step, the anti-ultraviolet agent and the antibacterial agent are mixed to improve the anti-ultraviolet and antibacterial properties of the plastic additive, thereby protecting the plastic material from damage by ultraviolet radiation and inhibiting the growth of surface bacteria. The compatibility promoter and the environmentally friendly plasticizer are mixed to improve the compatibility between the additive and the plastic matrix and to improve the flexibility and durability of the final plastic product.

[0049] S3, raw material mixed extrusion, the pretreated raw materials and mixture 1 and mixture 2 are added to a high-speed mixer and mixed evenly, and then added to a twin-screw extruder for melt blending, the extrusion temperature is set to 200° C., and the screw speed is 400 r / min.

[0050] In this step, the purpose of this step is to uniformly disperse the pretreated raw materials including modified bio-based flame retardants, nanosiloxanes, epoxy group-modified graphene, etc., as well as pre-mixed mixture one, such as anti-ultraviolet agents and antibacterial agents and mixture two, such as compatibility promoters and environmentally friendly plasticizers, in the plastic matrix through efficient mixing and melt blending processes, thereby preparing high-performance plastic additives with excellent performance.

[0051] S4, cooling and granulation, extrude the molten plastic additive through the die head of the extruder, and use a cooling water tank for cooling, granulate with a pelletizer, the cooling water temperature is 20°C, the pelletizer speed is 200r / min, the pellet length is 3mm, and finally the final product is obtained after screening and packaging.

[0052] Embodiment 2,

[0053] The present embodiment provides a high-performance plastic additive for improving the flame retardancy, mechanical properties, weather resistance and antistatic properties of plastic materials. The plastic material is polyethylene, and specifically includes the following components and weight portions: 15 parts of bio-based flame retardant, 10 parts of nano-siloxane, 8 parts of epoxy group-modified graphene, 5 parts of microencapsulated red phosphorus, 7 parts of metal organic framework, 2 parts of self-healing microcapsules, 3 parts of anti-ultraviolet agent, 1 part of antibacterial agent, 2 parts of compatibility promoter, and 2 parts of environmentally friendly plasticizer.

[0054] The preparation method of this embodiment is the same as that of embodiment 1, except for the weight proportions of each component.

[0055] Embodiment 3,

[0056] The present embodiment provides a high-performance plastic additive for improving the flame retardancy, mechanical properties, weather resistance and antistatic properties of plastic materials. The plastic material is polypropylene, and specifically includes the following components and weight portions: 25 parts of bio-based flame retardant, 5 parts of nano-siloxane, 3 parts of epoxy group-modified graphene, 10 parts of microencapsulated red phosphorus, 3 parts of metal organic framework, 5 parts of self-repairing microcapsules, 1 part of anti-ultraviolet agent, 3 parts of antibacterial agent, 1 part of compatibility promoter, and 1 part of environmentally friendly plasticizer.

[0057] The preparation method of this embodiment is the same as that of embodiment 1, except for the weight proportions of each component.

[0058] Embodiment 4,

[0059] The present embodiment provides a high-performance plastic additive for improving the flame retardancy, mechanical properties, weather resistance and antistatic properties of plastic materials. The plastic material is polyethylene terephthalate, and specifically includes the following components and weight portions: 20 parts of bio-based flame retardant, 8 parts of nano-siloxane, 5 parts of epoxy group-modified graphene, 8 parts of microencapsulated red phosphorus, 5 parts of metal organic framework, 3 parts of self-healing microcapsules, 2 parts of anti-ultraviolet agent, 2 parts of antibacterial agent, 1 part of compatibility promoter, and 1 part of environmentally friendly plasticizer.

[0060] The preparation method of this embodiment is the same as that of embodiment 1, except for the weight proportions of each component.

[0061] The performance tests were conducted on the plastic additives prepared in the above Examples 1-4, and the existing plastic additives were tested as Comparative Example 1. The results are shown in the following table:

[0062] Among them, flame retardant performance test, test standard: UL-94, test method, by observing the burning behavior of plastic samples under a specific flame source to evaluate its flame retardant performance;

[0063] Mechanical properties test, test standard: ASTM D638, test method, measuring the tensile strength and elongation at break of plastic samples to evaluate their mechanical properties;

[0064] Weathering test, test standard: ASTM G154, test method, evaluates the weathering resistance of plastic samples by cyclic exposure to UV and condensation environments;

[0065] Antistatic performance test, test standard: ASTM D257, test method, measure the surface resistivity of plastic samples to evaluate their antistatic performance.

[0066] Test data table:

[0067]

[0068]

[0069] According to the above table data, the high-performance plastic additive of the present invention shows better performance than existing products in terms of flame retardancy, mechanical properties, weather resistance and antistatic properties, as shown in the following:

[0070] Flame retardant performance: All examples achieved V-0 rating, which is better than the V-2 rating of existing products, proving that the unique bio-based flame retardant formulation of the present invention, including the introduction of modified cellulose nanocrystals, significantly improves the flame retardant ability of plastic materials, all reaching UL-94 V-0 rating, providing a higher level of fire safety protection for plastic products;

[0071] Mechanical properties: The tensile strength and elongation at break of the examples are generally higher than those of existing products, proving that the present invention effectively improves the tensile strength and elongation at break of plastics by adding nanomaterials such as nanosiloxane and epoxy-modified graphene, making the product more durable and tear-resistant;

[0072] Weatherability: The mass loss percentage of the embodiment is lower than that of the existing product, indicating better weatherability, proving that the weatherability additives designed by the present invention, such as the hindered amine light stabilizer, protect the plastic material from degradation by ultraviolet rays and environmental factors, and extend the service life of the product;

[0073] Antistatic performance: The surface resistivity of the embodiments is generally lower than that of existing products, indicating better antistatic performance. This proves that the present invention reduces static electricity accumulation by increasing the surface resistivity of plastics, thereby reducing the risk of electrostatic interference of plastic products in electronic and precision industrial applications.

[0074] In summary, the high-performance plastic additive of the present invention significantly improves the flame retardancy, mechanical strength and weather resistance of plastic products through the unique combination of bio-based flame retardants and advanced nanomaterials, while optimizing the antistatic performance, ensuring environmental protection and sustainability, and can be used for a variety of plastic materials, with excellent comprehensive performance and a wide range of applications. Its efficient preparation process further guarantees the high quality and market competitiveness of the product, providing a high-performance, economical and environmentally friendly plastic additive solution for modern industry and applications.

[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-performance plastic additive, It is characterized in that Specifically, it includes the following ingredients and their weight proportions: 15-25 parts of bio-based flame retardant, 5-10 parts of nano-siloxane, 3-8 parts of epoxy group-modified graphene, 5-10 parts of microencapsulated red phosphorus, 3-7 parts of metal organic framework, 2-5 parts of self-healing microcapsules, 1-3 parts of UV inhibitor, 1-3 parts of antibacterial agent, 1-2 parts of compatibility promoter, and 1-2 parts of environmentally friendly plasticizer.

2. The high performance plastic additive according to claim 1, Features: Specifically, it includes the following ingredients and their weight proportions: 20 parts of bio-based flame retardant, 8 parts of nano-siloxane, 5 parts of epoxy group-modified graphene, 8 parts of microencapsulated red phosphorus, 5 parts of metal organic framework, 3 parts of self-healing microcapsules, 2 parts of UV inhibitor, 2 parts of antibacterial agent, 1 part of compatibility promoter and 1 part of environmentally friendly plasticizer.

3. The high performance plastic additive according to claim 2, Features: The bio-based flame retardant is modified cellulose nanocrystals, the nanosiloxane is used as a reinforcing agent and a waterproofing agent, a silane coupling agent is used to perform surface modification on the nanosiloxane, the epoxy group-modified graphene is obtained by modifying the epoxy group to the graphene surface through non-covalent functionalization to combine π-π interactions or ionic bonds, and the average particle size of the microencapsulated red phosphorus is between 1 and 10 μm.

4. The high performance plastic additive according to claim 3, Features: The metal organic framework is a zirconium-based metal organic framework, and heating or vacuum treatment is used to remove solvent molecules or impurities in the metal organic framework. The self-repairing microcapsule contains a monomer with a double bond as a core material and a free radical initiator as a wall material. The anti-ultraviolet agent is a hindered amine light stabilizer, and the antibacterial agent is silver nanoparticles or a zinc ion releaser.

5. The high performance plastic additive according to claim 4, Features: The compatibility promoter is maleic anhydride grafted polypropylene, and the environmentally friendly plasticizer is a non-phthalate plasticizer.

6. The high performance plastic additive according to claim 5, Features: The bio-based flame retardant uses any one of wood, cotton, hemp and straw as natural cellulose, pre-treats it by mechanical crushing, alkali treatment or acid treatment to remove impurities and lignin or hemicellulose, then uses 1.8% sulfuric acid or hydrochloric acid to acid hydrolyze it at 122°C, centrifuges it at high speed and washes it multiple times with deionized water, and then uses grafting reaction, esterification and phosphorylation to introduce flame retardant functional groups, specifically including phosphorus, nitrogen and sulfur elements, to obtain modified cellulose nanocrystals.

7. A preparation method for preparing the high-performance plastic additive according to claim 6, Features: The method specifically comprises the following steps: S1. Raw material preparation and pretreatment: S1.1, using wood, cotton, hemp and straw as raw materials, mechanically crushing, alkali treatment to remove impurities and lignin, and then acid hydrolyzing with 1.8% sulfuric acid at 122°C for 2 hours, high-speed centrifugation and multiple washing, and then introducing phosphorus, nitrogen and sulfur elements as flame retardant functional groups through grafting reaction to obtain bio-based flame retardant; S2.2, using 1wt% of silane coupling agent to stir the nano-siloxane at room temperature for 2h to obtain surface-modified nano-siloxane; S3.3, using non-covalent functionalization to combine π-π interactions or ionic bonds to modify epoxy groups on the graphene surface to obtain epoxy group-modified graphene, with an epoxy compound concentration of 15 wt%, and reacting at room temperature for 1 h; S4.4, preparing microencapsulated red phosphorus with an average particle size of 5 μm, coating red phosphorus particles by interfacial polymerization to obtain microencapsulated red phosphorus, wherein the wall material is 10 wt% polyurethane, the reaction temperature is 60°C, and the reaction time is 4 hours; S5.5, heating the metal organic framework in a vacuum environment at 180° C. for 8 h to remove solvent molecules in the zirconium-based metal organic framework to obtain a metal organic framework; S6.

6. Prepare self-healing microcapsules by in-situ polymerization of a monomer having a double bond and a free radical initiator in a mass ratio of 5:1, wherein the monomer having a double bond is a core material, the free radical initiator is a wall material, the reaction temperature is 60°C, and the reaction time is 5h; S2, mixing components, mixing the anti-ultraviolet agent and the antibacterial agent in a mixing ratio of 1:1 for 30 minutes to obtain a mixture 1, and mixing the compatibility promoter and the environmentally friendly plasticizer in a ratio of 1:1 for 30 minutes to obtain a mixture 2; S3, raw material mixing and extrusion, adding the above-mentioned pretreated raw materials and mixture 1 and mixture 2 into a high-speed mixer and mixing them evenly, and then adding them into a twin-screw extruder for melt blending, the extrusion temperature is set to 200° C., and the screw speed is 400 r / min; S4, cooling and granulation, extrude the molten plastic additive through the die head of the extruder, and use a cooling water tank for cooling, granulate with a pelletizer, the cooling water temperature is 20°C, the pelletizer speed is 200r / min, the pellet length is 3mm, and finally the final product is obtained after screening and packaging.

8. The preparation method according to claim 7, Features: The high-performance plastic additive is used for improving the flame retardancy, mechanical properties, weather resistance and antistatic properties of plastic materials.

9. The preparation method according to claim 8, Features: The plastic material is polyvinyl chloride, polyethylene, polypropylene and polyethylene terephthalate.