Foaming phenolic resin

By using raw materials such as phenolic resin, carbon black and polyurethane in the production of foamed phenolic resin, combined with the ratio and preparation method of foaming agent, surfactant and curing agent, the curing speed problem in the existing technology is solved. It solves the problem of slowness, improves the stability and performance of the resin, and achieves more efficient production and service life.

CN118772571APending Publication Date: 2024-10-15HEFEI HAIFU NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410949172.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The curing speed of the existing foamed phenolic resin in the production process is slow, resulting in poor stability, and the production rate and stability need to be improved.

Method used

It uses phenolic resin, carbon black and polyurethane as the main raw materials, and adds foaming agent, surfactant, plasticizer and curing agent. It foams and solidifies by stirring, heating and pressurizing, and controls the temperature. And the pressure is in the range of 55-65℃ and 1.0-1.2MPA, add catalysts and flame retardants to improve the reaction rate and stability.

Benefits of technology

Significantly improve the production rate and stability of foamed phenolic resin, improve the performance of the resin, enhance the curing speed and flame resistance, and extend the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772571A_ABST
    Figure CN118772571A_ABST
Patent Text Reader

Abstract

The invention discloses foamed phenolic resin, and relates to the technical field of industrial resin, the foamed phenolic resin is prepared from the following raw materials in parts by mass: 80-100 parts of phenolic resin, 50-60 parts of carbon black, 30-40 parts of polyurethane and auxiliary raw materials, and the auxiliary raw materials comprise 5-10 parts of a foaming agent, 3-5 parts of a surfactant, 3-5 parts of a plasticizer and 5-10 parts of a curing agent. The foaming agent, the surfactant, the plasticizer and the curing agent are added into the auxiliary raw materials, and a reasonable proportion and a preparation method are adopted for production. The surfactant can increase the molecular activity of the raw materials and further improve the foaming reaction among the raw materials, and the plasticizer can change the interaction force among resin molecules, so that the curing reaction is accelerated, the performance of the phenolic resin is effectively improved, the curing speed is increased, and the production rate and stability of the foamed phenolic resin are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of industrial resins, in particular to foamed phenolic resins. Background Art

[0002] Foamed phenolic resin is a kind of foamed plastic obtained by foaming phenolic resin. Compared with the materials that dominated the market in the early days, such as polystyrene foam, polyvinyl chloride foam, polyurethane foam, etc., it has excellent flame retardant properties and is an ideal insulation material for electrical appliances, instruments, construction, petrochemicals and other industries, so it has been widely valued by people.

[0003] After searching, the Chinese patent publication number is CN111825817A, which discloses a method for preparing a highly active foaming phenolic resin and a neutral phenolic foam, belonging to the technical field of organic chemistry. The method for preparing the highly active foaming phenolic resin comprises the following steps: weighing a certain amount of phenol, liquid formaldehyde and an alkaline catalyst and adding them into a reaction bottle, reacting at 70 to 90°C for a period of time, cooling to 50 to 60°C, and then adding carbonamide and hexamethylenetetramine to react at a constant temperature for 20 to 40 minutes.

[0004] The prior art is similar to the above-mentioned foamed phenolic resin, which is made of phenol and liquid formaldehyde as main raw materials. However, the foamed phenolic resin made by this method has poor stability due to the slow curing speed during the production process, so there is room for improvement. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a foaming phenolic resin. The advantages of the present invention are that the production rate and stability of the foaming phenolic resin are improved.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The foamed phenolic resin comprises the following raw materials in parts by weight: 80-100 parts of phenolic resin, 50-60 parts of carbon black, 30-40 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 5-10 parts of foaming agent, 3-5 parts of surfactant, 3-5 parts of plasticizer and 5-10 parts of curing agent.

[0008] Preferably, the raw material composition includes the following parts by mass: 80 parts of phenolic resin, 50 parts of carbon black, 30 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 5 parts of foaming agent, 3 parts of surfactant, 3 parts of plasticizer and 5 parts of curing agent.

[0009] Preferably, the raw material composition includes the following parts by mass: 90 parts of phenolic resin, 55 parts of carbon black, 35 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 7.5 parts of foaming agent, 4 parts of surfactant, 4 parts of plasticizer and 7.5 parts of curing agent.

[0010] Preferably, the raw material composition includes the following parts by mass: 100 parts of phenolic resin, 60 parts of carbon black, 40 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 10 parts of foaming agent, 5 parts of surfactant, 5 parts of plasticizer and 10 parts of curing agent.

[0011] Preferably, the surfactant is at least one of dodecylbenzenesulfonic acid, sodium oleate and octadecene.

[0012] Preferably, the plasticizer is at least one of liquid stearic acid, polyol benzoate and chlorinated paraffin.

[0013] The preparation method of the foamed phenolic resin comprises the following steps:

[0014] Step 1: First, prepare phenolic resin, carbon black, polyurethane and auxiliary raw materials according to certain mass fractions, wherein the auxiliary raw materials include foaming agent, surfactant, plasticizer and curing agent, add phenolic resin, carbon black and polyurethane among these raw materials into a mixing tank, and stir them by using a stirring device;

[0015] Step 2: After stirring evenly, use a heating device to heat the mixing tube. When it reaches a certain temperature, add the foaming agent, surfactant and plasticizer and continue to stir and mix. After mixing, keep warm for a period of time, and then continue to heat to a certain temperature and pressurize the mixing tank. As the pressure increases, the raw materials slowly foam in the mixing tank;

[0016] Step 3: After the raw materials are completely foamed, add the curing agent, then stir, and slowly solidify as the temperature rises to obtain the foamed phenolic resin.

[0017] The present invention is further configured such that the insulation temperature is 55-65 degrees Celsius, the foaming temperature is 120-140 degrees Celsius, and the pressure is 1.0-1.2 MPA.

[0018] The present invention is further configured that a certain amount of catalyst can be added during the foaming process, and the catalyst is manganese dioxide.

[0019] The present invention is further configured that the raw material also includes a flame retardant, and the flame retardant is prepared by mixing ammonium polyphosphate, pentaerythritol and melamine in a ratio of 3:3:4 by mass.

[0020] The beneficial effects of the present invention are:

[0021] The invention discloses a foaming phenolic resin, which is produced by using phenolic resin, carbon black and polyurethane as main raw materials, adding a foaming agent, a surfactant, a plasticizer and a curing agent into auxiliary raw materials, and adopting a reasonable ratio and a preparation method; the surfactant can increase the molecular activity of each raw material, thereby improving the foaming reaction between the raw materials, and the plasticizer can change the interaction force between resin molecules, thereby accelerating the curing reaction, effectively improving the performance of the phenolic resin, and increasing the curing speed, thereby significantly improving the production rate and stability of the foaming phenolic resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the raw material composition of the foamed phenolic resin proposed in the present invention;

[0023] Figure 2 The present invention is a schematic diagram of the preparation process of the foamed phenolic resin. DETAILED DESCRIPTION

[0024] The technical solution of this patent is further described in detail below in conjunction with specific implementation methods.

[0025] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0026] In the description of this patent, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing this patent and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this patent.

[0027] In the description of this patent, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "set" should be understood in a broad sense, for example, it can be fixedly connected or set, or it can be detachably connected or set, or connected or set in one piece. For ordinary technicians in this field, the specific meanings of the above terms in this patent can be understood according to specific circumstances.

[0028] Embodiment 1

[0029] Reference Figure 1, foamed phenolic resin, including the following raw materials in parts by mass: 80-100 parts of phenolic resin, 50-60 parts of carbon black, 30-40 parts of polyurethane and auxiliary raw materials, the auxiliary raw materials include 5-10 parts of foaming agent, 3-5 parts of surfactant, 3-5 parts of plasticizer and 5-10 parts of curing agent.

[0030] Embodiment 2

[0031] Reference Figure 1 The foamed phenolic resin includes the following raw materials in parts by mass: 80 parts of phenolic resin, 50 parts of carbon black, 30 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 5 parts of foaming agent, 3 parts of surfactant, 3 parts of plasticizer and 5 parts of curing agent.

[0032] Embodiment 3

[0033] Reference Figure 1 The foamed phenolic resin includes the following raw materials in parts by mass: 90 parts of phenolic resin, 55 parts of carbon black, 35 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 7.5 parts of foaming agent, 4 parts of surfactant, 4 parts of plasticizer and 7.5 parts of curing agent.

[0034] Embodiment 4

[0035] Reference Figure 1 The foamed phenolic resin includes the following raw materials in parts by mass: 100 parts of phenolic resin, 60 parts of carbon black, 40 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 10 parts of foaming agent, 5 parts of surfactant, 5 parts of plasticizer and 10 parts of curing agent.

[0036] In the above embodiment, the surfactant is at least one of dodecylbenzenesulfonic acid, sodium oleate and octadecene; and the plasticizer is at least one of liquid stearic acid, polyol benzoate and chlorinated paraffin.

[0037] Reference Figure 2 , a method for preparing a foamed phenolic resin comprises the following steps:

[0038] Step 1: First, prepare phenolic resin, carbon black, polyurethane and auxiliary raw materials according to certain mass fractions, the auxiliary raw materials include foaming agent, surfactant, plasticizer and curing agent, add phenolic resin, carbon black and polyurethane among these raw materials into a mixing tank together, and stir them with a stirring device;

[0039] Step 2: After stirring evenly, use a heating device to heat the mixing tube. When it reaches a certain temperature, add the foaming agent, surfactant and plasticizer and continue to stir and mix. After mixing, keep warm for a period of time, and then continue to heat to a certain temperature and pressurize the mixing tank. As the pressure increases, the raw materials slowly foam in the mixing tank;

[0040] Step 3: After the raw materials are completely foamed, add the curing agent, then stir, and slowly solidify as the temperature rises to obtain the foamed phenolic resin.

[0041] Furthermore, the insulation temperature is 55-65 degrees Celsius, preferably 60 degrees Celsius, the foaming temperature is 120-140 degrees Celsius, preferably 130 degrees Celsius, and the pressure is 1.0-1.2MPA, preferably 1.1MPA. Within these temperature and pressure ranges, the production rate of the foamed phenolic resin is optimal; a certain amount of catalyst can be added during the foaming process, the catalyst is manganese dioxide, and the catalyst can further increase the reaction rate of foaming and curing.

[0042] Embodiment 5

[0043] Reference Figure 2 , a method for preparing a foamed phenolic resin comprises the following steps:

[0044] Step 1: First, prepare phenolic resin, carbon black, polyurethane and auxiliary raw materials according to certain mass fractions, the auxiliary raw materials include foaming agent, surfactant, plasticizer and curing agent, add phenolic resin, carbon black and polyurethane among these raw materials into a mixing tank together, and stir them with a stirring device;

[0045] Step 2: After stirring evenly, use a heating device to heat the mixing tube. When it reaches a certain temperature, add the foaming agent, surfactant, flame retardant and plasticizer and continue to stir and mix. After mixing, keep warm for a period of time, and then continue to heat to a certain temperature and pressurize the mixing tank. As the pressure increases, the raw materials slowly foam in the mixing tank;

[0046] Step 3: After the raw materials are fully foamed, add the curing agent, then stir, and slowly solidify as the temperature rises to obtain the foamed phenolic resin

[0047] The flame retardant is prepared by mixing ammonium polyphosphate, pentaerythritol and melamine in a weight ratio of 3:3:4, and the weight fraction of the flame retardant is 3-5 parts. The flame retardant can increase the flame resistance of the foamed phenolic resin and significantly improve the service life of the foamed phenolic resin when in use.

[0048] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. Foamed phenolic resin, It is characterized in that The invention comprises the following raw materials in parts by weight: 80-100 parts of phenolic resin, 50-60 parts of carbon black, 30-40 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 5-10 parts of foaming agent, 3-5 parts of surfactant, 3-5 parts of plasticizer and 5-10 parts of curing agent.

2. The foamed phenolic resin according to claim 1, It is characterized in that The invention comprises the following raw materials in parts by weight: 80 parts of phenolic resin, 50 parts of carbon black, 30 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 5 parts of foaming agent, 3 parts of surfactant, 3 parts of plasticizer and 5 parts of curing agent.

3. The foamed phenolic resin according to claim 1, It is characterized in that The composition includes the following raw materials in parts by weight: 90 parts of phenolic resin, 55 parts of carbon black, 35 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 7.5 parts of foaming agent, 4 parts of surfactant, 4 parts of plasticizer and 7.5 parts of curing agent.

4. The foamed phenolic resin according to claim 1, It is characterized in that The invention comprises the following raw materials in parts by weight: 100 parts of phenolic resin, 60 parts of carbon black, 40 parts of polyurethane and auxiliary raw materials, wherein the auxiliary raw materials include 10 parts of foaming agent, 5 parts of surfactant, 5 parts of plasticizer and 10 parts of curing agent.

5. The foamed phenolic resin according to any one of claims 2 to 4, It is characterized in that The surfactant is at least one of dodecylbenzenesulfonic acid, sodium oleate and octadecene.

6. The foamed phenolic resin according to claim 5, It is characterized in that The plasticizer is at least one of liquid stearic acid, polyol benzoate and chlorinated paraffin.

7. A method for preparing a foamed phenolic resin as claimed in claim 6, It is characterized in that The following steps are involved: Step 1: First, prepare phenolic resin, carbon black, polyurethane and auxiliary raw materials according to certain mass fractions, wherein the auxiliary raw materials include foaming agent, surfactant, plasticizer and curing agent, add phenolic resin, carbon black and polyurethane among these raw materials into a mixing tank, and stir them by using a stirring device; Step 2: After stirring evenly, use a heating device to heat the mixing tube. When it reaches a certain temperature, add the foaming agent, surfactant and plasticizer and continue to stir and mix. After mixing, keep warm for a period of time, and then continue to heat to a certain temperature and pressurize the mixing tank. As the pressure increases, the raw materials slowly foam in the mixing tank; Step 3: After the raw materials are completely foamed, add the curing agent, then stir, and slowly solidify as the temperature rises to obtain the foamed phenolic resin.

8. The method for preparing the foamed phenolic resin according to claim 7, It is characterized in that The insulation temperature is 55-65 degrees Celsius, the foaming temperature is 120-140 degrees Celsius, and the pressure is 1.0-1.2 MPA.

9. The method for preparing the foamed phenolic resin according to claim 8, It is characterized in that A certain amount of catalyst can be added during the foaming process, and the catalyst is manganese dioxide.

10. The method for preparing the foamed phenolic resin according to claim 9, It is characterized in that The raw materials also include a flame retardant, which is prepared by mixing ammonium polyphosphate, pentaerythritol and melamine in a ratio of 3:3:4 by weight.