Purple light excited fluorescent material as well as preparation and application thereof
By doping Eu3+ and Bi3+ ions into violet-excited fluorescent materials in a lead-free halide matrix, the problem of unstable color temperature and uneven luminous intensity of white LEDs and near-infrared pc-LEDs is solved, and efficient red and near-infrared light are achieved. Light emission, suitable for a variety of LED applications, meeting the needs for efficient and stable light sources.
Patent Information
- Application Number
- CN202410754086.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Existing white LEDs and near-infrared pc-LEDs have problems such as unstable color temperature, low color rendering index, blue light hazard, and uneven luminous intensity. Moreover, traditional near-infrared light sources are large in size, poor in efficiency, and short in life, making it difficult to meet the requirements of high efficiency and tunability. demand for ultra-wideband near-infrared phosphors.
Provides a violet light-excited fluorescent material Cs2MnCl4:xEu3+ and Cs2Mn1-yBiyCl4. By doping Eu3+ and Bi3+ ions, a lead-free halide matrix red and near-infrared emitting phosphor is prepared, which is suitable for white light LEDs, solar-like LEDs, Full-spectrum LED, near-infrared pc-LED, biomedical imaging and night vision equipment adopt sintering and cooling processing methods.
It has realized a fluorescent material with a wide excitation band, which can emit red light with a central wavelength of 617nm or near-infrared light of 780nm under violet light excitation. It has high photoluminescence quantum yield and stable physical and chemical properties, and is suitable for a variety of LED chips. application to meet commercial market needs.
Smart Images

Figure CN118772873A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fluorescent material preparation, and in particular to a fluorescent material excited by purple light and the preparation and application thereof. Background Art
[0002] With the rapid development of economy, people's living standard is also improving, and the requirements for lighting quality are getting higher and higher. White light-emitting diodes (W-LED) have been widely studied and applied due to their advantages such as low power consumption, high stability and excellent luminous efficiency. There are two common methods to obtain this white light. One is to synthesize white light through a multi-chip set of red, green and blue primary colors and light emission. However, due to the different light decay of the three primary color chips, the color temperature is unstable, the control circuit is more complicated and the cost is higher. Another method is to combine InGaN blue light chip with yellow phosphor Y3Al5O 12 :Ce 3+ (YAG:Ce 3+ ), this method has a strong blue light chip peak and the blue light part is too strong, resulting in uneven luminous intensity, low color rendering index, high color temperature and certain blue light hazards that are not conducive to physical and mental health. Therefore, we look for three-color (blue, green, red) phosphors that are effectively excited in the purple light region and combined with purple light chips to produce white light. This method can effectively avoid low color rendering index, high color temperature and blue light hazards, and is a method with application prospects. Red phosphor is one of the most important components of three-color phosphors, so the synthesis of red phosphors with strong absorption in the purple light region plays an important role in healthy lighting.
[0003] Designing efficient broadband near-infrared (NIR) luminescent materials has always been at the forefront of photonic crystal research. Its natural advantages have been widely used in the fields of near-infrared spectroscopy, medical diagnosis, non-destructive testing and night vision equipment. In particular, near-infrared light sources in the range of 700 to 1000 nm are of great significance because this wavelength window contains the characteristic absorption patterns of normal organic functional groups (such as O─H, C─H and N─H) in various components of food and human body, and has great potential in deep tissue imaging. In addition, this emission wavelength range matches low-cost, sensitive commercial silicon-based photodetectors, and a compact, portable, fast spectral analysis system can be constructed to meet the needs of rapid detection in daily life. Although traditional halogen tungsten lamps and incandescent bulbs can emit ultra-broadband near-infrared radiation in the near-ultraviolet to mid-infrared band, they are severely limited by large size, poor efficiency, poor heat dissipation, and short life. In contrast, near-infrared phosphor-converted light-emitting diodes (pc-LEDs) are considered a reliable choice for small-sized near-infrared light sources because of their tunable emission spectra, high radiation flux, simple preparation methods, and excellent durability. Therefore, the pursuit of near-infrared phosphors that meet broadband emission is the key to the development of ultra-broadband miniaturized near-infrared light sources. 3+ions are considered to be a promising activator that can achieve tunable ultra-broadband near-infrared emission when added to an appropriate crystal field environment of an inorganic matrix. 3+ It has become an urgent task to develop novel hosts for ions to produce broadband emission and high photoluminescence quantum yield (PLQY). Lead-free halide-based perovskites are gaining increasing attention as an emerging, non-toxic alternative to lead-based perovskites.
[0004] Lead-free halide-based perovskites are gaining increasing attention as an emerging, non-toxic alternative to lead-based perovskites. Summary of the invention
[0005] In order to solve the above problems, the purpose of the present invention is to provide a fluorescent material excited by violet light and its preparation and application. The fluorescent material (Cs2MnCl4:xEu 3+ ) is a violet light excited Eu 3+ The doped lead-free halide-based 617nm red emitting phosphor can meet the current urgent needs of white light LEDs, sunlight-like LEDs, and full-spectrum LEDs; the purple light-excited fluorescent material (Cs2Mn 1-y Bi y Cl4) is a violet light excited Bi 3+ The doped lead-free halide-based 780nm near-infrared emitting phosphor can meet the current urgent needs in near-infrared pc-LEDs, biomedical imaging, non-destructive testing and night vision equipment.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The first object of the present invention is to provide a fluorescent material excited by violet light, the chemical expression of which is Cs2MnCl4:xEu 3+ , where 0.005≤x≤0.08;
[0008] Or, the chemical expression of the fluorescent material is Cs2Mn 1-y Bi y Cl4 where 0.005≤y≤0.08.
[0009] In one embodiment of the present invention, x is 0.005, 0.01, 0.02, 0.04, 0.06 or 0.08;
[0010] y is 0.005, 0.01, 0.02, 0.04, 0.06 or 0.08.
[0011] In one embodiment of the present invention, the fluorescent material is a crystalline material.
[0012] In one embodiment of the present invention, when the chemical expression of the fluorescent material excited by violet light is Cs2MnCl4:xEu 3+ When , its excitation spectrum ranges from 200 to 550nm, the emission spectrum ranges from 550 to 720nm, and the central emission wavelength is 617nm red light;
[0013] When the violet light excites the fluorescent material, the chemical expression is Cs2Mn 1-y Bi y When Cl4, its excitation spectrum ranges from 200 to 600nm, the emission spectrum ranges from 700 to 900nm, and the central emission wavelength is 780nm near-infrared light.
[0014] The second object of the present invention is to provide a method for preparing a fluorescent material excited by violet light. When the chemical expression of the fluorescent material excited by violet light is Cs2MnCl4:xEu 3+ When, the preparation method comprises the following steps:
[0015] (A1) mixing a cesium source compound, a manganese source compound and a europium source compound to obtain a first mixed powder;
[0016] (A2) mixing the first mixed powder prepared in step (A1) with hydrochloric acid, and then sequentially performing sintering treatment and cooling treatment to obtain a fluorescent material excited by purple light;
[0017] When the violet light excites the fluorescent material, the chemical expression is Cs2Mn 1-y Bi y Cl4, its preparation method comprises the following steps:
[0018] (B1) mixing the cesium source compound, the manganese source compound and the bismuth source compound to obtain a second mixed powder;
[0019] (B2) The second mixed powder prepared in step (B2) is mixed with hydrochloric acid, and then sintered and cooled in sequence to obtain a fluorescent material excited by violet light.
[0020] In one embodiment of the present invention, in step (A1), according to the chemical formula of the fluorescent material Cs2MnCl4:xEu 3+ Wherein 0.005≤x≤0.08, on the basis of preparing various raw materials, 50% of the cesium source compound is additionally added as a cesium source supplement on the basis of the calculated amount of the cesium source compound;
[0021] In step (B1), according to the chemical formula of the fluorescent material Cs2Mn 1-y Bi yCl4 wherein 0.005≤x≤0.08, on the basis of preparing various raw materials, and then on the basis of the calculated amount of the cesium source compound, an additional 50% of the cesium source compound is added as a cesium source supplement.
[0022] Among them, on the basis of preparing various raw materials according to the chemical expression of the fluorescent material, when the cesium source compound is added normally, a product containing the cesium source phase cannot be obtained; therefore, it is necessary to additionally add the cesium source compound to ensure the presence of the cesium source phase in the product.
[0023] In one embodiment of the present invention, in step (A1), the cesium source compound is CsCl powder, the manganese source compound is MnCl2, and the europium source compound is EuCl3 powder;
[0024] In step (B1), the cesium source compound is CsCl powder, the manganese source compound is MnCl2, and the bismuth source compound is BiCl3 powder.
[0025] In one embodiment of the present invention, in step (A2), the amount of hydrochloric acid used is 2 to 5 mL (based on a 25 mL polytetrafluoroethylene container);
[0026] In step (B2), the amount of hydrochloric acid used is 2-5 mL (based on a 25 mL polytetrafluoroethylene container).
[0027] In one embodiment of the present invention, in step (A2), the sintering process is carried out in an air atmosphere at a temperature of 100 to 200° C. for a time of 12 to 24 hours.
[0028] Preferably, in step (A2), during the sintering process, the temperature is 120-180° C. and the time is 24 hours.
[0029] In one embodiment of the present invention, in step (A2), during the cooling process, the cooling rate is 1 to 5°C / h;
[0030] Preferably, the cooling rate is 3°C / h.
[0031] In one embodiment of the present invention, in step (B2), the sintering process is carried out in an air atmosphere at a temperature of 100 to 200° C. for a time of 12 to 24 hours.
[0032] Preferably, in step (B2), during the sintering process, the temperature is 120-180° C. and the time is 24 hours.
[0033] In one embodiment of the present invention, in step (B2), during the cooling process, the cooling rate is 1 to 5°C / h.
[0034] Preferably, the cooling rate is 3°C / h.
[0035] In the present invention, when the cooling rate is 1-5°C / h, the crystal nuclei obtained in the preparation process of the product are larger, the quality of the crystals formed subsequently is higher, and thus the luminescence intensity of the product is higher; when the cooling rate is lower than 1°C / h, although the crystal nuclei obtained in the preparation process of the product are larger, when the temperature drops below 100°C, the obtained crystals will be dissolved by the hydrochloric acid inside the polytetrafluoroethylene container, and thus the crystals disappear; when the cooling rate is higher than 5°C / h, the crystal nuclei obtained in the preparation process of the product are smaller, the quality of the crystals formed subsequently is worse, and thus the luminescence intensity of the product is worse.
[0036] In the present invention, during high-temperature sintering, the interior of the polytetrafluoroethylene container is under pressure; the specific method of high-temperature sintering is as follows:
[0037] The mixed powder and hydrochloric acid are placed in a polytetrafluoroethylene container, and then the polytetrafluoroethylene container containing the raw materials is placed in a reactor for sintering.
[0038] The third object of the present invention is to provide an application of a fluorescent material excited by purple light in the preparation of an LED chip, wherein the LED chip is selected from a white light LED chip or a near-infrared pc-LED chip.
[0039] In one embodiment of the present invention, when the chemical expression of the fluorescent material excited by violet light is Cs2MnCl4:xEu 3+ When used in combination with a semiconductor device, it can be used to prepare white light LED chips (which can be further applied to white light LEDs, sunlight-like LEDs, full-spectrum LEDs, etc.).
[0040] In one embodiment of the present invention, when the chemical formula of the fluorescent material excited by violet light is Cs2Mn 1- y Bi y When Cl4 is used, it can be used to prepare near-infrared pc-LED chips (which can be further applied to near-infrared pc-LEDs, biomedical imaging, non-destructive testing and night vision equipment, etc.).
[0041] A fourth object of the present invention is to provide an LED chip, wherein the LED chip comprises the above-mentioned fluorescent material excited by violet light.
[0042] In the fluorescent material system, all-inorganic lead-free halides are considered to be high-brightness fluorescent materials due to their large carrier diffusion length, high photoluminescence quantum yield, adjustable band gap, and excellent optoelectronic properties. At the same time, all-inorganic lead-free halides have good chemical stability and environmental friendliness, and show great application prospects in the fields of light-emitting diodes (LEDs), solar cells, lasers, and bio-imaging. Therefore, the all-inorganic lead-free halide system is a very promising fluorescent material.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] (1) The violet light-excited fluorescent material of the present invention has a wide excitation band, and the effective absorption range covers 200-550nm or 200-600nm, and can be excited by violet light. The obtained fluorescent material can emit red light with a central wavelength of 617nm or near-infrared light of 780nm under the excitation of 394nm or 417nm violet light.
[0045] (2) The ultraviolet light-excited fluorescent material of the present invention has the advantage of stable physical and chemical properties. At the same time, the fluorescent material can be prepared by a hydrothermal reaction method, and has the characteristics of a simple preparation process and high purity of the prepared sample. It can be used as a good candidate material for the widespread application of white light LEDs or pc-LEDs, and has broad application prospects.
[0046] (3) The emission wavelength of the ultraviolet light-excited fluorescent material of the present invention includes 550-720nm or 700-900nm, and can effectively absorb light in the wavelength range of 200-550nm or 200-600nm. It can be well matched with the existing ultraviolet light chip to meet the needs of the commercial market and is suitable for applications in white light LEDs, sunlight-like LEDs, full-spectrum LEDs, near-infrared pc-LEDs, biomedical imaging, non-destructive testing, and night vision equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 is a photoexcitation / emission spectrum of the fluorescent material excited by violet light prepared in Example 1 of the present invention;
[0048] Figure 2 is the XRD diffraction pattern of the fluorescent material excited by violet light prepared in Example 1 of the present invention;
[0049] Figure 3 The photoexcitation spectra of the fluorescent materials excited by violet light prepared in Examples 7, 8 and 9 of the present invention are as follows;
[0050] Figure 4 The photoemission spectra of the fluorescent materials excited by violet light prepared in Examples 7, 8 and 9 of the present invention are as follows;
[0051] Figure 5 These are the XRD diffraction patterns of the violet light excited fluorescent materials prepared in Examples 7, 8 and 9 of the present invention. DETAILED DESCRIPTION
[0052] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0053] In the following examples, unless otherwise specified, all reagents used are commercially available reagents, and all detection means and methods used are conventional detection means and methods in the art.
[0054] Example 1
[0055] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0056] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to a stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.5051:0.1258:0.0016), and mixing to obtain a raw material mixture;
[0057] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing the mixture in a muffle furnace for sintering at 180° C. for 24 h, and then cooling it to room temperature to obtain a fluorescent material excited by purple light (its photoexcitation / emission spectrum is shown in FIG. Figure 1 As shown, the XRD spectrum is Figure 2 shown).
[0058] analyze:
[0059] The spectral properties of the fluorescent material were tested using a fluorescence spectrometer (HITACHI F-7000). Figure 1 As shown. The results show that the fluorescent material has a wide excitation band with a peak near 394nm and a high spectral peak, which can match well with the purple light commercial chip. Under the excitation of 394nm purple light source, the fluorescent material emits red light, and the emission spectrum consists of a wide emission band (550-720nm) with a peak at 614nm.
[0060] The crystal structure of the fluorescent material prepared above was tested by X-ray diffraction (Ultima IV-185). Cu-Kα was used as the target material, and the scanning angle 2θ range was 10-70°. The XRD ray diffraction pattern was as follows: Figure 2 As shown, from Figure 2 It can be seen that the fluorescent material is consistent with the standard card (PDF#04-006-8998), indicating that Eu 3+ The doping of ions does not have a significant effect on the crystal structure, and the obtained fluorescent material is a pure phase substance isomorphous with Cs2MnCl4. The fluorescence emission spectrum data of the fluorescent material shows that the emission of the fluorescent material is in the red light region, and it can be used as a good red light emitting fluorescent material suitable for white light LEDs.
[0061] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2MnCl4:xEu3+ , x is 0.005.
[0062] Example 2
[0063] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0064] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to a stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.5051:0.1258:0.0031), and mixing to obtain a raw material mixture;
[0065] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing it in a muffle furnace for sintering at 160° C. for 24 h, and then cooling it to room temperature to obtain a fluorescent material excited by purple light, whose photoluminescence performance is similar to that of Example 1.
[0066] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2MnCl4:xEu 3+ , x is 0.01.
[0067] Example 3
[0068] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0069] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to a stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.5051:0.1258:0.0062), and mixing to obtain a raw material mixture;
[0070] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing it in a muffle furnace for sintering at 180° C. for 18 h, and then cooling it to room temperature to obtain a fluorescent material excited by purple light, whose photoluminescence performance is similar to that of Example 1.
[0071] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2MnCl4:xEu 3+ , x is 0.02.
[0072] Example 4
[0073] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0074] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to a stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.5051:0.1258:0.0124), and mixing to obtain a raw material mixture;
[0075] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing it in a muffle furnace for sintering at 180° C. for 18 h, and then cooling it to room temperature to obtain a fluorescent material excited by purple light, whose photoluminescence performance is similar to that of Example 1.
[0076] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2MnCl4:xEu 3+ , x is 0.04.
[0077] Example 5
[0078] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0079] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to a stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.5051:0.1258:0.0186), and mixing to obtain a raw material mixture;
[0080] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing it in a muffle furnace for sintering at 120° C. for 12 h, and then cooling it to room temperature to obtain a fluorescent material excited by purple light, whose photoluminescence performance is similar to that of Example 1.
[0081] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2MnCl4:xEu 3+ , x is 0.06.
[0082] Example 6
[0083] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0084] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to a stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.5051:0.1258:0.0248), and mixing to obtain a raw material mixture;
[0085] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing it in a muffle furnace for sintering at 180° C. for 18 h, and then cooling it to room temperature to obtain a fluorescent material excited by purple light, whose photoluminescence performance is similar to that of Example 1.
[0086] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2MnCl4:xEu 3+ , x is 0.08.
[0087] Table 1 Preparation parameters of Examples 1 to 6
[0088]
[0089] Example 7
[0090] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0091] (S1) weighing 1 g of CsCl, MnCl2 and BiCl3 raw material powders according to the stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:BiCl3=0.5051:0.1258:0.0016), and mixing to obtain a raw material mixture;
[0092] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing the mixture in a muffle furnace for sintering at 180° C. for 24 h, and then cooling it to room temperature to obtain a fluorescent material excited by violet light (its photoexcitation spectrum is shown in FIG. Figure 3 As shown in the photoemission spectrum Figure 4 As shown, the XRD spectrum is Figure 5 shown).
[0093] analyze:
[0094] The spectral properties of the fluorescent material were tested using a fluorescence spectrometer (HITACHI F-7000). Figure 3 and Figure 4 As shown. The results show that the fluorescent material has a wide excitation band with a peak value near 417nm and a high spectral peak, which can match well with the purple light commercial chip. Under the excitation of 394nm purple light source, the fluorescent material emits near-infrared light, and the emission spectrum consists of a wide emission band (700-900nm) with a peak value at 780nm.
[0095] The crystal structure of the fluorescent material prepared above was tested by X-ray diffraction (Ultima IV-185). Cu-Kα was used as the target material, and the scanning angle 2θ range was 10-70°. The XRD ray diffraction pattern was as follows: Figure 5 As shown, from Figure 5 It can be seen that the fluorescent material is consistent with the standard card (PDF#04-006-8998), indicating that Bi 3+ The doping of ions does not have a significant effect on the crystal structure, and the obtained fluorescent material is a pure phase substance isomorphous with Cs2MnCl4. The fluorescence emission spectrum data of the fluorescent material shows that the emission of the fluorescent material is in the near-infrared light region, and it can be used as a good near-infrared light emitting fluorescent material suitable for near-infrared pc-LEDs.
[0096] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2Mn 1-y Bi y Cl4, y is 0.005.
[0097] Example 8
[0098] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0099] (S1) weighing 1 g of CsCl, MnCl2 and BiCl3 raw material powders according to the stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:BiCl3=0.5051:0.1258:0.0031), and mixing to obtain a raw material mixture;
[0100] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing the mixture in a muffle furnace for sintering at 160° C. for 24 h, and then cooling it to room temperature to obtain a fluorescent material excited by violet light (its photoexcitation spectrum is shown in FIG. Figure 3 As shown in the photoemission spectrum Figure 4 As shown, the XRD spectrum is Figure 5 Its photoluminescence performance is similar to that of Example 7.
[0101] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2Mn 1-y Bi y Cl4, y is 0.01.
[0102] Example 9
[0103] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0104] (S1) weighing 1 g of CsCl, MnCl2 and BiCl3 raw material powders according to the stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:BiCl3=0.5051:0.1258:0.0062), and mixing to obtain a raw material mixture;
[0105] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing the mixture in a muffle furnace for sintering at 180° C. for 18 h, and then cooling it to room temperature to obtain a fluorescent material excited by violet light (its photoexcitation spectrum is shown in FIG. Figure 3 As shown in the photoemission spectrum Figure 4 As shown, the XRD spectrum is Figure 5 Its photoluminescence performance is similar to that of Example 7.
[0106] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2Mn 1-y Bi y Cl4, y is 0.02.
[0107] Example 10
[0108] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0109] (S1) weighing 1 g of CsCl, MnCl2 and BiCl3 raw material powders according to the stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:BiCl3=0.5051:0.1258:0.0124), and mixing to obtain a raw material mixture;
[0110] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing it in a muffle furnace and sintering it at 140° C. for 18 h, and then cooling it to room temperature to obtain a fluorescent material excited by purple light, whose photoluminescence performance is similar to that of Example 7.
[0111] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2Mn 1-y Bi y Cl4, y is 0.04.
[0112] Embodiment 11
[0113] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0114] (S1) weighing 1 g of CsCl, MnCl2 and BiCl3 raw material powders according to the stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:BiCl3=0.5051:0.1258:0.0186), and mixing to obtain a raw material mixture;
[0115] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing it in a muffle furnace for sintering at 120° C. for 12 h, and then cooling it to room temperature to obtain a fluorescent material excited by purple light, whose photoluminescence performance is similar to that of Example 7.
[0116] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2Mn 1-y Bi y Cl4, y is 0.06.
[0117] Example 12
[0118] This embodiment provides a method for preparing a fluorescent material excited by violet light, and the specific steps are as follows:
[0119] (S1) weighing 1 g of CsCl, MnCl2 and BiCl3 raw material powders according to the stoichiometric ratio, adding 50% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:BiCl3=0.5051:0.1258:0.0248), and mixing to obtain a raw material mixture;
[0120] (S2) placing the raw material mixture obtained in step (S1) in a polytetrafluoroethylene container, adding 2 mL of hydrochloric acid after the raw materials are evenly mixed, placing it in a muffle furnace for sintering at 120° C. for 12 h, and then cooling it to room temperature to obtain a fluorescent material excited by purple light, whose photoluminescence performance is similar to that of Example 7.
[0121] The general formula of the violet light excited fluorescent material obtained in this embodiment is Cs2Mn 1-y Bi y Cl4, y is 0.08.
[0122] Table 1 Preparation parameters of Examples 7 to 12
[0123]
[0124] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the explanation of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A fluorescent material excited by violet light, characterized in that: The chemical formula of the fluorescent material is Cs2MnCl4:xEu 3+ , where 0.005≤x≤0.08; Or, the chemical expression of the fluorescent material is Cs2Mn 1-y Bi y Cl4 where 0.005≤y≤0.
08.
2. The violet light excited fluorescent material according to claim 1, characterized in that: x is 0.005, 0.01, 0.02, 0.04, 0.06 or 0.08; y is 0.005, 0.01, 0.02, 0.04, 0.06 or 0.
08.
3. The violet light excited fluorescent material according to claim 1, characterized in that: The fluorescent material is a crystalline material.
4. The violet light excited fluorescent material according to claim 1, characterized in that: When the violet light excites the fluorescent material, the chemical expression is Cs2MnCl4:xEu 3+ When , its excitation spectrum ranges from 200 to 550nm, the emission spectrum ranges from 550 to 720nm, and the central emission wavelength is 617nm red light; When the violet light excites the fluorescent material, the chemical expression is Cs2Mn 1-y Bi y When Cl4, its excitation spectrum ranges from 200 to 600nm, the emission spectrum ranges from 700 to 900nm, and the central emission wavelength is 780nm near-infrared light.
5. A method for preparing a fluorescent material excited by violet light as claimed in any one of claims 1 to 4, characterized in that: When the violet light excites the fluorescent material, the chemical expression is Cs2MnCl4:xEu 3+ When, the preparation method comprises the following steps: (A1) mixing a cesium source compound, a manganese source compound and a europium source compound to obtain a first mixed powder; (A2) mixing the first mixed powder prepared in step (A1) with hydrochloric acid, and then sequentially performing sintering treatment and cooling treatment to obtain a fluorescent material excited by purple light; When the violet light excites the fluorescent material, the chemical expression is Cs2Mn 1-y Bi y Cl4, its preparation method comprises the following steps: (B1) mixing the cesium source compound, the manganese source compound and the bismuth source compound to obtain a second mixed powder; (B2) The second mixed powder prepared in step (B2) is mixed with hydrochloric acid, and then sintered and cooled in sequence to obtain a fluorescent material excited by violet light.
6. The method for preparing a fluorescent material excited by violet light according to claim 5, characterized in that: In step (A1), according to the chemical formula of the fluorescent material Cs2MnCl4:xEu 3+ Wherein 0.005≤x≤0.08, 50% of the cesium source compound is added as a cesium source supplement on the basis of the calculated amount of the cesium source compound; In step (B1), according to the chemical formula of the fluorescent material Cs2Mn 1-y Bi y Cl4 wherein 0.005≤x≤0.08, based on the calculated amount of the cesium source compound, an additional 50% of the cesium source compound is added as a cesium source supplement.
7. The method for preparing a fluorescent material excited by violet light according to claim 5, characterized in that: In step (A2), during the sintering process, the temperature is 100 to 200° C. and the time is 12 to 24 hours.
8. The method for preparing a fluorescent material excited by violet light according to claim 5, characterized in that: In step (A2), during the cooling process, the cooling rate is 1 to 5°C / h.
9. Use of the violet light excited fluorescent material as claimed in any one of claims 1 to 4 in the preparation of LED chips, characterized in that: The LED chip is selected from a white light LED chip or a near infrared pc-LED chip.
10. An LED chip, characterized in that: The LED chip comprises the fluorescent material excited by violet light as claimed in any one of claims 1 to 4.
Citation Information
Patent Citations
Preparation method and application of lead-free perovskite microcrystal
CN115717072A