Carbon dioxide reinjection well cementing method
Through the casing and liner cementing technology, the problem of wellbore cement sheath and casing corrosion in carbon dioxide geological storage is solved, the pressure bearing capacity and sealing of the well are improved, and the stable operation of offshore long-reach wells is ensured.
Patent Information
- Application Number
- CN202411156210.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-22
AI Technical Summary
In carbon dioxide geological storage, after the well is injected with carbon dioxide, it will corrode the wellbore cement sheath and casing in the storage area in the presence of water, resulting in imperfect integrity of the storage system, and the cementing quality of offshore extended-reach wells is low and there is pressure. Poor capabilities and risk of leakage.
A carbon dioxide reinjection well cementing method is adopted, including casing cementing, liner cementing and liner tieback cementing processes. The cementing fluid is pumped in, the mud pump is switched for displacement, pressure control and detection, and waiting for solidification. and other steps to ensure the sealing and pressure-bearing capacity of the casing and wellbore to prevent carbon dioxide leakage.
It improves the corrosion resistance of the wellbore cement sheath and casing, enhances the pressure-bearing capacity of the well, reduces the risk of cementing loss, and ensures long-term reliable operation of the well in the marine environment.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of well cementing in petroleum drilling and production engineering, and in particular to a well cementing method for a carbon dioxide reinjection well. Background Art
[0002] Since the late 1980s, industrial production and human life have consumed a large amount of fossil energy, resulting in increasing carbon dioxide emissions. The resulting greenhouse effect has led to an increasingly severe global climate environment. CO2 capture, utilization and storage (CCUS) is currently an important technical option for achieving large-scale zero-emission fossil energy and is the main means of carbon emission reduction in the power, steel, cement and chemical industries in the future.
[0003] In specific practice, carbon sequestration technology includes three aspects: capture, transportation and storage. Carbon capture and storage, often as the core of carbon sequestration technology, has received widespread attention worldwide. In the geological storage of carbon dioxide, the storage wells (buried storage wells) include injection wells, production wells and abandoned wells. After the well is injected with carbon dioxide, it will corrode the wellbore cement ring and casing in the storage area under the condition of water, thereby forming a channel for carbon dioxide leakage, resulting in the integrity of the storage system being no longer perfect. When offshore extended reach wells are used as reinjection wells, they face problems such as low cementing quality, shallow burial depth of the reinjection layer, poor bearing capacity of the formation, the risk of faults, easy cementing leakage, large dogleg deflection, and difficulty in centering the long stable inclined section casing. Secondly, due to the presence of CO2, the casing tail pipe has poor corrosion resistance.
[0004] In view of the above problems, the present invention document proposes a carbon dioxide reinjection well cementing method. Summary of the invention
[0005] The present invention provides a carbon dioxide reinjection well cementing method, which solves the above-mentioned problems.
[0006] The present invention provides the following technical solutions:
[0007] A carbon dioxide reinjection well cementing method comprises the following steps:
[0008] S1, casing cementing;
[0009] S1.1. Preparation work before cementing;
[0010] S1.2, pump in cementing fluid;
[0011] S1.3, switch to mud pump for displacement;
[0012] S1.4, perform pressure control and testing;
[0013] S1.5, wait for solidification;
[0014] S2, liner cementing;
[0015] S2.1, repeat step S1.1;
[0016] S2.2, tailing slurry is pumped in to fill the bottom of the wellbore;
[0017] S2.3, switch to the mud pump for displacement;
[0018] S2.4, perform pressure control and testing;
[0019] S2.5. Set the top packer, remove the running tool, and circulate and clean the cement slurry;
[0020] S2.6, waiting for solidification;
[0021] S3, tail pipe back-connection and cementing;
[0022] S3.1. Prepare for tie-back cementing work and conduct tie-back sealing test;
[0023] S3.2. Remove the mud in the wellbore and make preliminary preparations for cleaning after the surface pipeline pressure test;
[0024] S3.3, use the cementing pump to mix the lead slurry and cementing fluid evenly, and use the cementing pump to mix the tail slurry and fill the bottom of the wellbore;
[0025] S3.4, quickly remove the circulation head, put in the casing top plug, quickly connect the buckle and run the casing, and connect the top drive to run the casing into the wellbore;
[0026] S3.5. Add additional pressure to the final displacement pressure to meet the design requirements, and then maintain the pressure for 5 minutes to ensure that the casing is safely installed and forms a tight seal with the wellbore wall;
[0027] S3.6. Slowly lower the insert seal until it is fully inserted into the tie-back tube. When the second seal is inserted into the tie-back tube, release all the pressure in the casing and keep the ground pressure relief valve open. Continue to lower the insert seal and fully insert it into the tie-back tube while applying a certain downward pressure.
[0028] S3.7. Check whether the markings on the casing are consistent with those on the first trial insertion. If they are consistent, continue to press down until the designed hanging weight sets the casing packer and hanger, and maintain for a certain period of time to ensure the correct installation depth and position of the casing, as well as the effectiveness of the hanger and packer;
[0029] S3.8. Depressurize the cementing pump and check for backflow. If there is backflow, replace the backflow volume to hold the pressure and wait for solidification to ensure that there is no leakage of cementing fluid in the casing, and then wait for solidification.
[0030] In a possible design, the step S1.1 specifically includes the following steps:
[0031] S1.1.1. Determine the size of the casing centralizer, and run the casing and add the centralizer in sequence;
[0032] S1.1.2. Use cementing pump to pump water through the surface pipeline and test the pressure. The pressure should meet the maximum pump pressure required in the cementing method to ensure that the pipeline is firm and usable during the cementing process;
[0033] S1.1.3. Use the cementing pump to flush the flushing fluid to flush the impurities out of the wellbore and fully clean the wellbore wall surface.
[0034] In a possible design, step S1.2 specifically includes the following steps:
[0035] S1.2.1. Stop the cementing pump and open the stopper pin under the cement head to release the bottom rubber plug;
[0036] S1.2.2. Use cementing pump to pump in the lead slurry mixed water to pressurize the rubber plug, and the pumped lead slurry mixed water pushes the bottom rubber plug to the bottom of the wellbore, so that the cementing fluid starts to fill the wellbore from the bottom of the casing;
[0037] S1.2.3, mix the mixed slurry and cementing fluid evenly through the cementing pump;
[0038] S1.2.4. Use a cementing pump to mix the tailings slurry and pump the tailings slurry into the wellbore to fill the bottom of the wellbore.
[0039] In a possible design, step S1.3 specifically includes the following steps:
[0040] S1.3.1. Stop the cementing pump and open the stopper pin on the cement head to release the top rubber plug;
[0041] S1.3.2, cementing pump pumps tailings slurry into the hydraulic plug;
[0042] S1.3.3. Switch to the mud pump for displacement, and in the final stage switch to a small displacement pump.
[0043] In a possible design, step S1.4 specifically includes the following steps:
[0044] S1.4.1. After reaching the final displacement pressure, add additional pressure to meet the design requirements and maintain the pressure for a certain period of time to ensure the reliability of cementing. At the same time, check whether there is a pressure drop to ensure that there is no leakage of cementing fluid;
[0045] S1.4.2. Open the pressure relief valve of the cementing pump and check if there is backflow. If there is backflow, replace the backflow volume and hold the pressure to wait for solidification.
[0046] In a possible design, the step S2.2 specifically includes the following steps:
[0047] S2.2.1. Use a mud pump to pump in the isolation fluid, a cementing pump to pump in the flushing fluid, and a cementing pump to pump in the drilling water;
[0048] S2.2.2, mix the mixed slurry and cementing fluid evenly through the cementing pump;
[0049] S2.2.3. Use a cementing pump to mix the tailings slurry and pump the tailings slurry into the wellbore to fill the bottom of the wellbore.
[0050] In a possible design, step S2.3 specifically includes the following steps:
[0051] S2.3.1. Stop the cementing pump and open the stopper pin on the cement head to release the top rubber plug;
[0052] S2.3.2, cementing pump pumps tailings slurry mixed with hydraulic plug;
[0053] S2.3.3. Switch to the mud pump for displacement, and in the final stage switch to a small displacement pump.
[0054] In a possible design, step S2.4 specifically includes the following steps:
[0055] S2.4.1. After reaching the final displacement pressure, add additional pressure to meet the design requirements and maintain the pressure for a certain period of time to ensure the reliability of cementing. At the same time, check whether there is a pressure drop to ensure that there is no leakage of cementing fluid;
[0056] S2.4.2. Open the pressure relief valve of the cementing pump and check if there is backflow. If there is backflow, replace the backflow volume and hold the pressure to wait for solidification.
[0057] In a possible design, step S3.1 specifically includes the following steps:
[0058] S3.1.1. During the well cleaning process, a certain volume of thick slurry is placed below the tie-back tube to fill the bottom of the tie-back tube;
[0059] S3.1.2 Check the integrity of the inserted seal and packer, including the number of packer shear pins, and use double float collars to ensure the integrity of the inserted seal and packer, and use double float collars correctly to provide effective sealing and isolation;
[0060] S3.1.3. Replace the long elevator before running the casing, run the casing and add the centralizer in sequence, apply thread glue to the casing buckle below the float hoop, and grout to check the performance of the float valve;
[0061] S3.1.4. The cementing pump performs pressure test on the tie-back seal to test the sealing performance of the tie-back seal and ensure that the sealing system is normal;
[0062] S3.1.5. After the circulation hole is raised to the top of the tie-back tube, turn on the cementing pump to confirm that the circulation channel is unobstructed, then stop the cementing pump, install the casing slips, and connect the cementing circulation head and cementing pipeline to establish the circulation channel in preparation for cementing operations.
[0063] In a possible design, step S3.2 specifically includes the following steps:
[0064] S3.2.1. Before cementing, start to remove the mud in the wellbore by circulating at a small displacement and gradually increase the displacement to the designed displacement to ensure the wellbore is clean;
[0065] S3.2.2. The cementing pump passes water through the surface pipeline and tests the pressure to test the sealing performance of the surface pipeline to ensure that the cementing fluid will not leak;
[0066] S3.2.3. Use the cementing pump to pump flushing fluid to clean the wellbore and prepare for the next cementing fluid pumping.
[0067] It is to be understood that the foregoing general description and the following detailed description are exemplary only and are not restrictive of the invention.
[0068] The present invention sequentially performs casing cementing, liner cementing and liner tie-back cementing processes for different well sections, which can improve the corrosion resistance of the wellbore cement ring and casing, enhance the pressure bearing capacity of the well, reduce the risk of cementing leakage, prevent the formation of carbon dioxide leakage channels, and ensure the long-term reliable operation of the well in the marine environment. DETAILED DESCRIPTION
[0069] The embodiments of the present invention are described below in conjunction with the embodiments of the present invention.
[0070] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, a detailed description is given below in conjunction with the specific embodiments of the present invention. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.
[0071] Example
[0072] This example is based on an offshore extended reach well in a certain place. The wellbore and casing data are shown in the following table:
[0073]
[0074] This embodiment provides a carbon dioxide reinjection well cementing method, comprising the following steps:
[0075] Step 1: Casing cementing
[0076] 1. Preparation:
[0077] 1.1. Check the casing cement head and install the rubber plug in accordance with relevant regulations.
[0078] 1.2. Determine the size of the casing centralizer.
[0079] 1.3. Before starting cementing operations, reserve samples of cement, mixed water, drilling water, seawater, etc. for cementing.
[0080] 1.4. Lower the casing and add the centralizer in sequence, apply thread glue to the casing buckle below the float hoop, and grout to check the performance of the float valve.
[0081] 1.5. After the casing enters the open hole, control the lowering speed to be greater than 30 seconds per piece; if there is resistance, move the pipe string and establish circulation.
[0082] 1.6. After the casing is in place, install the safety slip, connect the cement head, cementing pipeline and exhaust pipeline, open the floating coupling and exhaust.
[0083] 1.7. Before cementing, start the circulation with a small displacement and establish the circulation, gradually increasing to the designed displacement; if there is leakage, reduce the displacement and plug the leak.
[0084] 1.8. Adjust the drilling fluid properties while ensuring downhole safety to reduce density, viscosity, shear force and yield value; recommended drilling fluid properties: FV≤50, PV≤20, YP≤5.
[0085] 1.9. Circulate the drilling fluid for at least 2 weeks and observe that there is no obvious drilling cuttings on the vibrating screen and the gas measurement value is less than 5%.
[0086] 2. Placement of centralizers: It is planned to install 190 to 200 resin centralizers to ensure the centering of the casing; install rigid centralizers about 3 meters above the float collar and float shoe and fix them with retaining rings; then install a resin centralizer for each casing.
[0087] 3. Start the work:
[0088] 3.1. The cementing pump passes water through the surface pipeline and tests the pressure, with low pressure of 300psi / 5min and high pressure of 3000psi / 15min.
[0089] 3.2. Pump in flushing fluid with the cementing pump.
[0090] 3.3. Mud pump pumps in isolation fluid with a density of 1.10 g / cm 3 , displacement 12bpm.
[0091] 3.4. Pump in flushing fluid with the cementing pump.
[0092] 3.5. Stop the pump and release the bottom plug.
[0093] 3.6. The cementing pump pumps in the slurry mixture and the hydraulic plug.
[0094] 3.7. Use cementing pump to mix the slurry.
[0095] 3.8. Cementing pump mixes the pump tail slurry.
[0096] 3.9. Stop the pump and release the double top plugs. (Pump 1bbls of cement slurry between the two rubber plugs.)
[0097] 3.10. The cementing pump pumps the tailings slurry into the hydraulic plug.
[0098] 3.11. Switch to the mud pump for displacement, fast displacement of 12bpm, slow displacement of the last 100bbls, slow displacement of 2bpm. (The maximum displacement volume does not exceed half of the shoe plug volume.)
[0099] 3.12. Bump pressure: add 500psi to the final displacement pressure and keep the pressure steady for 5 minutes. (Bump pressure is strictly prohibited to prevent empty displacement.) Release the pressure of cementing pump and check the backflow. (If the backflow does not stop, pump in all the backflow and check again. If it still does not work after repeated attempts for 2 times, hold the pressure and wait for solidification.)
[0100] 3.13. Waiting time should be ≥ 24 hours.
[0101] Specifically, this embodiment adopts:
[0102] Additional amount: The additional amount shall not be less than 20% of the electric logging annulus volume; when there is no electric logging wellbore data, the additional amount shall not be less than 50% of the standard annulus volume; no additional amount is required for the overlapping section of casing.
[0103] Flushing fluid formula: 30% PC-W21L + 70% drilling water.
[0104] Return height of cement slurry: the leading slurry returns to the mud line, and the tail slurry returns to 300m above the 9-5 / 8 pipe shoe.
[0105] Prepad fluid: 150bbls flushing fluid + 1200bbls isolation fluid + 60bbls flushing fluid.
[0106] Cement slurry: PC-CorroCEM cement slurry system is used. This system is a special scientific research result and has good CO2 corrosion resistance; the slurry density is 1.50g / cm 3 , tail slurry density 1.90g / cm 3 .
[0107] Displacement: Mud pumps are used to displace seawater throughout the entire process.
[0108] Check reflux: After pressure relief, check reflux. If reflux continues, pump back all the reflux volume. If it fails after repeated attempts twice, hold the pressure and wait for coagulation. The waiting time for coagulation refers to the test formula.
[0109] Thickening time: The thickening time of the slurry should take into account the safe time of wellhead operations.
[0110] The cement slurry formula design is shown in the following table:
[0111]
[0112]
[0113] Step 2: Tail pipe cementing
[0114] 1. Preparation:
[0115] 1.1. Communicate with the tail pipe engineer in advance to confirm the cementing process and key operations.
[0116] 1.2. Determine the size of the tail pipe centralizer.
[0117] 1.3. Before starting cementing operations, reserve samples of cement, mixed water, drilling water, seawater, etc. for cementing.
[0118] 1.4. Lower the tail pipe and add the centralizer in sequence, apply thread glue to the casing buckle below the float hoop, and grout to check the performance of the float valve.
[0119] 1.5. After the casing enters the open hole, control the lowering speed to be greater than 30 seconds per piece; if there is resistance, move the pipe string and establish circulation.
[0120] 1.6. Before cementing, start the circulation with a small displacement and establish the circulation, gradually increasing to the designed displacement; if there is leakage, reduce the displacement and plug the leak.
[0121] 1.7. Adjust the drilling fluid properties while ensuring downhole safety to reduce density, viscosity, shear force and yield value; recommended drilling fluid properties: FV≤50, PV≤20, YP≤5.
[0122] 1.8. Circulate the drilling fluid for at least 2 weeks and observe that there is no obvious drilling cuttings on the vibrating screen and the gas measurement value is less than 5%.
[0123] 2. Placement of centralizer:
[0124] It is planned to install 90 to 100 resin centralizers to ensure the centering of the casing; install rigid centralizers about 3 meters above the stopper, float collar and float shoe and fix them with stop rings; and then install a resin centralizer on each tail pipe.
[0125] 3. Start the work:
[0126] 3.1. Use a batch mixing tank to mix the cement slurry in advance.
[0127] 3.2. The cementing pump passes water through the surface pipeline and tests the pressure, with the low pressure being 300psi / 5min and the high pressure being 4500psi / 15min.
[0128] 3.3. Pump in flushing fluid with the cementing pump.
[0129] 3.4. Mud pump pumps in isolation fluid with a density of 1.10 g / cm 3 , displacement 8bpm.
[0130] 3.5. Pump in flushing fluid with the cementing pump.
[0131] 3.6. The cementing pump pumps in drilling water.
[0132] 3.7. Pump in the slurry with the cementing pump.
[0133] 3.8. The cementing pump pumps in tailings slurry.
[0134] 3.9. Stop the pump and release the shear plug.
[0135] 3.10. The cementing pump pumps into the drilling water pressure plug.
[0136] 3.11. Switch to the mud pump for displacement, with a quick displacement of 8bpm, and a slow displacement of 2bpm for the last 100bbls, and the maximum displacement shall not exceed half of the volume of the shoe plug.
[0137] 3.12. Bump pressure: add 500psi to the final displacement pressure and maintain the pressure steady for 5 minutes. It is strictly forbidden to require bump pressure to prevent empty displacement.
[0138] 3.13. Depressurize the cementing pump and check for backflow. If the backflow does not stop, pump in all the backflow and check again. If it still does not work after repeated attempts for 2 times, directly set the packer.
[0139] 3.14. Set the top packer according to the instructions of the tail pipe engineer, remove the running tool, and circulate and clean the cement slurry.
[0140] 3.15. Waiting time should be ≥ 72 hours.
[0141] Specifically, this embodiment adopts:
[0142] Additional amount: The additional amount shall not be less than 20% of the electric logging annulus volume; when there is no electric logging wellbore data, the additional amount shall not be less than 50% of the standard annulus volume; no additional amount is required for the overlapping section of casing.
[0143] Prepad fluid: 90bbls flushing fluid + 450bbls isolation fluid + 60bbls flushing fluid.
[0144] Isolation fluid formula: drilling water + PC-X60L + PC-G86L + PC-S32S, weighted to 1.10g / cm 3 .
[0145] Flushing fluid formula: 30% PC-W21L + 70% drilling water.
[0146] Return height of cement slurry: the leading slurry returns to 50m above the tail pipe hanger, and the tail slurry returns to 400m above the tail pipe shoe.
[0147] Prepad fluid: 90bbls flushing fluid + 450bbls isolation fluid + 60bbls flushing fluid.
[0148] Cement slurry: Aluminophosphate cement slurry system is used. This system is a special scientific research result and is not affected by CO2 corrosion. In theory, it can achieve permanent sealing of the CO2 reinjection layer; the slurry density is 1.82g / cm 3 , tail slurry density 1.82g / cm 3 .
[0149] Displacement: Mud pumps are used to displace seawater throughout the entire process.
[0150] Check the backflow: After depressurization, check the backflow. If the backflow continues, pump back the entire backflow volume. If it still does not work after repeated attempts for 2 times, directly set the packer.
[0151] Specifically, the cement slurry formula design is shown in the following table:
[0152]
[0153]
[0154] Step 3: Tail pipe back-connection and cementing
[0155] 1. Preparation:
[0156] 1.1. During well drilling, at least 100m of thick slurry should be placed below the tie-back tube.
[0157] 1.2. Lower the return tube scraper to clean the return tube.
[0158] 1.3. Check the integrity of the inserted seal and the number of shear pins of the packer. It is advisable to use double floating collars.
[0159] 1.4. Before starting cementing operations, reserve samples of cement, mixed water, drilling water, seawater, etc. for cementing.
[0160] 1.5. Replace the long hanging card before lowering the main pipe, lower the casing and add the centralizer in sequence, apply thread glue to the casing buckle below the float hoop, and grout to check the performance of the float valve.
[0161] 1.6. The cementing pump is pressure tested on the back-connection seal, specifically at 500psi / 3min and 1000psi / 5min.
[0162] 1.7. After lifting the circulation hole out of the top of the return tube, start the pump to open and confirm the circulation channel, stop the pump, seat the casing slips, and connect the cementing circulation head and cementing pipeline.
[0163] 1.8. Before cementing, start the circulation with a small displacement and establish the circulation, and gradually increase it to the designed displacement.
[0164] 1.9. Thickening time: The thickening time of the slurry should take into account the safe time for the tail pipe to hang the seal and circulate and clean the cement slurry.
[0165] 2. Placement of centralizer: It is planned to install a resin centralizer on each casing to ensure the centering degree of the casing.
[0166] 3. Start the work:
[0167] 3.1. The cementing pump passes water through the surface pipeline and tests the pressure, with low pressure of 300psi / 5min and high pressure of 3000psi / 15min.
[0168] 3.2. Pump in flushing fluid with the cementing pump.
[0169] 3.3. The cementing pump pumps in the slurry mixed water.
[0170] 3.4. Use cementing pump to mix the slurry.
[0171] 3.5. Cementing pump mixes the pump tail slurry.
[0172] 3.6. Quickly remove the circulation head, insert the casing top plug, quickly connect the buckle + insert the casing, and connect the top drive.
[0173] 3.7. Switch to the mud pump for displacement, with a fast displacement of 8bpm, and a slow replacement at the last 20bbls, with a slow replacement displacement of 3bpm, and the maximum displacement volume shall not exceed half of the shoe plug volume.
[0174] 3.8. Bump pressure: add 500psi to the final displacement pressure, maintain the pressure for 5 minutes, and bump pressure is required to prevent empty displacement.
[0175] 3.9. Slowly lower the insert seal into the tie-back tube. When the second seal is inserted into the tie-back tube, release all the pressure inside the casing and keep the ground pressure relief valve open. Continue to lower the insert seal and insert it completely into the tie-back tube, pressing down 5 to 8 klbs.
[0176] 3.10. Check whether the casing mark is consistent with the mark during the first trial insertion. If it is consistent, continue to press down until the designed hanging weight seals the casing packer and hanger, and maintain it for 5 minutes.
[0177] 3.11. Depressurize the cementing pump and check for backflow.
[0178] 3.12. Waiting time should be ≥ 24 hours.
[0179] Specifically, this embodiment adopts:
[0180] Additional amount: The overlapping section of the casing is not additional.
[0181] Return height of cement slurry: the leading slurry returns to the mud line, and the tail slurry returns to 1000m above the return tube.
[0182] Pre-flushing solution: 90bbls flushing solution.
[0183] Cement slurry: PC-CorroCEM cement slurry system is used. This system is a special scientific research result and has good CO2 corrosion resistance; the slurry density is 1.90g / cm 3 , tail slurry density 1.90g / cm 3 .
[0184] Displacement: Mud pumps are used to displace seawater throughout the entire process.
[0185] Check the reflux: After the pressure is released, check the reflux. If the reflux continues, pump back the entire reflux volume. If it still does not work after repeated attempts twice, hold the pressure and wait for coagulation. The waiting time for coagulation refers to the test formula.
[0186] Thickening time: The thickening time of the slurry should take into account the safe time of wellhead operations.
[0187] The pre-fluid is 90bbls flushing fluid;
[0188] Flushing fluid formula: 30% PC-W21L + 70% drilling water.
[0189] Specifically, the cement slurry formula design is shown in the following table:
[0190]
[0192] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention; the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A carbon dioxide reinjection well cementing method, characterized in that: The following steps are involved: S1, casing cementing; S1.
1. Preparation work before cementing; S1.2, pump in cementing fluid; S1.3, switch to mud pump for displacement; S1.4, perform pressure control and testing; S1.5, wait for solidification; S2, liner cementing; S2.1, repeat step S1.1; S2.2, tailing slurry is pumped in to fill the bottom of the wellbore; S2.3, switch to the mud pump for displacement; S2.4, perform pressure control and testing; S2.
5. Set the top packer, remove the running tool, and circulate and clean the cement slurry; S2.6, waiting for solidification; S3, tail pipe back-connection and cementing; S3.
1. Prepare for tie-back cementing work and conduct tie-back sealing test; S3.
2. Remove the mud in the wellbore and make preliminary preparations for cleaning after the surface pipeline pressure test; S3.3, use the cementing pump to mix the lead slurry and cementing fluid evenly, and use the cementing pump to mix the tail slurry and fill the bottom of the wellbore; S3.4, quickly remove the circulation head, put in the casing top plug, quickly connect the buckle and run the casing, and connect the top drive to run the casing into the wellbore; S3.
5. Add additional pressure to the final displacement pressure to meet the design requirements, and then maintain the pressure for 5 minutes to ensure that the casing is safely installed and forms a tight seal with the wellbore wall; S3.
6. Slowly lower the insert seal until it is fully inserted into the tie-back tube. When the second seal is inserted into the tie-back tube, release all the pressure in the casing and keep the ground pressure relief valve open. Continue to lower the insert seal and fully insert it into the tie-back tube while applying a certain downward pressure. S3.
7. Check whether the markings on the casing are consistent with those on the first trial insertion. If they are consistent, continue to press down until the designed hanging weight sets the casing packer and hanger, and maintain for a certain period of time to ensure the correct installation depth and position of the casing, as well as the effectiveness of the hanger and packer; S3.
8. Depressurize the cementing pump and check for backflow. If there is backflow, replace the backflow volume to hold the pressure and wait for solidification to ensure that there is no leakage of cementing fluid in the casing, and then wait for solidification.
2. A carbon dioxide reinjection well cementing method according to claim 1, characterized in that: The step S1.1 specifically includes the following steps: S1.1.
1. Determine the size of the casing centralizer, and run the casing and add the centralizer in sequence; S1.1.
2. Use cementing pump to pump water through the surface pipeline and test the pressure. The pressure should meet the maximum pump pressure required in the cementing method to ensure that the pipeline is firm and usable during the cementing process; S1.1.
3. Use the cementing pump to flush the flushing fluid to flush the impurities out of the wellbore and fully clean the wellbore wall surface.
3. A carbon dioxide reinjection well cementing method according to claim 1, characterized in that: The step S1.2 specifically includes the following steps: S1.2.
1. Stop the cementing pump and open the stopper pin under the cement head to release the bottom rubber plug; S1.2.
2. Use cementing pump to pump in the lead slurry mixed water to pressurize the rubber plug, and the pumped lead slurry mixed water pushes the bottom rubber plug to the bottom of the wellbore, so that the cementing fluid starts to fill the wellbore from the bottom of the casing; S1.2.3, mix the mixed slurry and cementing fluid evenly through the cementing pump; S1.2.
4. Use a cementing pump to mix the tailings slurry and pump the tailings slurry into the wellbore to fill the bottom of the wellbore.
4. A carbon dioxide reinjection well cementing method according to claim 1, characterized in that: The step S1.3 specifically includes the following steps: S1.3.
1. Stop the cementing pump and open the stopper pin on the cement head to release the top rubber plug; S1.3.2, cementing pump pumps tailings slurry into the hydraulic plug; S1.3.
3. Switch to the mud pump for displacement, and in the final stage switch to a small displacement pump.
5. A carbon dioxide reinjection well cementing method according to claim 1, characterized in that: The step S1.4 specifically includes the following steps: S1.4.
1. After reaching the final displacement pressure, add additional pressure to meet the design requirements and maintain the pressure for a certain period of time to ensure the reliability of cementing. At the same time, check whether there is a pressure drop to ensure that there is no leakage of cementing fluid; S1.4.
2. Open the pressure relief valve of the cementing pump and check if there is backflow. If there is backflow, replace the backflow volume and hold the pressure to wait for solidification.
6. A carbon dioxide reinjection well cementing method according to claim 1, characterized in that: The step S2.2 specifically includes the following steps: S2.2.
1. Use a mud pump to pump in the isolation fluid, a cementing pump to pump in the flushing fluid, and a cementing pump to pump in the drilling water; S2.2.2, mix the mixed slurry and cementing fluid evenly through the cementing pump; S2.2.
3. Use a cementing pump to mix the tailings slurry and pump the tailings slurry into the wellbore to fill the bottom of the wellbore.
7. A carbon dioxide reinjection well cementing method according to claim 1, characterized in that: The step S2.3 specifically includes the following steps: S2.3.
1. Stop the cementing pump and open the stopper pin on the cement head to release the top rubber plug; S2.3.2, cementing pump pumps tailings slurry mixed with hydraulic plug; S2.3.
3. Switch to the mud pump for displacement, and in the final stage switch to a small displacement pump.
8. A carbon dioxide reinjection well cementing method according to claim 1, characterized in that: The step S2.4 specifically includes the following steps: S2.4.
1. After reaching the final displacement pressure, add additional pressure to meet the design requirements and maintain the pressure for a certain period of time to ensure the reliability of cementing. At the same time, check whether there is a pressure drop to ensure that there is no leakage of cementing fluid; S2.4.
2. Open the pressure relief valve of the cementing pump and check if there is backflow. If there is backflow, replace the backflow volume and hold the pressure to wait for solidification.
9. A carbon dioxide reinjection well cementing method according to claim 1, characterized in that: The step S3.1 specifically includes the following steps: S3.1.
1. During the well cleaning process, a certain volume of thick slurry is placed below the tie-back tube to fill the bottom of the tie-back tube; S3.1.2 Check the integrity of the inserted seal and packer, including the number of packer shear pins, and use double float collars to ensure the integrity of the inserted seal and packer, and use double float collars correctly to provide effective sealing and isolation; S3.1.
3. Replace the long elevator before running the casing, run the casing and add the centralizer in sequence, apply thread glue to the casing buckle below the float hoop, and grout to check the performance of the float valve; S3.1.
4. The cementing pump performs pressure test on the tie-back seal to test the sealing performance of the tie-back seal and ensure that the sealing system is normal; S3.1.
5. After the circulation hole is raised to the top of the tie-back tube, turn on the cementing pump to confirm that the circulation channel is unobstructed, then stop the cementing pump, install the casing slips, and connect the cementing circulation head and cementing pipeline to establish the circulation channel in preparation for cementing operations.
10. A carbon dioxide reinjection well cementing method according to claim 1, characterized in that: The step S3.2 specifically includes the following steps: S3.2.
1. Before cementing, start to remove the mud in the wellbore by circulating at a small displacement, and gradually increase the displacement to the designed displacement to ensure the wellbore is clean; S3.2.
2. The cementing pump passes water through the surface pipeline and tests the pressure to test the sealing performance of the surface pipeline to ensure that the cementing fluid will not leak; S3.2.
3. Use the cementing pump to pump flushing fluid to clean the wellbore and prepare for the next cementing fluid pumping.
Citation Information
Patent Citations
Drilling liner cementing tool with packer and cementing method
CN111411917A
Offshore horizontal well multistage fracturing pipe column and well cementation and completion integration method
CN116752931A
Tail pipe well cementation tool with packer
CN212428710U
Mechanical Liner Drilling Cementing System
US20120222861A1
Cement placement in a wellbore with loss circulation zone
US20220178224A1