Self-supporting nickel-iron-molybdenum oxygen evolution catalyst, preparation and application of self-supporting nickel-iron-molybdenum oxygen evolution catalyst in hydrogen production through alkaline water decomposition
The self-supporting nickel-iron-molybdenum oxygen evolution catalyst is prepared by a one-step water bath method, which solves the problems of high cost and complex preparation process of precious metal catalysts, achieves efficient preparation of catalysts at low temperatures, improves electrocatalytic performance and stability, and is suitable for high current density electrocatalytic water splitting.
Patent Information
- Application Number
- CN202410848534.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
AI Technical Summary
The precious metal catalyst used in the existing electrocatalytic moisture desorption oxygen reaction is high in cost and has poor stability. The preparation process is complex and it is difficult to maintain activity and stability at high current density. In addition, the traditional preparation method requires high temperature and high pressure, which limits industrial application.
A one-step water bath method is used to prepare a self-supporting nickel-iron-molybdenum oxygen evolution catalyst. By reacting nickel salt, iron salt, ammonium molybdate, urea and ammonium fluoride in water, a catalyst with a nanosheet-wrapped pyramid structure is formed, which significantly increases the electrochemical specific surface area. and reactivity.
It achieves efficient preparation of catalysts at lower temperatures, reduces energy consumption and costs, significantly improves electrocatalytic performance at high current densities, reduces energy consumption, and performs efficient oxygen evolution reactions at lower overpotentials, improving improve energy conversion efficiency.
Smart Images

Figure CN118773652A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrocatalytic water-decomposition oxygen catalysts, and more specifically, relates to a self-supporting nickel-iron-molybdenum oxygen evolution catalyst, and its preparation and application in alkaline water-decomposition oxygen electrodes. Background Art
[0002] Hydrogen energy is touted as the ideal energy source of the 21st century because of its abundant sources, small molecular weight, high energy density and environmentally friendly use process. In addition, as a good carrier of renewable energy, it can not only realize the long cycle of electrical energy and thermal energy more economically, but also achieve large-scale energy storage. Electrocatalytic water splitting is an attractive method to provide clean and renewable hydrogen energy. However, the oxygen evolution reaction (OER) involves a multi-electron transfer step with four protons, which has slow kinetics and requires a high overpotential, which has become a bottleneck for water splitting. Precious metal catalysts (such as RuO2 and IrO2) are currently the most popular OER electrocatalysts, but their high cost and stability issues under high current density applications have seriously hindered their large-scale application.
[0003] Currently, many efficient and economical electrocatalysts, such as transition metal-based oxides, hydroxides, phosphides, sulfides, and nitrides, have been studied and developed as candidate catalysts for OER. However, the OER performance of the above catalysts is usually limited at relatively low current densities (e.g., 10 mA / cm 2 ), it is unclear whether they can maintain high activity and good stability at high current density. 2 ) is still a huge challenge for practical application.
[0004] In addition, the complexity of the catalyst preparation process and cost control are also current problems. Traditional preparation methods usually involve multi-step processes, which not only increases the difficulty of technical implementation, but also pushes up the overall production cost. For example, the common hydrothermal method requires the use of a reactor to meet the high temperature and high pressure catalyst growth environment, which seriously restricts its feasibility for large-scale industrial application. Although electrodeposition technology has been proposed as an alternative to simplify the preparation process, the initial equipment investment and maintenance costs are high, and the processing time is long, affecting production efficiency. More importantly, the performance of the catalysts deposited directly by these electrochemical methods is often unsatisfactory and it is difficult to meet the needs of high-efficiency water electrolysis reactions.
[0005] Therefore, the current market urgently needs to reform the catalyst preparation method, greatly simplify the preparation process, and reduce economic costs. In addition, the technology pursued should also be able to promote the rapid response ability of the catalyst, ensure its high activity and stability, so as to promote the electrolysis of water technology towards a more economical, green and efficient industrialization direction.
[0006] The invention method disclosed in the invention patent with publication number CN111871421A prepares nanowire catalysts with hydrotalcite-like nanosheets as basic building blocks by using urea hydrolysis at 100°C for 24 hours. This process must be performed in a high-pressure reactor, which not only limits the feasibility of large-scale production, but also increases production costs and reduces overall efficiency due to the long reaction cycle due to the reliance on special equipment. Summary of the invention
[0007] The present invention solves the technical problems that the oxygen evolution catalyst in the prior art needs to use expensive precious metal catalysts, has poor catalytic activity and stability, and has a complicated preparation process. The present invention selects a simple one-step water bath method to prepare a self-supporting nickel-iron-molybdenum oxygen evolution catalyst, which has a morphology of a pyramid wrapped with nanosheets, significantly improves the electrochemical specific surface area, exposes more active sites, and thus ensures efficient and stable alkaline water oxygen evolution reaction at high current density.
[0008] According to a first aspect of the present invention, a method for preparing a self-supporting nickel-iron-molybdenum oxygen evolution catalyst is provided, wherein nickel salt, iron salt, ammonium molybdate, urea and ammonium fluoride are added to water to obtain a mixed solution, a nickel substrate is added to the mixed solution, and then the mixed solution is heated in a water bath at a temperature of 85 to 95° C. for 6 h to 12 h, thereby obtaining a self-supporting nickel-iron-molybdenum oxygen evolution catalyst.
[0009] Preferably, in the mixed solution, the concentration of the iron salt is 0.002-0.009 mol / L.
[0010] Preferably, the concentration of the ammonium molybdate is 0.01-0.02 mol / L.
[0011] Preferably, in the mixed solution, the concentration of the nickel salt is 0.01-0.03 mol / L.
[0012] Preferably, in the mixed solution, the concentration of urea is 0.2-0.4 mol / L.
[0013] Preferably, in the mixed solution, the concentration of ammonium fluoride is 0.05-0.1 mol / L.
[0014] Preferably, the nickel substrate is a nickel plate, nickel foam, nickel felt or nickel sheet.
[0015] According to another aspect of the present invention, a self-supporting nickel-iron-molybdenum oxygen evolution catalyst prepared by any one of the methods is provided.
[0016] According to another aspect of the present invention, there is provided the use of the self-supporting nickel-iron-molybdenum oxygen evolution catalyst as an anode catalyst for alkaline water decomposition to produce hydrogen.
[0017] Preferably, the current density of the alkaline water decomposition hydrogen production is 500 mA / cm 2 above.
[0018] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:
[0019] (1) The electrode preparation process of the present invention is highly integrated, abandoning the cumbersome multi-step synthesis path, and realizing a single-step preparation at a relatively low temperature (85-95°C). It does not require high pressure and can be obtained only through a water bath reaction, which greatly reduces energy consumption and cost. Without the support of high-temperature and high-pressure equipment, the large-scale production of the electrode becomes possible, greatly broadening its feasibility in practical industrial applications. The present invention can obtain a nickel-iron-molybdenum composite nanostructure with a pyramid structure wrapped in nanosheets of different morphologies by regulating the synthesis process through the water bath time (6h to 12h). This unique structural characteristic not only increases the electrochemical specific surface area and enhances the adsorption capacity of the electrode material for the intermediate, but also promotes the effective participation of lattice oxygen, accelerates the generation and release process of oxygen molecules, and reduces unnecessary energy consumption, thereby essentially optimizing the electrocatalytic performance.
[0020] (2) The core advantage of the self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared by the present invention is that it successfully utilizes the lattice oxygen oxidation mechanism (LOM) to drive the efficient oxygen evolution reaction, cleverly bypassing the limitations of the traditional adsorbent evolution mechanism (AEM). The activation energy barrier of the reaction is reduced, so that the electrochemical oxygen evolution process can be carried out efficiently at a lower overpotential, significantly improving the energy conversion efficiency.
[0021] (3) The product prepared by the present invention has excellent oxygen evolution characteristics in alkaline electrolyte, and the current density reaches 500, 1000, 2000 and 3000 mA / cm 2 When , the corresponding overpotentials are 269, 289, 332 and 342 mV, respectively, indicating that it has efficient electrocatalytic oxygen evolution reaction activity, can significantly reduce the reaction barrier, and reduce the consumption of electrical energy in the process of electrocatalytic water decomposition.
[0022] (4) The present invention prepares a self-supporting nickel-iron-molybdenum oxygen evolution electrode for hydrogen production by alkaline water decomposition through a one-step water bath, which has the characteristics of simple synthesis process and easy control of components. The alkaline anion exchange membrane electrolyzer constructed with the prepared nickel-iron-molybdenum electrode for hydrogen production by alkaline water decomposition has low price and excellent activity and stability, and has broad research prospects and strategic significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1This is a scanning electron microscope image of a self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in Example 1 of the present invention, where the scale a represents 1 μm and the scale b represents 200 nm.
[0024] Figure 2 This is the XRD spectrum of a self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in Example 1 of the present invention.
[0025] Figure 3 Polarization curve of oxygen evolution reaction of a self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in Example 1 of the present invention in 1M KOH electrolyte.
[0026] Figure 4 This is the electrochemical impedance spectrum of a self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in Example 1 of the present invention in 1M KOH electrolyte.
[0027] Figure 5 This is the stability curve of a self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in Example 1 of the present invention in 1M KOH electrolyte.
[0028] Figure 6 Scanning electron microscope images of the self-supporting nickel-iron-molybdenum oxygen evolution electrodes with different reaction times prepared in Example 2 of the present invention, where the scale bar represents 2 μm.
[0029] Figure 7 Polarization curves of oxygen evolution reaction of the self-supporting nickel-iron-molybdenum oxygen evolution electrode with different concentrations of iron nitrate prepared in Example 3 of the present invention in 1M KOH electrolyte.
[0030] Figure 8 Polarization curves of oxygen evolution reaction of the self-supporting nickel-iron-molybdenum oxygen evolution electrode with different concentrations of ammonium molybdate prepared in Example 4 of the present invention in 1M KOH electrolyte. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0032] The present invention selects a simple one-step water bath method to prepare a self-supporting nickel-iron-molybdenum oxygen evolution catalyst, specifically, nickel salt, iron salt, ammonium molybdate, urea and ammonium fluoride are added into water to form a uniform mixed solution, the mixed solution is poured into a beaker, and then a conductive pure nickel substrate is placed, and heated in a water bath, so that the nickel-iron-molybdenum catalyst material can be grown on the conductive pure nickel substrate.
[0033] In some embodiments, the nickel salt is a chloride, sulfate, acetate or nitrate, and the iron salt is a chloride, sulfate, acetate or nitrate.
[0034] In some embodiments, the conductive pure nickel substrate is selected from any one of nickel plate, nickel foam, nickel felt, and nickel sheet.
[0035] In some embodiments, in the mixed solution, the concentration of the nickel salt is 0.01-0.03 mol / L.
[0036] In some embodiments, the concentration of the iron salt is 0.002-0.009 mol / L.
[0037] In some embodiments, the concentration of the ammonium molybdate is 0.01-0.02 mol / L.
[0038] In some embodiments, the concentration of urea is 0.2-0.4 mol / L.
[0039] In some embodiments, the concentration of ammonium fluoride is 0.05-0.1 mol / L.
[0040] In some embodiments, the hydrothermal reaction is carried out at a temperature of 85 to 95° C. and for a time of 6 to 12 hours.
[0041] The self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared by the invention has high activity and high stability.
[0042] The electrocatalytic water splitting experiments involved in the following examples all used the prepared nickel-iron-molybdenum oxygen evolution electrode as the anode in a standard three-electrode system (the anode catalyst was used as the working electrode, and the area was 1×1 cm 2 ; mercury / mercuric oxide as reference electrode; platinum sheet as counter electrode), the electrolyte was 1 M KOH.
[0043] The following are specific embodiments
[0044] Example 1
[0045] A self-supporting nickel-iron-molybdenum oxygen evolution electrode is prepared and used for hydrogen production by decomposing alkaline water. The steps of the preparation method described in this embodiment are:
[0046] Step 1: dissolve nickel nitrate hexahydrate in deionized water at a concentration of 0.02 mol / L and continue stirring for 5 minutes to obtain solution I;
[0047] Step 2: dissolve ferric nitrate hexahydrate in solution I at a concentration of 0.006 mol / L and continue stirring for 5 minutes to obtain solution II;
[0048] Step 3: Dissolve ammonium molybdate in solution II at a concentration of 0.015 mol / L and continue stirring for 5 minutes to obtain solution III;
[0049] Step 4: dissolve urea in solution III at a concentration of 0.3 mol / L and continue stirring for 5 minutes to obtain solution IV;
[0050] Step 5: dissolving ammonium fluoride in solution IV at a concentration of 0.075 mol / L and stirring for 5 minutes to obtain solution V;
[0051] Step 6: The solution V is transferred to a beaker, and a piece of clean nickel foam is added, and the mixture is reacted at 90° C. for 6 hours;
[0052] Step 7: The catalyst grown on the nickel foam obtained in step 6 is washed with deionized water and ethanol three to five times, and then dried at room temperature for 2 hours to obtain a highly active and stable self-supporting nickel-iron-molybdenum oxygen evolution electrode.
[0053] In the method for preparing the self-supporting nickel-iron-molybdenum oxygen evolution electrode, the nickel salt and the iron salt are nitrates.
[0054] The self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in Example 1 was directly subjected to microscopic morphology ( Figure 1 ) and X-ray diffraction ( Figure 2 ) characterization. Figure 1 As shown in a in FIG. 1 , the prepared nickel-iron-molybdenum electrode is an array structure composed of nanosheets. Figure 1 As can be seen from b, the nanosheet is wrapped with a pyramid structure. Figure 2 As shown, the XRD diffraction peaks show that the prepared nickel-iron-molybdenum electrode is mainly composed of two phases, NiFe LDH and Fe2(MoO4)3.
[0055] Figure 3 This is the polarization curve of oxygen evolution reaction in alkaline solution of the self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in Example 1. Figure 3 It can be seen that the alkaline water oxygen evolution reaction using this catalyst has a high current density of 500, 1000, 2000 and 3000 mA / cm 2 When , the corresponding overpotentials are 269, 289, 332 and 342 mV, respectively, indicating that it has efficient electrocatalytic oxygen evolution reaction activity, can significantly reduce the reaction barrier, and reduce the consumption of electrical energy in the process of electrocatalytic water decomposition.
[0056] Figure 4 This is the electrochemical impedance spectrum of the self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in Example 1 in alkaline water. Figure 4It can be seen that this self-supporting nickel-iron-molybdenum oxygen evolution electrode has an extremely small charge transfer resistance, which is much smaller than the foam nickel substrate itself and the commercial precious metal catalyst (RuO2), indicating that the electrode can complete rapid charge transfer at high current density.
[0057] Figure 5 This is the stability curve of the self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in Example 1 in 1M KOH electrolyte. Figure 5 It can be seen that this self-supporting nickel-iron-molybdenum oxygen evolution electrode has excellent stability in alkaline electrolyte and can 2 It can run stably for 110 hours under high current density and remain stable.
[0058] It can be seen that the self-supporting nickel-iron-molybdenum oxygen evolution electrode prepared in this embodiment is composed of a pyramid structure wrapped with nanosheets. It has the characteristics of good conductivity and high activity when used as an anode catalyst for alkaline water decomposition, and exhibits excellent activity and stability at high current density.
[0059] Example 2
[0060] A self-supporting nickel-iron-molybdenum oxygen evolution electrode is prepared and used for hydrogen production by decomposing alkaline water. The steps of the preparation method described in this embodiment are:
[0061] Step 1: dissolve nickel nitrate hexahydrate in deionized water at a concentration of 0.02 mol / L and continue stirring for 5 minutes to obtain solution I;
[0062] Step 2: dissolve ferric nitrate hexahydrate in solution I at a concentration of 0.006 mol / L and continue stirring for 5 minutes to obtain solution II;
[0063] Step 3: Dissolve ammonium molybdate in solution II at a concentration of 0.015 mol / L and continue stirring for 5 minutes to obtain solution III;
[0064] Step 4: dissolve urea in solution III at a concentration of 0.3 mol / L and continue stirring for 5 minutes to obtain solution IV;
[0065] Step 5: dissolving ammonium fluoride in solution IV at a concentration of 0.075 mol / L and stirring for 5 minutes to obtain solution V;
[0066] Step 6: The solution V is transferred to a beaker, and a piece of clean nickel foam is added, and four control experiments are set up at 90° C. for different reaction times (3 hours, 6 hours, 9 hours and 12 hours);
[0067] Step 7: The catalyst grown on the nickel foam obtained in step 6 is washed with deionized water and ethanol three to five times, and then dried at room temperature for 2 hours to obtain self-supporting nickel-iron-molybdenum oxygen evolution electrodes with different reaction times.
[0068] The self-supporting nickel-iron-molybdenum oxygen evolution electrodes with different reaction times prepared in Example 2 were directly subjected to microscopic morphology ( Figure 6 ) characterization. Figure 6 As shown in a in FIG. 1 , the self-supporting nickel-iron-molybdenum electrode prepared after 3 hours of reaction is an array structure composed of nanosheets. Figure 6 As shown in b, the self-supporting nickel-iron-molybdenum electrode prepared after 6 hours of reaction is an array of nanosheets with protrusions. Figure 1 From b, we can see that the protrusion is a pyramid structure. Figure 6 As shown in Figure c, the self-supporting nickel-iron-molybdenum electrode prepared after 9 hours of reaction is a composite structure of pyramids grown on an array of nanosheets. Figure 6 As shown in d, the self-supporting nickel-iron-molybdenum electrode prepared after 12 hours of reaction is a composite structure of pyramids grown on an array of nanosheets. As the reaction time increases, the pyramid structure grows from the inside out and the number increases.
[0069] Example 3
[0070] A self-supporting nickel-iron-molybdenum oxygen evolution electrode is prepared and used for hydrogen production by decomposing alkaline water. The steps of the preparation method described in this embodiment are:
[0071] Step 1: dissolve nickel nitrate hexahydrate in deionized water at a concentration of 0.02 mol / L and continue stirring for 5 minutes to obtain solution I;
[0072] Step 2: dissolving ferric nitrate hexahydrate in solution I at concentrations of 0.002, 0.004, 0.006 and 0.008 mol / L and stirring for 5 minutes to obtain solution II;
[0073] Step 3: Dissolve ammonium molybdate in solution II at a concentration of 0.015 mol / L and continue stirring for 5 minutes to obtain solution III;
[0074] Step 4: dissolve urea in solution III at a concentration of 0.3 mol / L and continue stirring for 5 minutes to obtain solution IV;
[0075] Step 5: dissolving ammonium fluoride in solution IV at a concentration of 0.075 mol / L and stirring for 5 minutes to obtain solution V;
[0076] Step 6: The solution V is transferred to a beaker, and a piece of clean nickel foam is added, and four control experiments are set up at 90° C. for different reaction times (3 hours, 6 hours, 9 hours and 12 hours);
[0077] Step 7: The catalyst grown on the nickel foam obtained in step 6 is washed with deionized water and ethanol three to five times, and then dried at room temperature for 2 hours to obtain self-supporting nickel-iron-molybdenum oxygen evolution electrodes with different ammonium molybdate concentrations.
[0078] The self-supporting nickel-iron-molybdenum oxygen evolution electrode with different concentrations of iron nitrate prepared in this example has good catalytic activity (such as Figure 7 It showed excellent activity at high current density, and the best performance was achieved when the iron nitrate concentration was 0.006 mol / L.
[0079] Example 4
[0080] A self-supporting nickel-iron-molybdenum oxygen evolution electrode is prepared and used for hydrogen production by decomposing alkaline water. The steps of the preparation method described in this embodiment are:
[0081] Step 1: dissolve nickel nitrate hexahydrate in deionized water at a concentration of 0.02 mol / L and continue stirring for 5 minutes to obtain solution I;
[0082] Step 2: dissolve ferric nitrate hexahydrate in solution I at a concentration of 0.006 mol / L and continue stirring for 5 minutes to obtain solution II;
[0083] Step 3: dissolve ammonium molybdate in solution II at concentrations of 0.012, 0.014, 0.015 and 0.016 mol / L and stir for 5 minutes to obtain solution III;
[0084] Step 4: dissolve urea in solution III at a concentration of 0.3 mol / L and continue stirring for 5 minutes to obtain solution IV;
[0085] Step 5: dissolving ammonium fluoride in solution IV at a concentration of 0.075 mol / L and stirring for 5 minutes to obtain solution V;
[0086] Step 6: The solution V is transferred to a beaker, and a piece of clean nickel foam is added, and four control experiments are set up at 90° C. for different reaction times (3 hours, 6 hours, 9 hours and 12 hours);
[0087] Step 7: The catalyst grown on the nickel foam obtained in step 6 is washed with deionized water and ethanol three to five times, and then dried at room temperature for 2 hours to obtain self-supporting nickel-iron-molybdenum oxygen evolution electrodes with different ammonium molybdate concentrations.
[0088] The self-supporting nickel-iron-molybdenum oxygen evolution electrode with different concentrations of ammonium molybdate prepared in this example has good catalytic activity (such as Figure 8As shown in the figure, it exhibits excellent activity at high current density, and the best performance is achieved when the ammonium molybdate concentration is 0.015 mol / L.
[0089] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a self-supporting nickel-iron-molybdenum oxygen evolution catalyst, characterized in that: Nickel salt, iron salt, ammonium molybdate, urea and ammonium fluoride are added into water to obtain a mixed solution, a nickel substrate is added into the mixed solution, and then the mixed solution is heated in a water bath at a temperature of 85 to 95° C. for 6 to 12 hours to obtain a self-supporting nickel-iron-molybdenum oxygen evolution catalyst.
2. The method for preparing a self-supporting nickel-iron-molybdenum oxygen evolution catalyst according to claim 1, wherein: In the mixed solution, the concentration of the iron salt is 0.002-0.009 mol / L.
3. The method for preparing a self-supporting nickel-iron-molybdenum oxygen evolution catalyst according to claim 1, wherein: The concentration of the ammonium molybdate is 0.01-0.02 mol / L.
4. The method for preparing a self-supporting nickel-iron-molybdenum oxygen evolution catalyst according to claim 1, wherein: In the mixed solution, the concentration of the nickel salt is 0.01-0.03 mol / L.
5. The method for preparing a self-supporting nickel-iron-molybdenum oxygen evolution catalyst according to claim 1, wherein: In the mixed solution, the concentration of urea is 0.2-0.4 mol / L.
6. The method for preparing a self-supporting nickel-iron-molybdenum oxygen evolution catalyst according to claim 1, characterized in that: In the mixed solution, the concentration of ammonium fluoride is 0.05-0.1 mol / L.
7. The method for preparing a self-supporting nickel-iron-molybdenum oxygen evolution catalyst according to claim 1, characterized in that: The nickel substrate is a nickel plate, nickel foam, nickel felt or nickel sheet.
8. A self-supporting nickel-iron-molybdenum oxygen evolution catalyst prepared according to any one of claims 1 to 7.
9. Application of the self-supporting nickel-iron-molybdenum oxygen evolution catalyst as claimed in claim 8 as an anode catalyst for hydrogen production by alkaline water decomposition.
10. The use according to claim 9, characterized in that The current density of the alkaline water decomposition hydrogen production is 500mA / cm 2 above.
Citation Information
Cited By
Iron-doped molybdate nano composite material, preparation method thereof and method for oxygen evolution of alkaline salt through electro-catalysis of iron-doped molybdate nano composite material
CN120026352A