Polyvinyl acetal type binder and preparation and application of battery pole piece of polyvinyl acetal type binder
Through the preparation of polyvinyl acetal-type binders, the problem of stress and strain caused by volume changes in the battery during charging and discharging is solved, the stability of the electrode and battery performance are improved, and more efficient electric energy storage is achieved.
Patent Information
- Application Number
- CN202410971560.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
AI Technical Summary
The volume change of existing batteries due to ion intercalation/deintercalation during the charging and discharging process leads to pulverization of the pole pieces and failure of the electrical contact between the active material and the current collector, resulting in irreversible capacity loss and battery failure, which cannot be effectively alleviated by the binder. Stress and strain caused by volume expansion.
It uses polyvinyl acetal type binder and is prepared through acetal reaction under catalyst conditions to generate a polymer with strong adhesion and high mechanical properties. It is used in the preparation of battery electrodes to relieve the stress caused by volume expansion. strain to improve electrode stability.
It improves the adhesion between the active material and the current collector, enhances the mechanical properties of the electrode, extends the cycle life of the battery, and improves the overall performance and stability of the battery.
Smart Images

Figure CN118772802A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rechargeable batteries, and in particular relates to the preparation of a polyvinyl acetal binder and the application of the binder in a negative electrode of a battery. Background Art
[0002] Non-renewable traditional fossil fuels can neither meet the growing energy demand nor cause pollution to the ecological environment. Electric energy storage is a promising technology that can store and convert intermittent energy (such as solar energy, wind energy, and tidal energy) to achieve continuous and efficient energy supply and reduce dependence on traditional fossil fuels. In existing electric energy storage systems, rechargeable batteries can achieve efficient conversion between electrical energy and chemical energy, providing a promising solution for the development of efficient and convenient green renewable energy storage systems.
[0003] However, during the charge and discharge process of the secondary battery, the large volume change caused by the embedding / de-embedding of ions will lead to a series of problems, including the pulverization of the pole piece, the failure of the electrical contact between the active material and the current collector, etc., which will cause irreparable capacity loss and even lead to battery failure. Therefore, although the binder accounts for a small proportion of the pole piece as a whole, its performance directly affects the battery performance. Currently, commonly used binders are polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC), etc., but these binders are usually unable to alleviate large volume changes, resulting in damage to the pole piece structure. In order to solve the above technical difficulties, the present application provides a simple and efficient method for preparing a polyvinyl acetal binder, which has strong adhesion and strong mechanical properties to alleviate the stress and strain caused by volume expansion during the cycle, thereby improving the stability of the electrode and improving the battery performance. Summary of the invention
[0004] The present invention aims to provide a simple and efficient preparation of a polyvinyl acetal type binder, and its application in battery pole pieces. The binder described in the present invention has strong adhesion, and has the advantages of high efficiency, low cost, strong operability, etc. The prepared polyvinyl acetal type binder can be used in the preparation of negative electrodes of rechargeable batteries. The prepared binder improves the adhesion between the active material and the current collector, and has strong mechanical properties, which can alleviate the stress and strain caused by volume expansion during the cycle, thereby improving the stability of the electrode and improving the battery performance.
[0005] The invention provides a polyvinyl acetal binder and preparation and application of a battery pole piece thereof. The polyvinyl acetal binder is a polymer product obtained by acetalization reaction of polyvinyl alcohol and various aldehydes under catalyst conditions.
[0006] Furthermore, the degree of polymerization of the polyvinyl alcohol is one or more of ultra-high degree of polymerization (molecular weight of 250,000 to 300,000), high degree of polymerization (molecular weight of 150,000 to 250,000), medium degree of polymerization (molecular weight of 70,000 to 150,000), and low degree of polymerization (molecular weight of 10,000 to 70,000).
[0007] Furthermore, the alcoholysis degree of the polyvinyl alcohol is one or more of 50% to 100%.
[0008] Furthermore, the aldehydes are aldehydes of the general formula RCHO. n H 2n O (n ≥ 2) monobasic saturated aldehydes: one or more of formaldehyde, acetaldehyde, propionaldehyde, valeraldehyde, hexanal, etc.; acyclic aliphatic aldehydes: one or more of octanal, nonanal, decanal, undecanal, lauric aldehyde (dodecane), tridecanal, myristic aldehyde (tetradecane), etc.; alicyclic aldehydes: one or more of privet aldehyde, ivinal, isocyclic citral, citric aldehyde, methyl citric aldehyde, lyral, etc.; aromatic aldehydes: one or more of benzaldehyde, phenylacetaldehyde, phenylpropionaldehyde, cinnamaldehyde, lily of the valley aldehyde, vanillin, ethyl vanillin, etc.; terpene aldehydes: one or more of citral, citronellal, hydroxycitronellal, perillaldehyde, trimethylheptenal, etc.
[0009] Furthermore, the aldehyde solution accounts for 0.01wt% to 30wt% of the polyvinyl alcohol solution.
[0010] Furthermore, the catalyst is one or more of an inorganic acid (hydrochloric acid, sulfuric acid, etc.) or an organic acid (R-COOH, R-SO3H, etc.).
[0011] The present invention also provides a method for preparing a pole piece from polyvinyl acetal, comprising the following steps:
[0012] Step 1: Heat and stir polyvinyl alcohol in water until it is completely dissolved to obtain a transparent and uniform polyvinyl alcohol aqueous solution.
[0013] Step 2: Under the catalytic action of an acidic catalyst, polyvinyl alcohol and aldehydes undergo a one-step acetalization reaction.
[0014] Step 3: Perform acetalization reaction at 20-200°C until the reaction becomes viscous and produces insoluble cross-linked flocs.
[0015] Step 4: Neutralize the residual acidic catalyst with alkali until the pH value of the system is 7-10.
[0016] Step 5: After washing and drying, the polyethanol acetal polymer is obtained.
[0017] Furthermore, the heating temperature in step 1 is 20-200°C.
[0018] Furthermore, the acidic catalyst in step 2 is one or more of an inorganic acid (hydrochloric acid, sulfuric acid, etc.) or an organic acid (R-COOH, R-SO3H, etc.).
[0019] Furthermore, in step 2, the pH value of the system is 1-5.
[0020] Furthermore, the reaction time in step three is 5 minutes to 48 hours.
[0021] Furthermore, the base in step 4 is one or more of sodium hydroxide, lithium hydroxide, potassium hydroxide, barium hydroxide, ammonia water, Schiff base, etc.
[0022] The invention also provides a method for preparing a pole piece from polyvinyl acetal, which comprises an active substance, a conductive agent and a binder.
[0023] Furthermore, the active material is one or more of graphite carbon materials, disordered carbon materials, lithium titanate materials, silicon-based materials, carbonyl compounds, Schiff base compounds, organic free radical compounds, organic sulfides, metal sulfur compounds, zinc powder, lithium cobalt oxide, lithium iron phosphate, lithium manganate, ternary materials lithium nickel cobalt manganate and lithium nickel cobalt aluminum oxide, transition metal oxides, polyanion materials, Prussian blue compounds, organic molecules and polymers, amorphous materials, vanadium-based, manganese-based compounds, Prussian blue analogs and organic compounds.
[0024] Furthermore, the conductive agent is one or more of carbon black, conductive graphite, carbon fiber, carbon nanotube, and graphene.
[0025] Furthermore, the binder is soluble in one or more organic solutions such as alcohols such as methanol, ethanol, and butanol, ketones such as cyclohexanone, butanone, and N-methylpyrrolidone, aromatic hydrocarbons, benzene, toluene, xylene, chlorinated hydrocarbons such as ethyl chloride and dichloroethane, formic acid, acetic acid, furfural, phenols, and azobenzenes.
[0026] Furthermore, the ratio of the active material, the conductive agent and the binder is (7-9.5): (0.3-2): (0.2-1).
[0027] The beneficial effects of the present invention are:
[0028] The binder preparation method of the present invention is simple and efficient, and the obtained binder has strong bonding properties, and has the advantages of high efficiency, low cost, strong operability, etc. The prepared polyvinyl acetal binder can be used in the preparation of pole pieces of secondary batteries. The prepared binder improves the adhesion between the active material and the current collector, and has strong mechanical properties, which can alleviate the stress and strain caused by volume expansion during the cycle, thereby improving the stability of the electrode and improving the battery performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The infrared spectra of the binders used in Example 1 and Comparative Example 1 are shown in FIG.
[0030] Figure 2 This is a tensile test of the negative electrodes of Example 1 and Comparative Example 1.
[0031] Figure 3 This is the puncture test of the negative electrode of Example 1 and Comparative Example 1.
[0032] Figure 4 It is the rate diagram of the negative electrode of Example 1 and Comparative Example 1.
[0033] Figure 5 The negative electrode of Example 1 and Comparative Example 1 is 1Ag -1 The cycle diagram below. DETAILED DESCRIPTION
[0034] In order to make the contents described in the present invention easier to understand, the technical solutions described in the present invention are further described and explained in conjunction with specific implementation methods below. However, the present invention is not limited to this. All technologies realized based on the above contents of the present invention are included in the scope that the present invention is intended to protect.
[0035] Example 1
[0036] A preparation method for a negative electrode of a zinc ion battery comprises the following steps:
[0037] Polyvinyl alcohol with a mass ratio of 1:9 is dissolved in water to form a transparent uniform solution, 5wt% of formaldehyde is added, and the pH value of the solution is adjusted to 3 with hydrochloric acid. After insoluble floccules are generated, the acid is washed away with sodium hydroxide, and polyvinyl alcohol formal is obtained after washing with water and drying.
[0038] The active material (zinc powder) and the conductive agent (carbon black) are added to the polyvinyl formal solution, wherein the mass ratio of zinc powder, carbon black and polyvinyl formal is 8:1:1. After stirring evenly, the slurry is scraped and dried at 80°C to obtain the negative electrode sheet, and the battery is assembled.
[0039] Example 2
[0040] A preparation method for a positive electrode of a lithium ion battery comprises the following steps:
[0041] Polyvinyl alcohol with a mass ratio of 2:8 is dissolved in water to form a transparent uniform solution, 10wt% of acetaldehyde is added, and the pH of the solution is adjusted to 2 with sulfuric acid. After insoluble floccules are generated, lithium hydroxide is used to wash away the participating acid, and polyvinyl acetal is obtained after washing with water and drying.
[0042] The active material (lithium iron phosphate) and the conductive agent (carbon black) are added to the polyvinyl acetal solution, wherein the mass ratio of lithium iron phosphate, carbon black and polyvinyl acetal is 8:1:1. After stirring evenly, the slurry is scraped and dried at 80°C to obtain the positive electrode sheet, and the battery is assembled.
[0043] Example 3
[0044] A preparation method for a negative electrode of a lithium ion battery comprises the following steps:
[0045] Polyvinyl alcohol with a mass ratio of 1.5:8.5 is dissolved in water to form a transparent uniform solution, 8wt% of acetaldehyde is added, and the pH value of the solution is adjusted to 1 with hydrochloric acid. After insoluble floccules are generated, the acid is washed away with ammonia water, and polyvinyl acetal is obtained after washing with water and drying.
[0046] The active material (lithium titanate) and the conductive agent (carbon black) are added to the polyvinyl acetal solution, wherein the mass ratio of lithium titanate, carbon black and polyvinyl acetal is 8.5:0.5:1. After stirring evenly, the slurry is scraped and dried at 80°C to obtain the negative electrode sheet, and the battery is assembled.
[0047] Example 4
[0048] A preparation method for a positive electrode of a lithium ion battery comprises the following steps:
[0049] Polyvinyl alcohol with a mass ratio of 3:7 is dissolved in water to form a transparent uniform solution, 3wt% of butyraldehyde is added, and the pH value of the solution is adjusted to 2 with sulfuric acid. After insoluble floccules are generated, potassium hydroxide is used to wash away the acid, and polyvinyl butyral is obtained after washing with water and drying.
[0050] The active material (lithium nickel cobalt manganese oxide) and the conductive agent (carbon black) are added to the polyvinyl butyral solution, wherein the mass ratio of lithium nickel cobalt manganese oxide, carbon black and polyvinyl butyral is 9:0.5:0.5. After stirring evenly, the slurry is scraped and dried at 80°C to obtain the positive electrode sheet, and the battery is assembled.
[0051] Example 5
[0052] A preparation method for a negative electrode of a lithium ion battery comprises the following steps:
[0053] Take polyvinyl alcohol with a mass ratio of 2:8 and dissolve it in water to form a transparent uniform solution, add 15wt% of a mixture of formaldehyde and acetaldehyde, and adjust the pH of the solution to 2 with sulfuric acid. After insoluble floccules are generated, wash away the participating acid with NaOH, wash with water, and dry to obtain polyvinyl alcohol acetaldehyde.
[0054] The active material (organic sulfide) and the conductive agent (carbon black) are added to the polyvinyl alcohol acetaldehyde solution, wherein the mass ratio of the organic sulfide, carbon black and polyvinyl alcohol acetaldehyde is 8:1:1. After stirring evenly, the slurry is scraped and dried at 80°C to obtain the negative electrode sheet, and the battery is assembled.
[0055] Example 6
[0056] A preparation method for a positive electrode of a zinc ion battery comprises the following steps:
[0057] Take polyvinyl alcohol with a mass ratio of 1:9 and dissolve it in water to form a transparent uniform solution, add 25wt% of a mixture of formaldehyde and acetaldehyde, and adjust the pH of the solution to 1 with hydrochloric acid. After insoluble floccules are generated, wash away the participating acid with ammonia water, wash with water, and dry to obtain polyvinyl alcohol acetaldehyde.
[0058] The active material (sodium vanadium phosphate) and the conductive agent (carbon black) are added to the polyvinyl alcohol acetaldehyde solution, wherein the mass ratio of sodium vanadium phosphate, carbon black and polyvinyl alcohol acetaldehyde is 9:0.5:0.5. After stirring evenly, the slurry is scraped and dried at 80°C to obtain the positive electrode sheet, and the battery is assembled.
[0059] Example 7
[0060] A preparation method for a negative electrode of a sodium ion battery comprises the following steps:
[0061] Take polyvinyl alcohol with a mass ratio of 2:8 and dissolve it in water to form a transparent uniform solution, add 5wt% of acetaldehyde mixture, and adjust the pH of the solution to 3 with hydrochloric acid. After insoluble floccules are generated, the acid is washed away with sodium hydroxide, and polyvinyl acetal is obtained after washing with water and drying.
[0062] The active material (sodium titanate) and the conductive agent (carbon black) are added to the polyvinyl acetal solution, wherein the mass ratio of sodium titanate, carbon black and polyvinyl acetal is 8.5:0.5:1. After stirring evenly, the slurry is scraped and dried at 80°C to obtain the negative electrode sheet, and the battery is assembled.
[0063] Example 8
[0064] A preparation method for a sodium ion battery positive electrode comprises the following steps:
[0065] Polyvinyl alcohol with a mass ratio of 1:9 is dissolved in water to form a transparent uniform solution, 15wt% of a butyraldehyde mixture is added, and the pH of the solution is adjusted to 1 with sulfuric acid. After insoluble floccules are generated, the acid is washed away with NaOH, and polyvinyl butyral is obtained after washing with water and drying.
[0066] The active material (layered transition metal oxide) and the conductive agent (carbon fiber) are added to the polyvinyl butyral solution, wherein the mass ratio of the layered transition metal oxide, the carbon fiber and the polyvinyl butyral is 8:1:1. After stirring evenly, the slurry is scraped and dried at 80°C to obtain the positive electrode sheet, and the battery is assembled.
[0067] Comparative Example 1
[0068] A preparation method for a negative electrode of a zinc ion battery comprises the following steps:
[0069] The active material (zinc powder) and the conductive agent (carbon black) are added to the PVDF binder solution, wherein the mass ratio of zinc powder, carbon black and PVDF is 8:1:1. After stirring evenly, the slurry is scraped and dried at 80°C to obtain the negative electrode sheet, and the battery is assembled.
[0070] Figure 1 The infrared spectra of the binders used in Example 1 and Comparative Example 1 are shown. It can be seen from the infrared spectra that PVF is successfully synthesized, and compared with PVDF, PVF has more polar groups.
[0071] Figure 2 The tensile test of the negative electrode of Example 1 and Comparative Example 1. PVDF@ZnP directly breaks under a stress of 16Mpa, and its plasticity changes drastically. PVF@ZnP cracks under a stress of 26Mpa and breaks slowly.
[0072] Figure 3 This is the puncture test of the negative electrode of Example 1 and Comparative Example 1. PVDF@ZnP was punctured when it could withstand a force of less than 0.5N, while PVF@ZnP could withstand a puncture force of 3N, which can effectively suppress the problems of dendrite puncture and electrode rupture caused by volume change during the cycle of the ZnP negative electrode.
[0073] Figure 4 The figure is a rate diagram of the negative electrode of Example 1 and Comparative Example 1. Compared with Comparative Example 1, it can be seen that the PVF@ZnP in Example 1 can remain stable at different current densities, while the PVDF@ZnP electrode sheet is powdered and the battery fails when the current density changes.
[0074] Figure 5 The negative electrode of Example 1 and Comparative Example 1 is 1Ag -1 The cycle diagram below matches Na2V6O 16 After assembling the full battery with 3H2O cathode, PVF@ZnP exhibited a higher discharge specific capacity, and the capacity retention rate reached 81.08% after 500 cycles, and the coulombic efficiency reached 99.97%, while PVDF@ZnP powdered after rapid cycling, resulting in battery failure and no capacity.
[0075] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A polyvinyl acetal type binder, characterized in that: The polyvinyl acetal binder is a polymer product obtained by acetalization reaction of polyvinyl alcohol and aldehydes under catalyst conditions.
2. The polyvinyl acetal type binder according to claim 1, characterized in that: The degree of polymerization of the polyvinyl alcohol includes one or more of ultra-high degree of polymerization, high degree of polymerization, medium degree of polymerization, and low degree of polymerization; the molecular weight of the ultra-high degree of polymerization is 250,000 to 300,000, the molecular weight of the high degree of polymerization is 150,000 to 250,000, the molecular weight of the medium degree of polymerization is 70,000 to 150,000, and the molecular weight of the low degree of polymerization is 10,000 to 70,000.
3. The polyvinyl acetal type binder according to claim 1, characterized in that: The alcoholysis degree of the polyvinyl alcohol is one or more of 50% to 100%.
4. The polyvinyl acetal type binder according to claim 1, characterized in that: Aldehydes are aldehydes of the general formula RCHO; Including the general formula C n H 2n O (n ≥ 2) monobasic saturated aldehydes: one or more of formaldehyde, acetaldehyde, propionaldehyde, valeraldehyde, hexanal, etc.; acyclic aliphatic aldehydes: one or more of octanal, nonanal, decanal, undecanal, lauric aldehyde (dodecane), tridecanal, myristic aldehyde (tetradecane), etc.; alicyclic aldehydes: one or more of privet aldehyde, ivinal, isocyclic citral, citric aldehyde, methyl citric aldehyde, lyral, etc.; aromatic aldehydes: one or more of benzaldehyde, phenylacetaldehyde, phenylpropionaldehyde, cinnamaldehyde, lily of the valley aldehyde, vanillin, ethyl vanillin, etc.; terpene aldehydes: one or more of citral, citronellal, hydroxycitronellal, perillaldehyde, trimethylheptenal, etc.
5. The polyvinyl acetal type binder according to claim 1, characterized in that: The aldehydes account for 0.01 wt% to 30 wt% of the polyvinyl alcohol.
6. The polyvinyl acetal type binder according to claim 1, characterized in that: The catalyst is one or more of an inorganic acid or an organic acid; the inorganic acid includes hydrochloric acid and sulfuric acid; the organic acid includes R-COOH and R-SO3H.
7. A method for preparing polyvinyl acetal according to any one of claims 1 to 6, characterized in that: The steps include: (1) heating and stirring polyvinyl alcohol in water until it is completely dissolved to obtain a transparent and uniform polyvinyl alcohol aqueous solution, wherein the heating temperature is 20 to 200° C.; (2) Under the catalytic action of an acidic catalyst, polyvinyl alcohol and aldehydes undergo a one-step acetalization reaction, wherein the pH value of the system is 1 to 5, wherein the catalyst is one or more of an inorganic acid or an organic acid; the inorganic acid includes hydrochloric acid and sulfuric acid; the organic acid includes R-COOH and R-SO3H; (3) performing an acetalization reaction at 20 to 200° C. for 5 minutes to 48 hours until the reaction becomes viscous and produces an insoluble cross-linked flocculent; (4) neutralizing the residual acidic catalyst with a base until the pH value of the system is 7 to 10, wherein the base is one or more of sodium hydroxide, lithium hydroxide, potassium hydroxide, barium hydroxide, ammonia water, Schiff base, etc.; (5) After washing with water and drying, the polyethanol acetal polymer is obtained.
8. Use of the polyvinyl acetal binder according to any one of claims 1 to 6 in the preparation of battery pole pieces, characterized in that: The pole piece comprises an active material, a conductive agent and a binder.
9. The use according to claim 8, characterized in that: The active material includes one or more of graphite carbon materials, disordered carbon materials, lithium titanate materials, silicon-based materials, carbonyl compounds, Schiff base compounds, organic free radical compounds, organic sulfides, metal sulfur compounds, zinc powder, lithium cobalt oxide, lithium iron phosphate, lithium manganate, ternary materials nickel cobalt manganate and nickel cobalt aluminum oxide, transition metal oxides, polyanion materials, Prussian blue compounds, organic molecules and polymers, amorphous materials, vanadium-based, manganese-based compounds, Prussian blue analogs and organic compounds; the conductive agent is one or more of carbon black, conductive graphite, carbon fiber, carbon nanotubes, and graphene; the binder is soluble in one or more of alcohols such as methanol, ethanol, and butanol, ketones such as cyclohexanone, butanone, and N-methylpyrrolidone, aromatic hydrocarbons, benzene, toluene, xylene, chlorinated hydrocarbons such as ethyl chloride and dichloroethane, formic acid, acetic acid, furfural, phenols, and azobenzenes.
10. The use according to claim 8, characterized in that: The ratio of the active material, the conductive agent and the binder is (7-9.5): (0.3-2): (0.2-1).