A method for improving the magnetic properties of NdFeB thin-film magnets
NdFeB thin-sheet magnets were prepared through vacuum smelting and magnetron sputtering technology, and combined with pulsed magnetic field and ultrasonic field treatment to form a composite protective film, solving the magnetic properties and corrosion resistance of NdFeB thin-sheet magnets, and achieving efficient magnetic properties Improve and reduce costs.
Patent Information
- Application Number
- CN202411274950.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-12
AI Technical Summary
During use, the magnetic properties of existing neodymium iron boron sheet magnets are affected by the high price of heavy rare earth elements and the corrosion problems of surface micropores, making it difficult to effectively improve magnetic properties and corrosion resistance.
Light rare earth alloys and heavy rare earth alloy belts are prepared by vacuum smelting, pulsed magnetic field and ultrasonic field treatment are applied, magnetron sputtering films are carried out and sintered and tempered heat treatment is carried out. Combined with multi-arc ion coating and electrodeposition technology, a composite protective film is formed to improve the Magnetic properties and corrosion resistance.
The use of heavy rare earth elements is greatly reduced, the coercive force of the neodymium iron boron sheet magnet is improved, and its corrosion resistance is significantly improved through the composite protective film to prevent the magnetic performance from decreasing.
Smart Images

Figure CN118782374B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnetic materials, and in particular to a method for improving the magnetic properties of a NdFeB thin-sheet magnet. Background Art
[0002] NdFeB sheet magnets are a type of sheet-like NdFeB permanent magnet material. As the mainstream permanent magnet material today, NdFeB permanent magnet material is widely used in defense, aerospace, information communication, medical equipment and other fields due to its relatively low price, wide application range and outstanding magnetic properties.
[0003] However, the coercive force of sintered NdFeB magnets composed of only three elements, Nd, Fe and B, is relatively low, generally not exceeding 1200kA / m. At present, there are methods to increase the coercive force of NdFeB magnets by adding heavy rare earth elements such as Tb and Dy to replace Nd, but heavy rare earth elements are expensive. Directly adding Tb and Dy will consume a large amount of heavy rare earth elements, greatly increasing the manufacturing cost of the magnet. In addition, NdFeB permanent magnet materials have defects such as surface micropores in their own composition and sintering process, which makes them easy to be corroded during use, thereby affecting their magnetic properties.
[0004] Therefore, it is necessary to propose a method for improving the magnetic properties of NdFeB thin film magnets which can reduce the amount of heavy rare earth elements and improve the corrosion resistance of the magnets. Summary of the invention
[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for improving the magnetic properties of NdFeB thin film magnets.
[0006] A method for improving the magnetic properties of NdFeB thin-film magnets comprises the following steps:
[0007] S1: Preparation of light rare earth alloy strip by vacuum melting and rapid quenching
[0008] First, titanium dioxide powder, graphite powder and aluminum ingot are used as raw materials to make a master alloy ingot, and then Al powder, Co powder, Al-Ce master alloy, Al-Cu master alloy and master alloy ingot are vacuum melted, and a light rare earth alloy strip is obtained through a rapid quenching strip throwing process;
[0009] S2: Preparation of heavy rare earth alloy ribbons by applying pulsed magnetic field and ultrasonic field
[0010] Al powder, Al-Tb master alloy, Al-Cu master alloy and Al-Ga master alloy are mixed and vacuum-melted, then poured into a mold and subjected to a phase-difference pulse magnetic field and an ultrasonic field to obtain a heavy rare earth alloy ribbon;
[0011] S3: Surface pretreatment of NdFeB thin films
[0012] The surface of the NdFeB thin slice was polished with sandpaper, and then placed in an ultrasonic cleaning machine, and ultrasonically cleaned with nitric acid solution, citric acid solution and deionized water in sequence, and then ultrasonically treated in alcohol for 5-10 minutes, and vacuum dried to obtain a pre-treated thin slice;
[0013] S4: Magnetron sputtering of light rare earth alloy film and heavy rare earth alloy film and sintering
[0014] Sputtering a light rare earth alloy film and a heavy rare earth alloy film on the upper and lower surfaces of the pretreated thin slice in different regions, and then sintering and tempering the thin slice to obtain a heat-treated thin slice;
[0015] S5: Al 70 Ti 30 Composite film deposition using alloy as target
[0016] Al 70 Ti 30 The alloy is used as a target material, and an Al-Ti composite film is deposited on the surface of the heat-treated thin slice by a multi-arc ion coating machine to obtain a coated thin slice;
[0017] S6: Prepare electroplating solution and perform electrodeposition
[0018] Anhydrous aluminum chloride and 1-ethyl-3-methylimidazole chloride are stirred and dissolved, and then anhydrous manganese chloride is added and stirred and dissolved to prepare an electroplating solution. Then, the above-mentioned coated thin sheet is used as a cathode and electrodeposition is carried out in the electroplating solution to obtain a secondary coated NdFeB thin sheet.
[0019] Furthermore, S1 includes the following steps:
[0020] S1.1: Add titanium dioxide powder and graphite powder in a molar ratio of 2-3:1 into a high-speed disperser, disperse at high speed for 20-30 minutes, mix evenly, and seal into an aluminum tube to obtain a filled aluminum tube;
[0021] S1.2: placing the above-mentioned filled aluminum tube in a box furnace, preheating to 400-500°C, and then hot rolling the preheated filled aluminum tube into a sheet with a thickness of 1-2 mm to obtain a precursor;
[0022] S1.3: Place the aluminum ingot in a pit-type resistance furnace, heat it at 700-800°C for 1-2 hours, and then introduce argon gas into the pit-type resistance furnace to exhaust the air;
[0023] S1.4: Keeping the temperature constant, add the above precursor into the pit type resistance furnace while stirring, then continue stirring for 1-2 hours, and then cast to obtain the master alloy ingot;
[0024] S1.5: Add Al powder, Co powder, Al-Ce master alloy and Al-Cu master alloy into a vacuum arc melting furnace and melt for 30-40 minutes to obtain a light rare earth alloy melt;
[0025] S1.6: adding the above master alloy ingot into the above light rare earth alloy melt, repeatedly smelting 4-5 times, and uniformly mixing to obtain a composite light rare earth alloy ingot;
[0026] S1.7: The composite light rare earth alloy ingot is thrown into a strip shape at a speed of 6-8 m / s by a vacuum rapid quenching strip throwing device to obtain a light rare earth alloy strip.
[0027] Further, S2 includes the following steps:
[0028] S2.1: Add Al powder, Al-Tb master alloy, Al-Cu master alloy and Al-Ga master alloy into a vacuum arc melting furnace and melt for 1-2 hours to obtain a heavy rare earth alloy melt;
[0029] S2.2: pour the heavy rare earth alloy melt into a mold of a melt pulse magnetic field treatment device, then turn on a pulse power supply, apply a phase-difference pulse magnetic field with a pulse voltage of 180-200V and a pulse frequency of 5-15Hz to the heavy rare earth alloy melt, and treat for 20-30min;
[0030] S2.3: A dual-frequency ultrasonic field device is used to apply a 15-20kHz ultrasonic field to the mold. After ultrasonic field treatment for 10-20 minutes, the pulse power supply is turned on again, and a phase-difference pulse magnetic field and an ultrasonic field are applied simultaneously. The treatment is continued for 1-2 hours to obtain a heavy rare earth alloy strip.
[0031] Further, S4 includes the following steps:
[0032] S4.1: installing the pretreated thin slice obtained in step S3 in a magnetron sputtering apparatus, and then installing the light rare earth alloy strip obtained in step S1.7 on a target base, and then sputtering circular light rare earth alloy films on the upper and lower surfaces of the pretreated thin slice respectively by dual-target co-sputtering;
[0033] S4.2: replacing the light rare earth alloy strip on the target base with the heavy rare earth alloy strip obtained in step S2.3, and then sputtering a heavy rare earth alloy film on the unsputtered light rare earth alloy film areas on the upper and lower surfaces of the pretreated wafer respectively by dual-target co-sputtering to obtain a film-attached wafer;
[0034] S4.3: placing the film-attached sheet in a vacuum sintering furnace, sintering at a temperature of 850-950° C. for 3-4 hours, and cooling to room temperature in the furnace to obtain a sintered sheet;
[0035] S4.4: placing the sintered slice in a tempering furnace, tempering at a temperature of 480-500° C. for 5-6 hours, and performing heat treatment to obtain a heat-treated slice.
[0036] Further, S5 includes the following steps:
[0037] S5.1: Al 70 Ti 30 The alloy is fixed on the target holder of the multi-arc ion coating machine, and the oxygen flow rate is set to 120-130 mL / min, the nitrogen flow rate is set to 700-800 mL / min, the substrate negative bias voltage is set to 80-90 V, and the target current is set to 85-95 A;
[0038] S5.2: At a temperature of 400-500° C., an Al-Ti composite film is deposited on the surface of the heat-treated thin slice obtained in step S4.4 by a multi-arc ion plating machine. After deposition for 2-3 hours, a coated thin slice is obtained.
[0039] Further, S6 includes the following steps:
[0040] S6.1: Add anhydrous aluminum chloride and 1-ethyl-3-methylimidazole chloride into a reaction box at a molar ratio of 2-3:1, and stir at a rate of 200-300 r / min until completely dissolved;
[0041] S6.2: Keeping the stirring rate constant, add anhydrous manganese chloride in an amount equal to the molar amount of anhydrous aluminum chloride to the reaction box, and stir until it is completely dissolved to obtain an electroplating solution;
[0042] S6.3: Using the coated thin sheet obtained in step S5.2 as a cathode and the spiral aluminum wire as an anode, electroplating is performed in the above-mentioned electroplating solution to obtain a secondary coated NdFeB thin sheet.
[0043] Furthermore, the molar ratio of graphite to aluminum is 2-3:1, and the light rare earth alloy melt, by atomic number, comprises: 30-40% Co, 20-30% Cu, 10-20% Ce, and the balance is Al.
[0044] Furthermore, the heavy rare earth alloy strip comprises, by atomic number, 40-50% Tb, 10-20% Ga, 5-10% Cu, and the remainder Al.
[0045] Furthermore, the area of the circular light rare earth alloy film region is the maximum circular region that can be made with the center of the NdFeB thin film magnet as the center of the circle.
[0046] Furthermore, the deposition current density of the electrodeposition is 4-6 mA / cm 2 , the deposition time is 10-16min.
[0047] Compared with the prior art, the present invention has at least the following beneficial effects:
[0048] 1. The present invention magnetron sputters light rare earth alloy film and heavy rare earth alloy film in different regions on the surface of pretreated NdFeB thin slices, and after sintering, diffusion and tempering heat treatment, the heavy rare earth alloy and light rare earth alloy penetrate into the interior of the magnet, which not only greatly reduces the amount of heavy rare earth elements, but also effectively improves the coercive force of the NdFeB thin slice magnet, and then coats the surface of the heat-treated thin slice twice in succession to improve the corrosion resistance of the NdFeB thin slice and prevent the reduction of magnetic properties of the NdFeB thin slice due to corrosion.
[0049] 2. The present invention disperses and mixes titanium dioxide powder and graphite powder in proportion at high speed, seals them in an aluminum tube, preheats and hot-rolls, and then mixes and smelts them with the melt of the aluminum ingot to make an intermediate alloy ingot, and then mixes and smelts the ingot with a light rare earth alloy melt melted from aluminum powder, cobalt powder and Al-Ce intermediate alloy, and quickly quenches and spins the ingot, which can effectively reduce the grain size of the light rare earth alloy, thereby improving the diffusion efficiency of the light rare earth alloy, and achieving the effect of further improving the coercive force of the NdFeB thin film magnet.
[0050] 3. The present invention mixes aluminum powder, Al-Tb master alloy, Al-Cu master alloy and Al-Ga master alloy and melts them into a melt by vacuum melting, and then pours the melt into a mold. During the natural cooling of the melt, a phase-difference pulse magnetic field is first applied, an ultrasonic field is applied, and then a phase-difference pulse magnetic field and an ultrasonic field are simultaneously applied, so that the grain size of the obtained heavy rare earth alloy can be reduced, more heavy rare earth alloy can be infiltrated into the NdFeB thin sheet, thereby further improving the coercive force of the NdFeB thin sheet magnet.
[0051] 4. The present invention prepares an electroplating solution using anhydrous aluminum chloride, anhydrous manganese chloride and 1-ethyl-3-methylimidazole chloride as raw materials, and then electrodeposit a Mn-Al composite protective film on the surface of the NdFeB thin-film magnet in the electroplating solution, thereby effectively improving the corrosion resistance of the NdFeB thin-film magnet and preventing the magnetic properties from being reduced due to surface corrosion.
[0052] 5. The present invention deposits an Al-Ti composite protective film on the surface of the heat-treated thin slice by using a multi-arc ion plating machine before electroplating the Mn-Al composite protective film. This can not only further improve the corrosion resistance of the NdFeB thin slice magnet, but also prevent secondary corrosion caused by the residual plating solution in the micropores on the surface of the NdFeB magnet during the electroplating deposition process. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.
[0054] Figure 1 The present invention is a flowchart of a method for improving the magnetic properties of NdFeB thin-film magnets used in an embodiment of the present invention. DETAILED DESCRIPTION
[0055] A method for improving the magnetic properties of NdFeB thin-film magnets provided by the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0056] Example 1
[0057] A method for improving the magnetic properties of NdFeB thin-film magnets, such as Figure 1 As shown, the following steps are included:
[0058] S1: Preparation of light rare earth alloy strip by vacuum melting and rapid quenching
[0059] Titanium dioxide powder and graphite powder are added to a high-speed disperser in a molar ratio of 2:1, dispersed at high speed for 20 minutes, and evenly mixed, and then sealed in an aluminum tube to obtain a filled aluminum tube. The filled aluminum tube is then placed in a box furnace and preheated to 400°C. The preheated filled aluminum tube is rolled into a sheet with a thickness of 1 mm using a hot rolling process to obtain a precursor. Subsequently, the aluminum ingot is placed in a pit-type resistance furnace and heated at 700°C for 1 hour. Argon gas is introduced into the pit-type resistance furnace to exhaust the air, and then the temperature is maintained constant. The precursor is added to the pit-type resistance furnace while stirring, and then continued to stir for 1 hour, and then cast to obtain an intermediate alloy ingot for standby use. , wherein the molar ratio of graphite to aluminum is 2:1, then, Al powder, Co powder, Al-Ce master alloy and Al-Cu master alloy are added into a vacuum arc melting furnace, smelted for 30 minutes, and a light rare earth alloy melt is obtained, wherein, by atomic number, the light rare earth alloy melt comprises: 30% Co, 20% Cu, 10% Ce, and the balance is Al, and then the master alloy ingot is added into the above light rare earth alloy melt, smelted repeatedly for 4 times, and uniformly mixed to obtain a composite light rare earth alloy ingot, and finally, the composite light rare earth alloy ingot is thrown into a strip at a speed of 6 m / s by a vacuum rapid quenching strip throwing device to obtain a light rare earth alloy strip;
[0060] S2: Preparation of heavy rare earth alloy ribbons by applying pulsed magnetic field and ultrasonic field
[0061] Al powder, Al-Tb master alloy, Al-Cu master alloy and Al-Ga master alloy are added into a vacuum arc melting furnace and melted for 1 hour to obtain a heavy rare earth alloy melt, and then the heavy rare earth alloy melt is poured into a mold of a melt pulse magnetic field treatment device, and then a pulse power supply is turned on to apply a phase-difference pulse magnetic field with a pulse voltage of 180V and a pulse frequency of 5Hz to the heavy rare earth alloy melt for 20 minutes, and then a dual-frequency ultrasonic field device is used to apply an ultrasonic field of 15kHz to the mold. After the ultrasonic field treatment for 10 minutes, the pulse power supply is turned on again, and the phase-difference pulse magnetic field and the ultrasonic field are applied simultaneously for 1 hour to obtain a heavy rare earth alloy strip, wherein the heavy rare earth alloy strip includes, by atomic number, 40% Tb, 10% Ga, 5% Cu, and the remainder is Al;
[0062] S3: Surface pretreatment of NdFeB thin films
[0063] The surface of the NdFeB thin slice was polished with sandpaper, and then placed in an ultrasonic cleaning machine, and ultrasonically cleaned with nitric acid solution, citric acid solution and deionized water in sequence, and then ultrasonically treated in alcohol for 5 minutes, and vacuum dried to obtain a pretreated thin slice;
[0064] S4: Magnetron sputtering of light rare earth alloy film and heavy rare earth alloy film and sintering
[0065] The above-mentioned pretreated thin slice is installed in a magnetron sputtering apparatus, and then the above-mentioned light rare earth alloy belt is installed on a target base, and then circular light rare earth alloy films are respectively sputtered on the upper and lower surfaces of the pretreated thin slice by double-target co-sputtering, wherein the area of the circular light rare earth alloy film region is a circular region with the largest area that can be made with the center of the NdFeB thin slice magnet as the center of the circle, and then the light rare earth alloy belt on the target base is replaced with the above-mentioned heavy rare earth alloy belt, and then heavy rare earth alloy films are respectively sputtered on the unsputtered light rare earth alloy film regions on the upper and lower surfaces of the pretreated thin slice by double-target co-sputtering to obtain a film-attached thin slice, and then the film-attached thin slice is placed in a vacuum sintering furnace, sintered at a temperature of 850°C for 3h, and cooled to room temperature with the furnace to obtain a sintered thin slice, and finally, the sintered thin slice is placed in a tempering furnace, tempered at a temperature of 480°C for 5h, and heat treated to obtain a heat-treated thin slice;
[0066] S5: Al 70 Ti 30 Composite film deposition using alloy as target
[0067] Al 70 Ti 30The alloy was fixed on the target holder of a multi-arc ion plating machine, and the oxygen flow rate was set to 120 mL / min, the nitrogen flow rate was set to 700 mL / min, the substrate negative bias voltage was set to 80 V, and the target current was set to 85 A. Then, at a temperature of 400° C., an Al-Ti composite film was deposited on the surface of the above-mentioned heat-treated thin slice by a multi-arc ion plating machine. After deposition for 2 hours, a coated thin slice was obtained;
[0068] S6: Prepare electroplating solution and perform electrodeposition
[0069] Anhydrous aluminum chloride and 1-ethyl-3-methylimidazole chloride are added to a reaction box in a molar ratio of 2:1, and stirred at a rate of 200 r / min until they are completely dissolved. Then, anhydrous manganese chloride in an amount equal to that of anhydrous aluminum chloride is added to the reaction box while maintaining the stirring rate unchanged, and stirred until they are completely dissolved to obtain an electroplating solution. Finally, the above-mentioned coated sheet is used as a cathode and the spiral aluminum wire is used as an anode to perform electrodeposition in the electroplating solution to obtain a secondary coated NdFeB sheet, wherein the deposition current density of the electrodeposition is 4 mA / cm 2 , the deposition time is 10min.
[0070] Performance Test:
[0071] Firstly, the coercivity of the secondary coated NdFeB thin film was measured by using NIM-10000HC magnetometer;
[0072] Then, a sodium chloride solution with a mass fraction of 3.5% was selected as the corrosion medium, and the full immersion test method was used to test the first corrosion time of the coating and the first corrosion time of the substrate of the secondary coated NdFeB thin film. The experimental temperature was 25°C. The results are shown in Table 1 below.
[0073] Example 2
[0074] A method for improving the magnetic properties of NdFeB thin-film magnets, such as Figure 1 As shown, the following steps are included:
[0075] S1: Preparation of light rare earth alloy strip by vacuum melting and rapid quenching
[0076] Titanium dioxide powder and graphite powder are added to a high-speed disperser at a molar ratio of 2.5:1, dispersed at high speed for 25 minutes, and evenly mixed, and then sealed in an aluminum tube to obtain a filled aluminum tube. The filled aluminum tube is then placed in a box furnace and preheated to 450°C. The preheated filled aluminum tube is rolled into a sheet with a thickness of 1.5 mm using a hot rolling process to obtain a precursor. Subsequently, the aluminum ingot is placed in a pit-type resistance furnace, heated at 750°C for 1.5 hours, argon gas is introduced into the pit-type resistance furnace to exhaust the air, and then the temperature is maintained constant. The precursor is added to the pit-type resistance furnace while stirring, and then stirring is continued for 1.5 hours, and then casting is performed to obtain an intermediate alloy ingot. , standby, wherein the molar ratio of graphite to aluminum is 2.5:1, then, Al powder, Co powder, Al-Ce master alloy and Al-Cu master alloy are added to a vacuum arc melting furnace, smelted for 35 minutes, and a light rare earth alloy melt is obtained, wherein, by atomic number, the light rare earth alloy melt includes: 35% Co, 25% Cu, 15% Ce, and the balance is Al, and then the master alloy ingot is added to the above light rare earth alloy melt, and the smelting is repeated 4 times, and the mixture is evenly mixed to obtain a composite light rare earth alloy ingot, and finally, the composite light rare earth alloy ingot is thrown into a strip at a speed of 7m / s by a vacuum rapid quenching strip throwing device to obtain a light rare earth alloy strip;
[0077] S2: Preparation of heavy rare earth alloy ribbons by applying pulsed magnetic field and ultrasonic field
[0078] Al powder, Al-Tb master alloy, Al-Cu master alloy and Al-Ga master alloy are added into a vacuum arc melting furnace and smelted for 1.5 hours to obtain a heavy rare earth alloy melt, and then the heavy rare earth alloy melt is poured into a mold of a melt pulse magnetic field treatment device, and then a pulse power supply is turned on to apply a phase-difference pulse magnetic field with a pulse voltage of 190V and a pulse frequency of 10Hz to the heavy rare earth alloy melt for 25 minutes, and then a dual-frequency ultrasonic field device is used to apply an ultrasonic field of 18kHz to the mold. After the ultrasonic field treatment for 15 minutes, the pulse power supply is turned on again, and the phase-difference pulse magnetic field and the ultrasonic field are applied simultaneously for 1.5 hours to obtain a heavy rare earth alloy strip, wherein the heavy rare earth alloy strip includes, by atomic number, 45% Tb, 15% Ga, 8% Cu, and the remainder is Al;
[0079] S3: Surface pretreatment of NdFeB thin films
[0080] The surface of the NdFeB thin slice was polished with sandpaper, and then placed in an ultrasonic cleaning machine, and ultrasonically cleaned with nitric acid solution, citric acid solution and deionized water in sequence, and then ultrasonically treated in alcohol for 8 minutes, and vacuum dried to obtain a pre-treated thin slice;
[0081] S4: Magnetron sputtering of light rare earth alloy film and heavy rare earth alloy film and sintering
[0082] The above-mentioned pretreated thin slice is installed in a magnetron sputtering apparatus, and then the above-mentioned light rare earth alloy belt is installed on a target base, and then circular light rare earth alloy films are respectively sputtered on the upper and lower surfaces of the pretreated thin slice by double-target co-sputtering, wherein the area of the circular light rare earth alloy film region is the largest circular region that can be made with the center of the NdFeB thin slice magnet as the center of the circle, and then, the light rare earth alloy belt on the target base is replaced with the above-mentioned heavy rare earth alloy belt, and then, by double-target co-sputtering, a heavy rare earth alloy film is respectively sputtered on the unsputtered light rare earth alloy film regions on the upper and lower surfaces of the pretreated thin slice to obtain a film-attached thin slice, and then the film-attached thin slice is placed in a vacuum sintering furnace, sintered at a temperature of 800°C for 3.5 hours, and cooled to room temperature with the furnace to obtain a sintered thin slice, and finally, the sintered thin slice is placed in a tempering furnace, tempered at a temperature of 490°C for 5.5 hours, and heat-treated to obtain a heat-treated thin slice;
[0083] S5: Al 70 Ti 30 Composite film deposition using alloy as target
[0084] Al 70 Ti 30 The alloy was fixed on the target holder of a multi-arc ion plating machine, and the oxygen flow rate was set to 125 mL / min, the nitrogen flow rate was set to 750 mL / min, the substrate negative bias voltage was set to 85 V, and the target current was set to 90 A. Then, at a temperature of 450° C., an Al-Ti composite film was deposited on the surface of the above-mentioned heat-treated thin slice by a multi-arc ion plating machine. After deposition for 2.5 hours, a coated thin slice was obtained;
[0085] S6: Prepare electroplating solution and perform electrodeposition
[0086] Anhydrous aluminum chloride and 1-ethyl-3-methylimidazole chloride are added to a reaction box at a molar ratio of 2.5:1, and stirred at a rate of 250 r / min until they are completely dissolved. Then, anhydrous manganese chloride in an amount equal to that of anhydrous aluminum chloride is added to the reaction box while maintaining the stirring rate unchanged, and stirred until they are completely dissolved to obtain an electroplating solution. Finally, the above-mentioned coated sheet is used as a cathode and the spiral aluminum wire is used as an anode to perform electrodeposition in the electroplating solution to obtain a secondary coated NdFeB sheet, wherein the deposition current density of the electrodeposition is 5 mA / cm 2 , the deposition time is 13min.
[0087] Performance Test:
[0088] Firstly, the coercivity of the secondary coated NdFeB thin film was measured by using NIM-10000HC magnetometer;
[0089] Then, a sodium chloride solution with a mass fraction of 3.5% was selected as the corrosion medium, and the full immersion test method was used to test the first corrosion time of the coating and the first corrosion time of the substrate of the secondary coated NdFeB thin film. The experimental temperature was 25°C. The results are shown in Table 1 below.
[0090] Example 3
[0091] A method for improving the magnetic properties of NdFeB thin-film magnets, such as Figure 1 As shown, the following steps are included:
[0092] S1: Preparation of light rare earth alloy strip by vacuum melting and rapid quenching
[0093] Titanium dioxide powder and graphite powder are added to a high-speed disperser in a molar ratio of 3:1, dispersed at high speed for 30 minutes, and evenly mixed, and then sealed in an aluminum tube to obtain a filled aluminum tube. The filled aluminum tube is then placed in a box furnace and preheated to 500°C. The preheated filled aluminum tube is rolled into a sheet with a thickness of 2 mm using a hot rolling process to obtain a precursor. Subsequently, the aluminum ingot is placed in a pit-type resistance furnace and heated at 800°C for 2 hours. Argon is introduced into the pit-type resistance furnace to exhaust the air, and then the temperature is maintained constant. The precursor is added to the pit-type resistance furnace while stirring, and then stirring is continued for 2 hours, and then casting is performed to obtain an intermediate alloy ingot for standby use. , wherein the molar ratio of graphite to aluminum is 3:1, then, Al powder, Co powder, Al-Ce master alloy and Al-Cu master alloy are added into a vacuum arc melting furnace, smelted for 40 minutes, and a light rare earth alloy melt is obtained, wherein, by atomic number, the light rare earth alloy melt comprises: 40% Co, 30% Cu, 20% Ce, and the balance is Al, and then the master alloy ingot is added into the above light rare earth alloy melt, smelted repeatedly for 5 times, and uniformly mixed to obtain a composite light rare earth alloy ingot, and finally, the composite light rare earth alloy ingot is thrown into a strip at a speed of 8m / s by a vacuum rapid quenching strip throwing device to obtain a light rare earth alloy strip;
[0094] S2: Preparation of heavy rare earth alloy ribbons by applying pulsed magnetic field and ultrasonic field
[0095] Al powder, Al-Tb master alloy, Al-Cu master alloy and Al-Ga master alloy are added into a vacuum arc melting furnace and smelted for 2 hours to obtain a heavy rare earth alloy melt, and then the heavy rare earth alloy melt is poured into a mold of a melt pulse magnetic field treatment device, and then a pulse power supply is turned on to apply a phase-difference pulse magnetic field with a pulse voltage of 200V and a pulse frequency of 15Hz to the heavy rare earth alloy melt for 30 minutes, and then a dual-frequency ultrasonic field device is used to apply a 20kHz ultrasonic field to the mold. After the ultrasonic field treatment for 20 minutes, the pulse power supply is turned on again, and the phase-difference pulse magnetic field and the ultrasonic field are applied simultaneously for 2 hours to obtain a heavy rare earth alloy strip, wherein the heavy rare earth alloy strip includes, by atomic number, 50% Tb, 20% Ga, 10% Cu, and the remainder is Al;
[0096] S3: Surface pretreatment of NdFeB thin films
[0097] The surface of the NdFeB thin slice was polished with sandpaper, and then placed in an ultrasonic cleaning machine, and ultrasonically cleaned with nitric acid solution, citric acid solution and deionized water in sequence, and then ultrasonically treated in alcohol for 10 minutes, and vacuum dried to obtain a pre-treated thin slice;
[0098] S4: Magnetron sputtering of light rare earth alloy film and heavy rare earth alloy film and sintering
[0099] The above-mentioned pretreated thin slice is installed in a magnetron sputtering apparatus, and then the above-mentioned light rare earth alloy belt is installed on a target base, and then circular light rare earth alloy films are respectively sputtered on the upper and lower surfaces of the pretreated thin slice by double-target co-sputtering, wherein the area of the circular light rare earth alloy film region is a circular region with the largest area that can be made with the center of the NdFeB thin slice magnet as the center of the circle, and then, the light rare earth alloy belt on the target base is replaced with the above-mentioned heavy rare earth alloy belt, and then, by double-target co-sputtering, a heavy rare earth alloy film is respectively sputtered on the unsputtered light rare earth alloy film regions on the upper and lower surfaces of the pretreated thin slice to obtain a film-attached thin slice, and then the film-attached thin slice is placed in a vacuum sintering furnace, sintered at a temperature of 950°C for 4h, and cooled to room temperature with the furnace to obtain a sintered thin slice, and finally, the sintered thin slice is placed in a tempering furnace, tempered at a temperature of 500°C for 6h, and heat treated to obtain a heat-treated thin slice;
[0100] S5: Al 70 Ti 30 Composite film deposition using alloy as target
[0101] Al 70 Ti 30The alloy was fixed on the target holder of a multi-arc ion plating machine, and the oxygen flow rate was set to 130 mL / min, the nitrogen flow rate was set to 800 mL / min, the substrate negative bias voltage was set to 90 V, and the target current was set to 95 A. Then, at a temperature of 500° C., an Al-Ti composite film was deposited on the surface of the above-mentioned heat-treated thin slice by a multi-arc ion plating machine. After deposition for 3 hours, a coated thin slice was obtained;
[0102] S6: Prepare electroplating solution and perform electrodeposition
[0103] Anhydrous aluminum chloride and 1-ethyl-3-methylimidazole chloride are added to a reaction box in a molar ratio of 3:1, and stirred at a rate of 300 r / min until they are completely dissolved. Then, anhydrous manganese chloride in an amount equal to that of anhydrous aluminum chloride is added to the reaction box while maintaining the stirring rate unchanged, and stirred until they are completely dissolved to obtain an electroplating solution. Finally, the above-mentioned coated sheet is used as a cathode and the spiral aluminum wire is used as an anode to perform electrodeposition in the electroplating solution to obtain a secondary coated NdFeB sheet, wherein the deposition current density of the electrodeposition is 6 mA / cm 2 , the deposition time is 16min.
[0104] Performance Test:
[0105] Firstly, the coercivity of the secondary coated NdFeB thin film was measured by using NIM-10000HC magnetometer;
[0106] Then, a sodium chloride solution with a mass fraction of 3.5% was selected as the corrosion medium, and the full immersion test method was used to test the first corrosion time of the coating and the first corrosion time of the substrate of the secondary coated NdFeB thin film. The experimental temperature was 25°C. The results are shown in Table 1 below.
[0107] Table 1: Coercivity and corrosion time results of the secondary coated NdFeB thin film of Example 1
[0108] Performance Indicators Coercivity (kOe) First corrosion time of coating (h) First corrosion time of substrate (h) Example 1 19.4 298 >800 Example 2 19.4 297 >800 Example 3 19.5 298 >800
[0109] Comparative Example 1
[0110] The coercivity, first corrosion time of the coating and first corrosion time of the substrate of the same batch of NdFeB sheets as those in step S3 of Example 1 were tested according to the performance testing method of Example 1. The results are shown in Table 2 below.
[0111] Table 2: Comparison of coercivity and corrosion time of the secondary coated NdFeB sheets of Example 1 and Comparative Example 1
[0112] Performance Indicators Coercivity (kOe) First corrosion time of coating (h) First corrosion time of substrate (h) Example 1 19.4 298 >800 Comparative Example 1 12.7 64 76
[0113] By comparing the performance test results of Example 1 with those of Comparative Example 1, it can be seen that by magnetron sputtering light rare earth alloy films and heavy rare earth alloy films on the surface of the pretreated NdFeB thin film in different regions, after sintering, diffusion and tempering heat treatment, the heavy rare earth alloy and light rare earth alloy penetrate into the interior of the magnet, which not only greatly reduces the amount of heavy rare earth elements used, but also effectively improves the coercive force of the NdFeB thin film magnet. Then, the heat-treated thin film surface is coated twice in succession to improve the corrosion resistance of the NdFeB thin film and prevent the reduction of magnetic properties of the NdFeB thin film due to corrosion.
[0114] Comparative Example 2
[0115] The difference between this comparative example 2 and example 1 is that the step of preparing the intermediate alloy ingot in step S1 is removed, that is, the intermediate alloy ingot is not added to the light rare earth alloy melt, and the light rare earth alloy strip is directly prepared. Then, the coercive force of the obtained secondary coated NdFeB thin film is tested with reference to the performance test method in example 1, and the results are shown in Table 3 below.
[0116] Table 3: Comparison of coercivity and corrosion time of the secondary coated NdFeB sheets of Example 1 and Comparative Example 2
[0117] Performance Indicators Coercivity (kOe) Example 1 19.4 Comparative Example 2 17.5
[0118] By comparing the performance test results of Example 1 and Comparative Example 2, it can be seen that by dispersing and mixing titanium dioxide powder and graphite powder in proportion at high speed, sealing them in an aluminum tube, preheating and hot rolling, and then smelting them with the melt after the aluminum ingot is melted to make an intermediate alloy ingot, and then smelting them with a light rare earth alloy melt melted by aluminum powder, cobalt powder and Al-Ce intermediate alloy, and rapidly quenching and strip spinning, the grain size of the light rare earth alloy can be effectively reduced, thereby improving the diffusion efficiency of the light rare earth alloy, thereby achieving the effect of further improving the coercive force of the NdFeB thin film magnet.
[0119] Comparative Example 3
[0120] The difference between this comparative example 3 and example 1 is that the phase-difference pulse magnetic field treatment and the ultrasonic field treatment in step S2 are removed, that is, the heavy rare earth alloy melt is naturally cooled without applying any external factors, and then the coercive force of the obtained secondary coated NdFeB thin film is tested with reference to the performance test method in example 1, and the results are shown in Table 4 below.
[0121] Table 4: Comparison of coercivity and corrosion time of the secondary coated NdFeB sheets of Example 1 and Comparative Example 3
[0122] Performance Indicators Coercivity (kOe) Example 1 19.4 Comparative Example 3 18.1
[0123] By comparing the performance test results of Example 1 with those of Comparative Example 3, it can be seen that by mixing aluminum powder, Al-Tb master alloy, Al-Cu master alloy and Al-Ga master alloy and vacuum melting them into a melt, and then pouring the melt into a mold, during the natural cooling of the melt, by first applying a phase-difference pulse magnetic field, then applying an ultrasonic field, and then simultaneously applying a phase-difference pulse magnetic field and an ultrasonic field, the grain size of the obtained heavy rare earth alloy can be reduced, and more heavy rare earth alloy can be infiltrated into the NdFeB sheet, thereby further improving the coercive force of the NdFeB sheet magnet.
[0124] Comparative Example 4
[0125] The difference between this comparative example 4 and example 1 is that step S6 is removed, and then the first corrosion time of the coating and the first corrosion time of the substrate of the prepared coated NdFeB thin film are tested by referring to the performance test method in example 1, and the results are shown in Table 5 below.
[0126] Table 5: Comparison of coercivity and corrosion time of the secondary coated NdFeB sheets of Example 1 and Comparative Example 4
[0127] Performance Indicators First corrosion time of coating (h) First corrosion time of substrate (h) Example 1 298 >800 Comparative Example 4 153 650
[0128] By comparing the performance test results of Example 1 with those of Comparative Example 4, it can be seen that by preparing an electroplating solution with anhydrous aluminum chloride, anhydrous manganese chloride and 1-ethyl-3-methylimidazole chloride as raw materials, and then electrodepositing a Mn-Al composite protective film on the surface of the NdFeB thin film magnet in the electroplating solution, the corrosion resistance of the NdFeB thin film magnet can be effectively improved, and the magnetic properties can be prevented from being reduced due to surface corrosion.
[0129] Comparative Example 5
[0130] The difference between this comparative example 5 and example 1 is that step S5 is removed, that is, electrodeposition is directly performed on the surface of the heat-treated thin sheet, and then the first corrosion time of the coating and the first corrosion time of the substrate of the prepared coated NdFeB thin sheet are tested with reference to the performance test method in example 1, and the results are shown in Table 6 below.
[0131] Table 6: Comparison of coercivity and corrosion time of the secondary coated NdFeB sheets of Example 1 and Comparative Example 5
[0132] Performance Indicators First corrosion time of coating (h) First corrosion time of substrate (h) Example 1 298 >800 Comparative Example 5 297 18
[0133] By comparing the performance test results of Example 1 with those of Comparative Example 5, it can be seen that by first using a multi-arc ion plating machine to deposit an Al-Ti composite protective film on the surface of the heat-treated thin slice before electro-depositing the Mn-Al composite protective film, it can not only further improve the corrosion resistance of the NdFeB thin slice magnet, but also prevent secondary corrosion caused by the residual plating solution in the micropores on the surface of the NdFeB magnet during the electroplating deposition process.
[0134] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for improving the magnetic properties of NdFeB thin-film magnets, characterized in that: The steps include: S1: Preparation of light rare earth alloy strip by vacuum melting and rapid quenching First, titanium dioxide powder, graphite powder and aluminum ingot are used as raw materials to make a master alloy ingot, and then Al powder, Co powder, Al-Ce master alloy, Al-Cu master alloy and master alloy ingot are vacuum melted, and a light rare earth alloy strip is obtained through a rapid quenching strip throwing process; S2: Preparation of heavy rare earth alloy ribbons by applying pulsed magnetic field and ultrasonic field Al powder, Al-Tb master alloy, Al-Cu master alloy and Al-Ga master alloy are mixed and vacuum-melted, then poured into a mold and subjected to a phase-difference pulse magnetic field and an ultrasonic field to obtain a heavy rare earth alloy ribbon; S3: Surface pretreatment of NdFeB thin films The surface of the NdFeB thin slice was polished with sandpaper, and then placed in an ultrasonic cleaning machine, and ultrasonically cleaned with nitric acid solution, citric acid solution and deionized water in sequence, and then ultrasonically treated in alcohol for 5-10 minutes, and vacuum dried to obtain a pre-treated thin slice; S4: Magnetron sputtering of light rare earth alloy film and heavy rare earth alloy film and sintering Sputtering a light rare earth alloy film and a heavy rare earth alloy film on the upper and lower surfaces of the pretreated thin slice in different regions, and then sintering and tempering the thin slice to obtain a heat-treated thin slice; S5: Al 70 Ti 30 Composite film deposition using alloy as target Al 70 Ti 30 The alloy is used as a target material, and an Al-Ti composite film is deposited on the surface of the heat-treated thin slice by a multi-arc ion coating machine to obtain a coated thin slice; S6: Prepare electroplating solution and perform electrodeposition Anhydrous aluminum chloride and 1-ethyl-3-methylimidazole chloride are stirred and dissolved, and then anhydrous manganese chloride is added, and the stirring and dissolving are continued to prepare an electroplating solution, and then the above-mentioned coated thin sheet is used as a cathode to perform electrodeposition in the electroplating solution to obtain a secondary coated NdFeB thin sheet; S4 includes the following steps: S4.1: installing the pretreated thin sheet obtained in step S3 in a magnetron sputtering apparatus, and then installing the light rare earth alloy strip obtained in step S1 on a target base, and then sputtering circular light rare earth alloy films on the upper and lower surfaces of the pretreated thin sheet respectively by dual-target co-sputtering; S4.2: replacing the light rare earth alloy strip on the target base with the heavy rare earth alloy strip obtained in step S2, and then sputtering a heavy rare earth alloy film on the upper and lower surfaces of the pretreated wafer without the light rare earth alloy film by a dual-target co-sputtering method, respectively, to obtain a film-attached wafer; S4.3: placing the film-attached sheet in a vacuum sintering furnace, sintering at a temperature of 850-950° C. for 3-4 hours, and cooling to room temperature in the furnace to obtain a sintered sheet; S4.4: placing the sintered sheet in a tempering furnace and tempering at a temperature of 480-500° C. for 5-6 hours to obtain a heat-treated sheet; S5 includes the following steps: S5.1: Al 70 Ti 30 The alloy is fixed on the target holder of the multi-arc ion coating machine, and the oxygen flow rate is set to 120-130 mL / min, the nitrogen flow rate is set to 700-800 mL / min, the substrate negative bias voltage is set to 80-90 V, and the target current is set to 85-95 A; S5.2: depositing an Al-Ti composite film on the surface of the heat-treated thin slice obtained in step S4.4 by a multi-arc ion plating machine at a temperature of 400-500° C. for 2-3 hours to obtain a coated thin slice; S6 includes the following steps: S6.1: Add anhydrous aluminum chloride and 1-ethyl-3-methylimidazole chloride into a reaction box at a molar ratio of 2-3:1, and stir at a rate of 200-300 r / min until completely dissolved; S6.2: Keeping the stirring rate constant, add anhydrous manganese chloride in an amount equal to the molar amount of anhydrous aluminum chloride to the reaction box, and stir until it is completely dissolved to obtain an electroplating solution; S6.3: Using the coated thin sheet obtained in step S5.2 as a cathode and the spiral aluminum wire as an anode, electroplating is performed in the above-mentioned electroplating solution to obtain a secondary coated NdFeB thin sheet.
2. A method for improving the magnetic properties of NdFeB thin-film magnets according to claim 1, characterized in that: S1 includes the following steps: S1.1: Add titanium dioxide powder and graphite powder in a molar ratio of 2-3:1 into a high-speed disperser, disperse at high speed for 20-30 minutes, mix evenly, and seal into an aluminum tube to obtain a filled aluminum tube; S1.2: placing the above-mentioned filled aluminum tube in a box furnace, preheating to 400-500°C, and then hot rolling the preheated filled aluminum tube into a sheet with a thickness of 1-2 mm to obtain a precursor; S1.3: Place the aluminum ingot in a pit-type resistance furnace, heat it at 700-800°C for 1-2 hours, and then introduce argon gas into the pit-type resistance furnace to exhaust the air; S1.4: Keeping the temperature constant, add the above precursor into the pit type resistance furnace while stirring, then continue stirring for 1-2 hours, and then cast to obtain the master alloy ingot; S1.5: Add Al powder, Co powder, Al-Ce master alloy and Al-Cu master alloy into a vacuum arc melting furnace and melt for 30-40 minutes to obtain a light rare earth alloy melt; S1.6: adding the above master alloy ingot into the above light rare earth alloy melt, repeatedly smelting 4-5 times, and uniformly mixing to obtain a composite light rare earth alloy ingot; S1.7: The composite light rare earth alloy ingot is thrown into a strip shape at a speed of 6-8 m / s by a vacuum rapid quenching strip throwing device to obtain a light rare earth alloy strip.
3. A method for improving the magnetic properties of NdFeB thin-film magnets according to claim 2, characterized in that: S2 includes the following steps: S2.1: Add Al powder, Al-Tb master alloy, Al-Cu master alloy and Al-Ga master alloy into a vacuum arc melting furnace and melt for 1-2 hours to obtain a heavy rare earth alloy melt; S2.2: pour the heavy rare earth alloy melt into a mold of a melt pulse magnetic field treatment device, then turn on a pulse power supply, apply a phase-difference pulse magnetic field with a pulse voltage of 180-200V and a pulse frequency of 5-15Hz to the heavy rare earth alloy melt, and treat for 20-30min; S2.3: A dual-frequency ultrasonic field device is used to apply a 15-20kHz ultrasonic field to the mold. After ultrasonic field treatment for 10-20 minutes, the pulse power supply is turned on again, and a phase-difference pulse magnetic field and an ultrasonic field are applied simultaneously. The treatment is continued for 1-2 hours to obtain a heavy rare earth alloy strip.
4. A method for improving the magnetic properties of NdFeB thin-film magnets according to claim 2, characterized in that: The molar ratio of graphite to aluminum is 2-3:1, and the light rare earth alloy melt includes, by atomic number, 30-40% Co, 20-30% Cu, 10-20% Ce, and the balance is Al.
5. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 1, characterized in that: Calculated by atomic number, the heavy rare earth alloy belt includes: 40-50% Tb, 10-20% Ga, 5-10% Cu, and the balance is Al.
6. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 1, characterized in that: The area of the circular light rare earth alloy film region is the maximum circular region that can be made with the center of the NdFeB thin film magnet as the center of the circle.
7. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 1, characterized in that: The deposition current density of electrodeposition is 4-6 mA / cm 2 , the deposition time is 10-16min.
Citation Information
Patent Citations
Corrosion-resistant lanthanum-cerium-rich sintered neodymium iron boron magnet and preparation method
CN105427994A
A preparation method of high-performance sintered Nd-Fe-B permanent magnet material
CN109192493A
Preparation method of high-coercivity sintered neodymium-iron-boron magnet
CN111916284A
High-coercivity neodymium iron boron magnetic material and preparation method thereof
CN115101281A
Sintered nd-fe-b magnet composition and a production method for the sintered nd-fe-b magnet
US20170372823A1