Two-dimensional foam Pd4S nano-catalyst with ultrahigh methanol electro-catalysis stability
By using two-dimensional foam Pd4S nanocatalysts in methanol fuel cells, the problems of high cost and easy poisoning of Pd-based catalysts are solved, high stability and low-cost methanol electrocatalytic performance is achieved, and the electrocatalytic stability of the catalyst is significantly improved. .
Patent Information
- Application Number
- CN202410751917.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
Existing Pd-based catalysts in methanol fuel cells have problems such as high usage costs and easy poisoning, and their structures are prone to agglomeration during catalytic reactions, resulting in decreased activity and affecting stability.
Using two-dimensional Pd-PdO mixed-phase nanomaterials as precursors, a two-dimensional foam Pd4S nanocatalyst with ultra-high methanol electrocatalytic stability was prepared by reacting with n-dodecanethiol through a hydrothermal method. The sulfur element was used to reduce costs and improve Catalyst stability.
It achieves high stability and low-cost methanol electrocatalytic performance, and significantly improves the peak current retention rate of the catalyst after cyclic voltammetry testing, far exceeding the traditional c-Pd/C catalyst.
Smart Images

Figure HDA0004888257830000011 
Figure HDA0004888257830000012 
Figure HDA0004888257830000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nano-catalytic materials, and in particular relates to a method for preparing a two-dimensional foamed Pd4S nano-catalyst with ultra-high methanol electrocatalytic stability. Background Art
[0002] The extensive use of fossil energy such as coal and oil has produced a large amount of greenhouse gases, mainly carbon dioxide, which has brought about global climate change. In order to curb the adverse effects of global climate change, people have found a series of new ways to obtain energy, but most of them are limited by regionality or intermittent.
[0003] Fuel cells have attracted widespread attention from academia and industry because of their unrestricted geographical location and sustainable operation. The fuel cells currently being developed for commercial use are mainly proton exchange membrane fuel cells (such as methanol proton exchange membrane fuel cells), but the use cost of methanol proton exchange membrane fuel cells remains high, and the working performance still needs to be further improved. In recent years, the development of anion exchange membranes has made direct methanol fuel cells a research hotspot. Direct methanol fuel cells use small molecular weight methanol such as methanol, ethylene glycol and propylene glycol as anode fuel. Compared with hydrogen fuel cells, direct methanol fuel cells have ultra-high volume energy density, and the lower cost of methanol fuel makes the commercialization of direct methanol fuel cells possible. Among them, the anode catalyst of direct methanol fuel cells is one of its key issues. At present, Pd-based catalysts have been widely studied because of their excellent catalytic activity for the oxidation of methanol molecules, but the high cost of Pd and its easy poisoning by intermediates in the catalytic process hinder its industrial application. Therefore, people are working to reduce the demand for Pd in the catalyst while also improving the stability of the catalyst. The construction of metal compounds can not only reduce the amount of Pd used in the catalyst, but also change the electronic structure of Pd by introducing foreign elements, thereby optimizing the adsorption strength of the catalyst to the catalytic small molecules, thereby improving the catalytic performance of the catalyst to the methanol small molecules. However, the structure of the catalyst is prone to agglomeration during the catalytic reaction, resulting in a decrease in its activity. The three-dimensional foam structure can not only well retain the advantages of the ultra-high specific surface area and ultra-high electronic conductivity of the two-dimensional nanomaterials, but also because of its own foam-like structure, it can play a good self-supporting role, which can avoid the agglomeration of the catalyst during use to a certain extent. Summary of the invention
[0004] Based on the above problems existing in the prior art, the object of the present invention is to provide a two-dimensional foam Pd4S nanocatalyst with ultra-high methanol electrocatalytic stability and a preparation method thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme:
[0006] The preparation method of the two-dimensional foam Pd4S nanocatalyst with ultra-high methanol electrocatalytic stability is to use the two-dimensional Pd-PdO mixed phase nanomaterial as a precursor and n-dodecyl mercaptan as a sulfur source to synthesize the two-dimensional foam Pd4S nanocatalyst by hydrothermal method. Specifically, it includes the following steps:
[0007] Step 1, adding 10-15 mg of palladium acetylacetonate and 15-30 mg of potassium nitrate crystals to an ethanol aqueous solution, and stirring evenly to form a precursor solution;
[0008] Step 2: placing the precursor solution obtained in step 1 in a 55-60° C. forced air drying oven to remove the solvent, collecting the solid and grinding it evenly in an agate mortar to obtain a precursor powder;
[0009] Step 3, reacting the precursor powder obtained in step 2 in a tube furnace at a reaction temperature of 210-300° C. for 120-180 min in an air atmosphere, and after the reaction is completed and cooled to ambient temperature, centrifuging and washing the obtained product to obtain a Pd-PdO mixed phase nanomaterial;
[0010] Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 0-10 mL of oleylamine as a solvent and 2-5000 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 180-300° C. for 45-180 min, and after the reaction is completed and cooled to ambient temperature, centrifuging and washing the obtained product to obtain a two-dimensional foam Pd4S nanocatalyst with ultra-high methanol electrocatalytic stability.
[0011] Furthermore, the volume ratio of ethanol to water in the ethanol-water solution in step 1 is 1:6.
[0012] Furthermore, in step 3, the centrifugal washing is performed multiple times with a mixture of ethanol and water (the volume ratio of ethanol to water is 1:1), and the centrifugal speed is 9000-11000 rpm.
[0013] Furthermore, in step 4, the washing is performed multiple times with a mixed solution of ethanol and cyclohexane (the volume ratio of cyclohexane to ethanol is 1:3), and the centrifugal speed is 9000-11000 rpm.
[0014] The principle of the present invention is: using palladium acetylacetonate as a pyrolysis precursor and potassium nitrate as a two-dimensional morphology directing agent, a Pd-PdO mixed-phase nanomaterial is synthesized as a substrate through a molten salt one-step pyrolysis method, and then n-dodecanethiol is introduced as a sulfur source to transform Pd-PdO into a two-dimensional foam Pd4S nanocatalyst.
[0015] The two-dimensional foamed Pd4S nanocatalyst prepared by the invention can be used to stably catalyze methanol electrooxidation reaction.
[0016] The beneficial effects of the present invention are embodied in:
[0017] 1. The present invention firstly prepares Pd-PdO mixed-phase nanomaterials by a one-step method, and then introduces a sulfur source to modify it to form a two-dimensional foam Pd4S nanocatalyst. The preparation method of the present invention requires simple equipment and the obtained product has good reproducibility; the two-dimensional foam Pd4S nanocatalyst obtained by the present invention not only has the structural advantage of a unique three-dimensional network, but also reduces the use cost of the catalyst because of the introduction of cheap sulfur elements to form metal sulfides, and has good stability for a variety of methanol electrocatalytic oxidation reactions.
[0018] 2. The two-dimensional foam Pd4S nanocatalyst prepared by the present invention provides a synthesis idea for synthesizing three-dimensional foam structures.
[0019] 3. The two-dimensional foam Pd4S nanomaterial prepared by the present invention is used as an electrocatalyst to catalyze methanol electrooxidation, and exhibits an electrocatalytic stability far exceeding that of c-Pd / C. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the X-ray diffraction pattern (XRD) of the two-dimensional foam Pd4S nanocatalyst obtained in Example 1.
[0021] Figure 2 a and c are transmission electron microscopy (TEM) images of the two-dimensional foam Pd4S nanocatalyst obtained in Example 1. Figure 2 b is an atomic force microscope (AFM) image of the two-dimensional foam Pd4S nanocatalyst obtained in Example 1, Figure 2 d, e and f are ultra-high resolution transmission electron microscopy (HRTEM) images of the two-dimensional foam Pd4S nanocatalyst obtained in Example 1 at different magnifications.
[0022] Figure 3 The scanning transmission electron microscope (STEM) image and the surface scanning element distribution map (Mapping) of the two-dimensional foam Pd4S nanocatalyst obtained in Example 1.
[0023] Figure 4 a is the performance curve of commercial palladium carbon (c-Pd / C) before and after 10000 cycles of cyclic voltammetry test in 0.5M KOH+1M MeOH solution, with a scan rate of 0.1V / s; Figure 4 b is the performance curve of the two-dimensional foam Pd4S nanocatalyst before and after 10000 cycles of cyclic voltammetry test in 0.5M KOH+1M MeOH solution, with a scan rate of 0.1V / s; Figure 4c is the peak current retention rate of the two-dimensional foam Pd4S nanocatalyst obtained in Example 1 and the standard catalyst c-Pd / C after 10,000 cycles of cyclic voltammetry test in 0.5M KOH+1M MeOH solution, with a scan rate of 0.1V / s. DETAILED DESCRIPTION
[0024] The following is a detailed description of an embodiment of the present invention. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.
[0025] Example 1
[0026] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0027] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0028] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0029] Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 5 mL of oleylamine as a solvent and 2 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 210° C. for 60 min, and after the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst.
[0030] The X-ray diffraction pattern, atomic force microscope image, transmission electron microscope image, ultra-high resolution transmission electron microscope image and element distribution map of the two-dimensional foam Pd4S nanocatalyst prepared in this example are shown in Figure 2. Figures 1 to 3 As shown. Figures 1 to 3 It can be seen that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak, a thickness of about 2 nm, two element signals of Pd and S, and a foam-like nanomorphology.
[0031] About 0.01 mg of the two-dimensional foam Pd4S nanocatalyst obtained in this example was dispersed on a glassy carbon electrode with a diameter of 3 mm, and its catalytic performance was tested in a 0.5M KOH+1M MeOH solution. The performance curves and peak current retention rates before and after 10,000 cycles of cyclic voltammetry testing are shown in Figure 2. Figure 4 As shown, the scan rate is 0.1 V / s, where c-Pd / C is used as the standard catalyst. Figure 4 c It can be seen that the peak current retention rate of the two-dimensional foam Pd4S nanocatalyst prepared in this embodiment after 10,000 cycles of cyclic voltammetry test in methanol is 97.98%, compared with the peak current retention rate of c-Pd / C of 35.30%, and the catalytic stability is significantly improved.
[0032] Example 2
[0033] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0034] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0035] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0036] Step 4: Use the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, add 10 mL of oleylamine as a solvent and 2 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, and react at 210° C. for 60 min. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst.
[0037] Characterization shows that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak and a foam-like nano-morphology.
[0038] The test was carried out in the same manner as in Example 1. The peak current retention rate of the two-dimensional foamed Pd4S nanocatalyst prepared in this example after 10,000 cycles of cyclic voltammetry test in methanol was 89.3%.
[0039] Example 3
[0040] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0041] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0042] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0043] Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 5 mL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 210° C. for 60 min, and after the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst.
[0044] Characterization shows that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak and a foam-like nano-morphology.
[0045] The test was carried out in the same manner as in Example 1. The peak current retention rate of the two-dimensional foamed Pd4S nanocatalyst prepared in this example after 10,000 cycles of cyclic voltammetry test in methanol was 88.2%.
[0046] Example 4
[0047] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0048] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0049] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0050] Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 5 mL of oleylamine as a solvent and 7 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 210° C. for 60 min, and after the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst.
[0051] Characterization shows that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak and a foam-like nano-morphology.
[0052] The test was carried out in the same manner as in Example 1. The peak current retention rate of the two-dimensional foamed Pd4S nanocatalyst prepared in this example after 10,000 cycles of cyclic voltammetry test in methanol was 89.0%.
[0053] Example 5
[0054] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0055] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0056] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0057] Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 5 mL of oleylamine as a solvent and 2 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 180° C. for 60 min, and after the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst.
[0058] Characterization shows that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak and a foam-like nano-morphology.
[0059] The test was carried out in the same manner as in Example 1. The peak current retention rate of the two-dimensional foamed Pd4S nanocatalyst prepared in this example after 10,000 cycles of cyclic voltammetry test in methanol was 87.4%.
[0060] Example 6
[0061] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0062] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0063] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0064] Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 5 mL of oleylamine as a solvent and 2 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 250° C. for 60 min, and after the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst with ultra-high methanol catalytic stability.
[0065] Characterization shows that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak and a foam-like nano-morphology.
[0066] The test was carried out in the same manner as in Example 1. The peak current retention rate of the two-dimensional foamed Pd4S nanocatalyst prepared in this example after 10,000 cycles of cyclic voltammetry test in methanol was 88.5%.
[0067] Example 7
[0068] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0069] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0070] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0071] Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 5 mL of oleylamine as a solvent and 2 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 300° C. for 60 min, and after the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst.
[0072] Characterization shows that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak and a foam-like nano-morphology.
[0073] The test was carried out in the same manner as in Example 1. The peak current retention rate of the two-dimensional foamed Pd4S nanocatalyst prepared in this example after 10,000 cycles of cyclic voltammetry test in methanol was 86.7%.
[0074] Example 8
[0075] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0076] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0077] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0078] Step 4: Use the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, add 5 mL of oleylamine as a solvent and 2 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, and react at 210° C. for 45 min. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst.
[0079] Characterization shows that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak and a foam-like nano-morphology.
[0080] The test was carried out in the same manner as in Example 1. The peak current retention rate of the two-dimensional foamed Pd4S nanocatalyst prepared in this example after 10,000 cycles of cyclic voltammetry test in methanol was 90.1%.
[0081] Example 9
[0082] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0083] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0084] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0085] Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 5 mL of oleylamine as a solvent and 2 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 210° C. for 120 min, and after the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst.
[0086] Characterization shows that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak and a foam-like nano-morphology.
[0087] The test was carried out in the same manner as in Example 1. The peak current retention rate of the two-dimensional foamed Pd4S nanocatalyst prepared in this example after 10,000 cycles of cyclic voltammetry test in methanol was 85.3%.
[0088] Example 10
[0089] Step 1: Add 10 mg of palladium acetylacetonate and 15 mg of potassium nitrate crystals to an ethanol aqueous solution (the volume ratio of ethanol to water is 1:6), and stir evenly to form a precursor solution.
[0090] Step 2: Place the precursor solution obtained in step 1 in a 55° C. forced air drying oven to remove the solvent, collect the solid and grind it evenly in an agate mortar to obtain a precursor powder.
[0091] Step 3: The precursor powder obtained in step 2 is reacted in a tube furnace at a reaction temperature of 210° C. for 180 min under an air atmosphere. After the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of ethanol and water in a volume ratio of 1:1, and the centrifugal speed is 11000 rpm) to obtain Pd-PdO mixed-phase nanomaterials.
[0092] Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 5 mL of oleylamine as a solvent and 2 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 210° C. for 180 min, and after the reaction is completed and cooled to ambient temperature, the obtained product is centrifuged and washed (washed 4 times with a mixture of cyclohexane and ethanol in a volume ratio of 1:3, and the centrifugal speed is 11000 rpm) to obtain a two-dimensional foam Pd4S nanocatalyst with ultra-high methanol catalytic stability.
[0093] Characterization shows that the two-dimensional foamed Pd4S nanocatalyst obtained in this example has a clear Pd4S diffraction signal peak and a foam-like nano-morphology.
[0094] The test was carried out in the same manner as in Example 1. The peak current retention rate of the two-dimensional foamed Pd4S nanocatalyst prepared in this example after 10,000 cycles of cyclic voltammetry test in methanol was 84.1%.
[0095] The above are merely exemplary embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a two-dimensional foamed Pd4S nanocatalyst with ultra-high methanol electrocatalytic stability, characterized in that: Two-dimensional Pd4S foam nanocatalyst was synthesized by hydrothermal method using two-dimensional Pd-PdO mixed-phase nanomaterials as precursors and n-dodecanethiol as the sulfur source.
2. The preparation method according to claim 1, characterized in that: The steps include: Step 1, adding 10-15 mg of palladium acetylacetonate and 15-30 mg of potassium nitrate crystals to an ethanol aqueous solution, and stirring evenly to form a precursor solution; Step 2, placing the precursor solution obtained in step 1 in a 55-60° C. forced air drying oven to remove the solvent, collecting the solid and grinding it evenly to obtain a precursor powder; Step 3, reacting the precursor powder obtained in step 2 in a tube furnace at a reaction temperature of 210-300° C. for 120-180 min in an air atmosphere, and after the reaction is completed and cooled to ambient temperature, centrifuging and washing the obtained product to obtain a Pd-PdO mixed phase nanomaterial; Step 4: Using the Pd-PdO mixed-phase nanomaterial obtained in step 3 as a substrate, adding 0-10 mL of oleylamine as a solvent and 2-5000 μL of n-dodecanethiol as a sulfur source in a hydrothermal reactor, reacting at 180-300° C. for 45-180 min, and after the reaction is completed and cooled to ambient temperature, centrifuging and washing the obtained product to obtain a two-dimensional foam Pd4S nanocatalyst with ultra-high methanol electrocatalytic stability.
3. The preparation method according to claim 2, characterized in that: The volume ratio of ethanol to water in the ethanol-water solution in step 1 is 1:
6.
4. The preparation method according to claim 2, characterized in that: In step 3, the centrifugal washing is performed multiple times with a mixture of ethanol and water, and the centrifugal speed is 9000-110000 rpm.
5. The preparation method according to claim 2, characterized in that: In step 4, the washing is performed multiple times with a mixture of ethanol and cyclohexane, and the centrifugal speed is 9000-110000 rpm.
6. A two-dimensional foamed Pd4S nanocatalyst with ultra-high methanol electrocatalytic stability obtained by the preparation method according to any one of claims 1 to 5.
7. An application of the two-dimensional foamed Pd4S nanocatalyst according to claim 6, characterized in that: Used to catalyze methanol electrooxidation reaction.