NiCoCrAlYRe low-expansion metal bonding layer and preparation method thereof
By combining the NiCoCrAlYRe low-expansion metal bonding layer with the single-crystal high-temperature alloy matrix, the coating is deposited using the vacuum arc plating method, which solves the problem of mismatch in thermal expansion coefficient between the thermal barrier coating, the ceramic surface layer and the metal matrix, and improves the efficiency of turbine blades. Excellent resistance to high temperature oxidation corrosion and long life.
Patent Information
- Application Number
- CN202410856167.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The metal bonding layer of the existing thermal barrier coating does not match the thermal expansion coefficient of the ceramic surface layer and the metal matrix at high temperatures, resulting in unstable interfaces and limiting the long-life development of turbine blades.
NiCoCrAlYRe low-expansion metal bonding layer is used, and the coating is deposited by vacuum arc plating. The element composition is 33% Ni, 29% Co, 17% Cr, 15.5% Al, 0.5% Y, 5% Re, combined with the single crystal superalloy matrix, undergoes mill flow treatment, deposition and diffusion treatment to improve the compatibility and oxidation corrosion resistance of the bonding layer.
It achieves good matching with the ceramic surface layer and alloy matrix, improves the high-temperature oxidation corrosion resistance and thermal bonding strength of the coating, slows down the diffusion of elements, enhances the density and strain capacity of the coating, and lengthens the turbine blades. service life.
Smart Images

Figure CN118773548A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal bonding layer materials, and in particular relates to a NiCoCrAlYRe low expansion metal bonding layer and a preparation method thereof. Background Art
[0002] The temperature at the front inlet of the new generation of engines is constantly increasing. Depositing thermal barrier coatings on the surface of blade alloys can increase the operating temperature and high-temperature corrosion resistance of turbine blades. Thermal barrier coating technology is one of the key technologies in the development of advanced aircraft engines. The MCrAlY series of thermal barrier coatings are developed from coated anti-oxidation coatings. When used as a separate anti-oxidation coating, it has the characteristics of good bonding with the substrate and excellent high-temperature protection performance; when used as a bonding layer, there is insufficient research on the matching of thermal expansion coefficients of alloys / bonding layers / YSZ, the formation law of surface TGO, and the diffusion mechanism of elements, resulting in a decrease in the role of the bonding layer in improving the matching of the ceramic surface layer and the substrate, which fundamentally limits the development of long-life thermal barrier coatings.
[0003] The main difficulty of the low expansion metal bonding layer is that, on the basis of meeting the requirements of high temperature oxidation and thermal corrosion resistance, the thermal expansion coefficient must be well matched with the ceramic surface layer and the metal matrix, and the interface structure must be stable at high temperature. Summary of the invention
[0004] Based on the above background, the purpose of the present invention is to provide a NiCoCrAlYRe coating with a smaller thermal expansion coefficient and good compatibility with a ceramic surface layer and an alloy substrate, and a preparation method thereof.
[0005] In view of this, according to one aspect of an embodiment of the present invention, a NiCoCrAlYRe low expansion metal bonding layer is provided, which forms a metallurgical bond with a single crystal high temperature alloy substrate, wherein the element components are 33% Ni, 29% Co, 17% Cr, 15.5% Al, 0.5% Y, and 5% Re by mass.
[0006] Optionally, the single crystal high temperature alloy substrate is an IC10 alloy substrate.
[0007] According to another aspect of an embodiment of the present invention, a method for preparing a NiCoCrAlYRe low expansion metal bonding layer is also provided, and the method for preparing any of the metal bonding layers comprises:
[0008] Step S01: using a NiCoCrAlYRe target material, and installing the target material on a cathode seat of a vacuum arc coating machine;
[0009] Step S02: performing surface activation treatment on the single crystal high temperature alloy substrate;
[0010] Step S03: cleaning and drying the surface of the single crystal high temperature alloy substrate;
[0011] Step S04: depositing a coating on the surface of the single crystal high temperature alloy substrate;
[0012] Step S05: performing diffusion treatment on the deposited coating.
[0013] Optionally, the surface activation treatment method in step S02 is a grinding fluid treatment method.
[0014] Optionally, the grinding fluid treatment method is to use corundum sand with a particle size of 0.154 mm to add it into a liquid sand blowing machine for sand blowing, with a working pressure of 0.2MPa to 0.5MPa and a treatment time of 10min.
[0015] Optionally, step S04 further includes: deposition parameters are arc current I=550A-750A, workpiece bias voltage U=20V-30V, deposition time is 150min-200min, vacuum degree is 6×10 -3 Pa~7×10 -3 Pa.
[0016] Optionally, step S04 also includes: a preheating step: the vacuum degree reaches 6×10 -3 Pa~7×10 -3 Pa later, bombardment heating, arc current I = 550A ~ 750A, workpiece bias U = 200V ~ 300V, bombardment time is 5min.
[0017] Optionally, step S05 further includes: the vacuum degree of the diffusion process is 1×10 -2 Pa~1×10 -3 Pa, temperature is 850℃-900℃, time is 3h.
[0018] The present invention has the following beneficial effects: (1) The present invention adopts arc ion plating method to prepare NiCoCrAlYRe coating, which has a smaller thermal expansion coefficient, has good compatibility and matching with ceramic surface layer and alloy substrate, and does not cause cracking of coating and interface instability during use; (2) has good resistance to high temperature oxidation corrosion, and improves the resistance to high temperature oxidation corrosion of substrate alloy at high temperature; (3) has good thermal bonding strength with substrate alloy; (4) has low diffusion coefficient, and can slow down the diffusion of elements such as Al and Cr from coating to substrate alloy at high temperature, and can prevent metal elements such as Ti, Mo, W, Ni from alloy substrate to coating. At the same time, since the arc ion plating (ARC) method has the characteristics of moderate deposition rate, good coating density, and metallurgical bonding with substrate, the coating prepared by ARC method has strong compatibility with substrate, good thickness and density, thereby greatly improving the strain capacity of coating. NiCoCrAlYRe coating is prepared by vacuum arc plating technology, and the preparation process is simple, efficient, and low cost, which can meet the demand for long life of protective coating on the outer surface of turbine blades. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is an electron microscope image of a NiCoCrAlYRe low expansion metal bonding layer according to an embodiment of the present invention.
[0020] Figure 2 The figure is a curve diagram showing the variation of thermal expansion coefficient of a NiCoCrAlYRe low expansion metal bonding layer with temperature according to an embodiment of the present invention. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] According to one aspect of an embodiment of the present invention, a NiCoCrAlYRe low expansion metal bonding layer is provided, which forms a metallurgical bond with a single crystal high temperature alloy substrate, wherein the element components are 33% Ni, 29% Co, 17% Cr, 15.5% Al, 0.5% Y, and 5% Re by mass.
[0023] Furthermore, the single crystal high temperature alloy substrate is an IC10 alloy substrate.
[0024] According to another aspect of an embodiment of the present invention, a method for preparing a NiCoCrAlYRe low expansion metal bonding layer is provided, wherein the method for preparing any of the metal bonding layers comprises:
[0025] Step S01: using a NiCoCrAlYRe target material, and installing the target material on a cathode seat of a vacuum arc coating machine;
[0026] Step S02: Activate the surface of the single crystal high temperature alloy substrate to enhance the bonding between the bonding layer and the substrate. Further, the surface activation method in step S02 is a grinding flow treatment method.
[0027] Step S03: cleaning and drying the surface of the single crystal high temperature alloy substrate;
[0028] Step S04: depositing a coating on the surface of the single crystal high temperature alloy substrate;
[0029] Step S05: performing diffusion treatment on the deposited coating.
[0030] Furthermore, the grinding fluid treatment method is to use corundum sand with a particle size of 0.154 mm to add it into a liquid sand blowing machine for sand blowing, the working pressure is 0.2MPa~0.5MPa, and the treatment time is 10min.
[0031] Further, step S04 also includes: deposition parameters are arc current I=550A-750A, workpiece bias voltage U=20V-30V, deposition time is 150min-200min, vacuum degree is 6×10 -3 Pa~7×10 -3 Pa.
[0032] Furthermore, step S04 also includes: preheating step: the vacuum degree reaches 6×10 -3 Pa~7×10 -3 After Pa, bombardment heating is performed, the arc current I = 550A ~ 750A, the workpiece bias U = 200V ~ 300V, and the bombardment time is 5min, which is helpful to remove impurities on the substrate surface.
[0033] Furthermore, step S05 also includes: the vacuum degree of the diffusion process is 1×10 -2 Pa~1×10 -3 Pa, temperature is 850-900℃, time is 3h.
[0034] Example
[0035] Prepare the following on multiple 30*10*1.5mm samples: Figure 1 The NiCoCrAlYRe low expansion metal bond layer shown comprises:
[0036] 1. Single crystal high temperature alloy turbine blades are used as the substrate, IC10 alloy is selected as the substrate alloy, NiCoCrAlYRe coating is prepared on IC10 alloy by arc ion plating equipment, and NiCoCrAlYRe target is used to achieve the deposition of NiCoCrAlYRe coating. Raw materials are selected, NiCoCrAlYRe target is used, in which the elements are 33% Ni, 29% Co, 17% Cr, 15.5% Al, 0.5% Y, 5% Re by mass, and the target is installed on the cathode seat of the vacuum arc coating machine.
[0037] 2. Activate the surface of parts by grinding flow treatment. Add corundum sand with a particle size of 0.154 mm into the liquid sand blasting machine. The working pressure is 0.2MPa~0.5MPa and the treatment time is 10min.
[0038] 3. Clean and dry
[0039] 4. Use a fixture to load the parts into the vacuum chamber of the arc ion plating equipment.
[0040] 5. Install the parts to be coated in the vacuum chamber and evacuate the vacuum to a degree of 6×10 -3 Pa~7×10 - 3 Pa, bombardment heating, arc current I = 550A ~ 750A, workpiece bias U = 200V ~ 300V, bombardment time is 5min, then a layer of NiCoCrAlYRe is deposited on the surface of the part, arc current I = 550A ~ 750A, workpiece bias U = 20V ~ 30V, deposition time is 150min ~ 200min, vacuum degree is 6×10 -3 Pa~7×10 -3 Pa.
[0041] 6. Diffusion treatment of parts with NiCoCrAlYRe coating, diffusion treatment, vacuum degree 10 -2 Pa~10 -3 Pa, temperature 850-900℃, time 3h.
[0042] from Figure 1 It can be seen that the bonding layer ( Figure 1 The middle layer in the coating has a dense structure and is well bonded to the substrate. After a thermal shock test (5 minutes of heat preservation and 5 minutes of cooling) at 1100 degrees Celsius, the coating has no wrinkling, cracking, peeling, or shedding for more than 4000 times, and is in good condition. Figure 2It can be seen that the expansion coefficient of the NiCoCrAlYRe metal bonding layer of the present invention changes little with temperature. In the temperature range of 50°C to 1150°C, the thermal expansion coefficients of samples NiCoCrAlYRe-1 and NiCoCrAlYRe-2 are (11.89-17.68) x10 -6 K -1 and (11.62~17.61)x10 -6 K -1 .
[0043] The above is only a specific embodiment of the present invention, and the present invention is described in detail. The unexplained part is a conventional technology. However, the protection scope of the present invention is not limited to this. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. The protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A NiCoCrAlYRe low expansion metal bonding layer, characterized in that: It forms a metallurgical bond with a single crystal high temperature alloy matrix, wherein the element components are 33% Ni, 29% Co, 17% Cr, 15.5% Al, 0.5% Y, and 5% Re respectively by mass.
2. The metal bonding layer according to claim 1, characterized in that: The single crystal high temperature alloy substrate is an IC10 alloy substrate.
3. A method for preparing a NiCoCrAlYRe low expansion metal bonding layer, characterized in that: The method of preparing any one of the metal bonding layers as claimed in claims 1 to 2 comprises: Step S01: using a NiCoCrAlYRe target material, and installing the target material on a cathode seat of a vacuum arc coating machine; Step S02: performing surface activation treatment on the single crystal high temperature alloy substrate; Step S03: cleaning and drying the surface of the single crystal high temperature alloy substrate; Step S04: depositing a coating on the surface of the single crystal high temperature alloy substrate; Step S05: performing diffusion treatment on the deposited coating.
4. The method according to claim 3, characterized in that The surface activation treatment method in step S02 is a grinding fluid treatment method.
5. The method according to claim 4, characterized in that The grinding fluid treatment method is to use corundum sand with a particle size of 0.154 mm to add it into a liquid sand blowing machine for sand blowing. The working pressure is 0.2MPa~0.5MPa and the treatment time is 10min.
6. The method according to claim 3, characterized in that Step S04 also includes: deposition parameters are arc current I=550A-750A, workpiece bias voltage U=20V-30V, deposition time 150min-200min, vacuum degree 6×10 -3 Pa~7×10 -3 Pa.
7. The method according to claim 3, characterized in that Step S04 also includes: Preheating step: vacuum degree reaches 6×10 -3 Pa~7×10 -3 Pa later, bombardment heating, arc current I = 550A ~ 750A, workpiece bias U = 200V ~ 300V, bombardment time is 5min.
8. The method according to claim 3, characterized in that Step S05 also includes: the vacuum degree of the diffusion process is 1×10 -2 Pa~1×10 -3 Pa, temperature is 850℃-900℃, time is 3h.
Citation Information
Patent Citations
MCrAlY+AlSiY composite coating and preparation technique thereof
CN101724301A
High-performance thermal barrier coating of aero-engine blade and multi-process combined preparation method
CN111560584A
Thermal barrier coating and preparation method thereof
CN116479380A
Double-layer thermal barrier coating with advanced interface
CN116615573A
Engine member, exhaust vale, piston crown and internal combustion engine
JP2003278597A