Secondary battery and electronic device

By using lithium composite metal oxides, binders and specific inorganic additives in secondary batteries, combined with the electrolyte components of fluoroethylene carbonate, nitrogen-containing lithium salts and propyl propionate, the problem of high voltage in secondary batteries is solved. It achieves better low-temperature performance and high-temperature performance due to poor cycle performance and resistance issues in low-temperature and high-temperature environments.

CN118782874APending Publication Date: 2024-10-15NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410764288.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing secondary batteries have poor cycle performance under high voltage, and have problems with lithium ion acceptance in low temperature environments and rising resistance in high temperature environments, which affect their service life and safety performance.

Method used

By using lithium composite metal oxides, binders, and specific inorganic additives in secondary batteries, the electrolyte components of fluoroethylene carbonate, nitrogen-containing lithium salts, and propyl propionate are combined to adjust their use in the positive electrode and electrolyte. ratio to improve lithium ion acceptance and resistance characteristics at low and high temperatures.

Benefits of technology

It effectively suppresses the increase in initial resistance of the secondary battery at low temperatures, improves low-temperature performance, and suppresses the increase in resistance in high-temperature environments, improving the overall performance of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004892084980000041
    Figure BDA0004892084980000041
  • Figure BDA0004892084980000081
    Figure BDA0004892084980000081
  • Figure BDA0004892084980000211
    Figure BDA0004892084980000211
Patent Text Reader

Abstract

The invention provides a secondary battery and an electronic device. The secondary battery comprises a positive electrode and an electrolyte, the positive electrode comprises a lithium composite metal oxide, a binder and an inorganic additive, and metal elements in the inorganic additive comprise at least one of an aluminum element, a magnesium element, a titanium element, a zirconium element, a niobium element, an indium element, a tungsten element, a tin element, a zinc element or an antimony element. And the electrolyte contains fluoroethylene carbonate, nitrogen-containing lithium salt and propyl propionate. According to the secondary battery provided by the invention, based on the mass of the electrolyte, when the sum of the mass percentages of the fluoroethylene carbonate and the nitrogen-containing lithium salt is more than 0.76 mass% and less than 10.17 mass%, and the mass percentage of the propyl propionate is more than 12 mass% and less than 65 mass%, the lithium ion acceptability of the secondary battery at a low temperature can be improved; initial resistance increase at low temperature is inhibited, and high-temperature performance of the secondary battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage, and in particular to a secondary battery and an electronic device. Background Art

[0002] With the rapid development of electronic products such as smart phones, tablet computers and smart wearables, higher requirements are placed on the service life and safety performance of secondary batteries, taking into account the different usage time and working environment temperature of different electronic digital products. With the increase of charging cut-off voltage, the energy density of the battery has been significantly improved. However, in the prior art, as the voltage of the secondary battery increases, the cycle performance of the high-voltage secondary battery deteriorates. After using high-voltage positive electrode film-forming additives to improve the cycle characteristics, the low-temperature characteristics are greatly affected. Summary of the invention

[0003] The present application provides a secondary battery and an electronic device, which can improve both the low-temperature performance and the high-temperature performance of the secondary battery by adjusting the composition of the positive electrode used in the secondary battery and the components in the electrolyte.

[0004] In a first aspect, the present application provides a secondary battery, the secondary battery comprising a positive electrode and an electrolyte. The positive electrode comprises a lithium composite metal oxide, a binder and an inorganic additive, and the metal element in the inorganic additive comprises at least one of aluminum, magnesium, titanium, zirconium, niobium, indium, tungsten, tin, zinc or antimony. The electrolyte contains fluoroethylene carbonate, a nitrogen-containing lithium salt and propyl propionate, and based on the mass of the electrolyte, the sum of the mass percentage of fluoroethylene carbonate and the nitrogen-containing lithium salt is greater than 0.76 mass% and less than 10.17 mass%, and the mass percentage of propyl propionate is greater than 12 mass% and less than 65 mass%.

[0005] The inventors of the present application have found that propyl propionate easily forms a thick film on the surface of the positive electrode material, especially in the presence of inorganic additives, which catalyze the film formation of propyl propionate, causing the film impedance to increase and affecting the low-temperature characteristics of the secondary battery. The inventor speculates that for a secondary battery, when the positive electrode includes a lithium composite metal oxide, a binder, and any inorganic additive containing aluminum, magnesium, titanium, zirconium, niobium, indium, tungsten, tin, zinc or antimony, and the electrolyte contains fluoroethylene carbonate, nitrogen-containing lithium salt and propyl propionate, and the total content of fluoroethylene carbonate and nitrogen-containing lithium salt is greater than 0.76 mass % and less than 10.17 mass %, and the content of propyl propionate is greater than 12 mass % and less than 65 mass %, it can improve the lithium ion acceptance of the secondary battery at low temperatures (ambient temperature below -20°C), suppress the increase in its initial resistance at low temperatures, thereby improving the low temperature performance of the secondary battery, and taking into account the improvement of the high temperature performance of the secondary battery, especially suppressing the resistance increase of the secondary battery after storage at high temperature (ambient temperature greater than 45°C).

[0006] In some embodiments, based on the mass of the electrolyte, the sum of the mass percentages of fluoroethylene carbonate and the nitrogen-containing lithium salt is greater than 4.89 mass % and less than 10.17 mass %. By adjusting the value of the sum of the mass percentages of fluoroethylene carbonate and the nitrogen-containing lithium salt within the above range, the lithium ion acceptance performance of the secondary battery at low temperatures can be further improved.

[0007] In some embodiments, based on the mass of the electrolyte, the mass percentage of propyl propionate is greater than 22 mass % and less than 47 mass %. By adjusting the mass percentage of propyl propionate within the above range, the low temperature performance of the secondary battery can be further improved, while the high temperature performance of the secondary battery can be improved, especially the resistance increase of the secondary battery after high temperature storage can be suppressed.

[0008] In some embodiments, the binder includes at least one of polyvinylidene fluoride, polyacrylonitrile, and polyacrylic acid. By adding the above binder to the positive electrode, the lithium ion acceptance of the secondary battery at low temperature can be further improved, thereby helping to suppress the initial resistance of the secondary battery at low temperature, while taking into account the improvement of the high temperature performance of the secondary battery.

[0009] In some embodiments, the positive electrode further contains a dispersant, which includes at least one of sodium salt, potassium salt and ammonium salt of dioctyl sulfosuccinate, dipentyl sulfosuccinate and dicyclopentyl sulfosuccinate. By adding the above dispersant to the positive electrode, the lithium ion acceptance of the secondary battery at low temperature can be further improved, while taking into account the improvement of the high temperature performance of the secondary battery.

[0010] In some embodiments, the nitrogen-containing lithium salt is selected from LiN(FCO)2, LiN(FCO)(FSO2), LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,2-perfluoroethane disulfonyl imide lithium, cyclic 1,3-perfluoropropane disulfonyl imide lithium [CAS: 189217-62-7], LiN(CF3SO2)(C4F9SO2), 4,5-dicyano-2-trifluoromethyl imidazolium lithium salt, 4,5-dicyano-2-pentafluoroethyl imidazolium lithium salt , 2,4,5-tricyanoimidazole lithium salt, 5,6-dicyano-2-trifluoromethylbenzimidazole lithium salt, 5,6-dicyano-2-pentafluoroethylbenzimidazole lithium salt, 2,5,6-tricyanobenzimidazole lithium salt, 4,7-dicyano-2-trifluoromethylbenzimidazole lithium salt, 4,7-dicyano-2-pentafluoroethylbenzimidazole lithium salt, 2,4,7-tricyanobenzimidazole lithium salt, 4,5,6,7-tetracyano-2-trifluoromethylbenzimidazole lithium salt, 4,5,6,7-tetracyano-2-pentafluoroethylbenzimidazole lithium salt or at least one of 2,4,5,6,7-pentacyanobenzimidazole lithium salt. By selecting the above-mentioned nitrogen-containing lithium salt in the electrolyte, it can synergistically improve the lithium ion acceptance of the secondary battery at low temperatures with fluoroethylene carbonate and propyl propionate, inhibit its initial resistance increase at low temperatures, thereby improving the low temperature performance of the secondary battery, while taking into account the improvement of the high temperature performance of the secondary battery, especially inhibiting the resistance increase of the secondary battery after high-temperature storage.

[0011] In some embodiments, based on the mass of the electrolyte, the mass percentage of fluoroethylene carbonate is 0.53 mass % or more and 8.95 mass % or less, or the mass percentage of nitrogen-containing lithium salt is 0.23 mass % or more and 3.45 mass % or less, or the mass percentage of propyl propionate is 24 mass % or more and 39 mass % or less. By adjusting the above ranges, the low-temperature initial resistance of the secondary battery can be further improved while taking into account the improvement of its high-temperature performance.

[0012] In some embodiments, the electrolyte includes other additives, including 1,2-bis(difluorophosphine)ethane [CAS: 3965-00-2], a compound of formula 1, a compound of formula 2, vinylene carbonate [CAS: 872-36-6], lithium fluorosulfonate [CAS: 13453-75-3], succinonitrile [CAS: 110-61-2], adiponitrile [CAS: 111-69-3], 1,3,6-hexanitrile [CAS: 1772-25-4], 1,2,3-tris(2-cyanoethoxy)propane [CAS: 2465- When at least one of the following is used, the stability of the film formed by propyl propionate on the surface of the positive electrode material at high temperature can be improved, and the ion conduction rate of lithium ions can be increased, thereby further improving the resistance characteristics after high temperature storage.

[0013]

[0014] In some embodiments, the lithium composite metal oxide contains a first element, and the first element includes at least one of lanthanum, yttrium, cerium, tungsten or strontium. Based on the mass of the lithium composite metal oxide, the mass percentage of the first element is greater than 0.01 mass% and less than 1 mass%. By adding the above-mentioned first element to the lithium composite metal oxide and adjusting the mass percentage value of the first element within the above-mentioned range, it is beneficial to further improve the low-temperature initial resistance of the lithium-ion battery and enhance its low-temperature performance.

[0015] In some of the embodiments, the positive electrode includes a primer layer and an active material layer disposed on the current collector, and the above-mentioned inorganic additive is contained in the active material layer and / or the primer layer. In some of the embodiments, the positive electrode includes an edge layer and an active material layer disposed on the current collector, and the above-mentioned inorganic additive is contained in the edge layer. By changing the position where the inorganic additive is added, the inorganic additive can be added to any one or more of the active material layer, the primer layer or the edge layer. From the viewpoint of improving the initial resistance at low temperature, it is preferably contained in the primer layer or the edge layer. From the viewpoint of improving the resistance after high-temperature storage, it is preferably contained in the active material layer.

[0016] In a second aspect, the present application provides an electronic device, which includes the above-mentioned secondary battery.

[0017] The present application uses a positive electrode containing a lithium composite metal oxide, a binder and the above-mentioned inorganic additives, and at the same time, the electrolyte contains an appropriate amount of fluoroethylene carbonate, nitrogen-containing lithium salt and propyl propionate, so that it can not only improve the lithium ion acceptance of the secondary battery at low temperatures, but also inhibit its initial resistance increase at low temperatures, and also inhibit its resistance increase after high-temperature storage. It can be seen that the secondary battery described in the present application has both better low-temperature performance and better high-temperature performance. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0019] For simplicity, only some numerical ranges are clearly disclosed herein. However, any lower limit can be combined with any upper limit to form a range that is not clearly recorded, and any lower limit can be combined with other lower limits to form a range that is not clearly recorded, and any upper limit can be combined with any other upper limit to form a range that is not clearly recorded. In addition, although it is not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form a range that is not clearly recorded.

[0020] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C.

[0021] Secondary battery

[0022] A first aspect of an embodiment of the present application provides a secondary battery, the secondary battery comprising an electrolyte, a positive electrode, a negative electrode and a separator.

[0023] Electrolyte

[0024] The electrolyte of this embodiment contains fluoroethylene carbonate, nitrogen-containing lithium salt and propyl propionate. Based on the mass of the electrolyte, the sum of the mass percentages of fluoroethylene carbonate and the nitrogen-containing lithium salt is greater than 0.76 mass % and less than 10.17 mass %, and the mass percentage of propyl propionate is greater than 12 mass % and less than 65 mass %.

[0025] Exemplarily, in some embodiments, further from the viewpoint of improving lithium ion acceptance, based on the quality of electrolyte, the total content of fluoroethylene carbonate and nitrogen-containing lithium salt is more than 0.76 mass %, preferably more than 1.21 mass %. In addition, as the upper limit of the total content of fluoroethylene carbonate and nitrogen-containing lithium salt, from the viewpoint that the electrochemical characteristics under low temperature environment improve, be below 10.17 mass %, preferably below 9.64 mass %.

[0026] For example, in some embodiments, the total content of fluoroethylene carbonate and nitrogen-containing lithium salt is a mass %, and a is 0.76, 1.21, 1.63, 1.97, 2.48, 3.33, 4.02, 4.86, 4.89, 5.88, 6.9, 8.64, 9.64, 10.17 or within the range consisting of any two of the above values. When the total content of fluoroethylene carbonate and nitrogen-containing lithium salt is within the above range, it helps to further improve the low-temperature initial resistance.

[0027] Exemplarily, in some embodiments, from the viewpoint of improving the lithium ion acceptance of secondary battery, based on electrolyte quality, the content of fluoroethylene carbonate is more than 0.53 mass %, and the content that is preferably fluoroethylene carbonate is more than 0.87 mass %, more preferably more than 1.45 mass %, more preferably more than 2.57 mass %.In addition, as the upper limit of the content of fluoroethylene carbonate, from the viewpoint of improving low temperature initial resistance, the content of fluoroethylene carbonate is below 8.95 mass %, preferably below 7.15 mass %, more preferably below 6.23 mass %, more preferably below 5.19 mass %, particularly preferably below 4.12 mass %.When within the above range, contribute to further improve low temperature initial resistance.

[0028] Exemplarily, in some embodiments, the nitrogen-containing lithium salt is selected from LiN(FCO)2, LiN(FCO)(FSO2), LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,2-perfluoroethane disulfonyl imide lithium, cyclic 1,3-perfluoropropane disulfonyl imide lithium, LiN(CF3SO2)(C4F9SO2), 4,5-dicyano-2-trifluoromethyl imidazole lithium salt, 4,5-dicyano-2-pentafluoroethyl imidazole lithium salt, 2,4,5- At least one of tricyanoimidazole lithium salt, 5,6-dicyano-2-trifluoromethylbenzimidazole lithium salt, 5,6-dicyano-2-pentafluoroethylbenzimidazole lithium salt, 2,5,6-tricyanobenzimidazole lithium salt, 4,7-dicyano-2-trifluoromethylbenzimidazole lithium salt, 4,7-dicyano-2-pentafluoroethylbenzimidazole lithium salt, 2,4,7-tricyanobenzimidazole lithium salt, 4,5,6,7-tetracyano-2-trifluoromethylbenzimidazole lithium salt, 4,5,6,7-tetracyano-2-pentafluoroethylbenzimidazole lithium salt or 2,4,5,6,7-pentacyanobenzimidazole lithium salt.

[0029] For example, in some embodiments, from the viewpoint of improving lithium ion acceptance, based on the mass of the electrolyte, the content of the nitrogen-containing lithium salt is 0.23% by mass or more, preferably 0.34% by mass or more, more preferably 0.41% by mass or more, and further preferably 0.52% by mass or more. In addition, as the upper limit of the content of the nitrogen-containing lithium salt, from the viewpoint of improving the low-temperature initial resistance, the content of the nitrogen-containing lithium salt is 3.45% by mass or less, preferably 2.78% by mass or less, more preferably 2.21% by mass or less, further preferably 1.78% by mass or less, and particularly preferably 1.45% by mass or less. When within the above range, it helps to further improve the low-temperature initial resistance.

[0030] Exemplarily, in some embodiments, from the viewpoint of improving the lithium ion acceptance of the secondary battery, based on the mass of the electrolyte, the content of propyl propionate is 12% by mass or more, preferably 22% by mass or more, more preferably 24% by mass or more, further preferably 28% by mass or more, and further preferably 31% by mass or more. In addition, as the upper limit of the content of propyl propionate, from the viewpoint of suppressing the increase in resistance after high temperature storage, the content of propyl propionate is 65% by mass or less, preferably 52% by mass or less, more preferably 47% by mass or less, further preferably 45% by mass or less, and particularly preferably 39% by mass or less. When within the above range, it helps to further suppress the increase in resistance after high temperature storage.

[0031] Exemplarily, in some embodiments, the electrolyte may further include other additives, such as 1,2-bis(difluorophosphine)ethane, a compound of formula 1, a compound of formula 2, vinylene carbonate, lithium fluorosulfonate, succinonitrile, adiponitrile, 1,3,6-hexanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, vinyl sulfate, fluorobenzene, cyclohexylbenzene, biphenyl, tris(trimethylsilane)phosphate or tris(trimethylsilane)borate. At least one of the other additives can improve the stability of the aforementioned film at high temperatures and increase the ion conduction rate of lithium ions, thereby further improving the resistance characteristics after high temperature storage. The above-mentioned other additives may be only one or more.

[0032]

[0033] For example, in some embodiments, from the viewpoint of improving the conduction of lithium ions in the aforementioned coating, based on the mass of the electrolyte, the content of other additives is 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and further preferably 0.5% by mass or more. In addition, as the upper limit of the content of other additives, from the viewpoint of improving the low-temperature initial resistance, the content of other additives is 10% by mass or less, preferably 9% by mass or less, more preferably 8% by mass or less, further preferably 7% by mass or less, and particularly preferably 5% by mass or less. When within the above range, it helps to further improve the low-temperature initial resistance characteristics.

[0034] The present application does not particularly limit the type of electrolyte, and any substance known as an electrolyte can be used arbitrarily, as long as it does not damage the effect of the present application. The present application does not particularly limit the quality of the electrolyte, as long as it does not damage the effect of the present application. For example, the lithium salt used in the electrolyte of the present application includes lithium hexafluorophosphate, and the content of lithium hexafluorophosphate is 9 to 15% by mass, preferably 9 to 13% by mass, and more preferably 9 to 12% by mass based on the mass of the electrolyte. By setting the above content range, the improvement of low-temperature initial resistance and resistance characteristics after high-temperature storage can be more balanced.

[0035] The present application has no particular restrictions on the type of solvent for the electrolyte, and may include any non-aqueous solvent known in the prior art that can be used as a solvent for the electrolyte. In some embodiments, the non-aqueous solvent includes, but is not limited to, one or more of the following: linear carbonates, cyclic carboxylates, cyclic ethers, linear ethers, phosphorus-containing organic solvents, and sulfur-containing organic solvents.

[0036] positive electrode

[0037] The positive electrode of this embodiment includes a positive electrode current collector and a positive electrode mixture layer provided on the positive electrode current collector. The positive electrode mixture layer can be one layer or multiple layers, including a positive electrode active material layer, and optionally including a bottom coating layer or an edge layer. The positive electrode mixture layer contains a positive electrode active material, a binder, and an inorganic additive.

[0038] Exemplarily, in some embodiments, the bottom coating layer is located between the current collector and the positive electrode active material layer, and is used to improve the mechanical adhesion between the current collector and the active material layer and reduce the resistance therebetween.

[0039] Exemplarily, in some embodiments, the edge layer is provided at the edge of the current collector and is juxtaposed with the positive electrode active layer, and is used to improve the insulation between the positive electrode edge and the negative electrode edge. The positive electrode active material is any material that can reversibly intercalate and deintercalate lithium ions.

[0040] Exemplarily, in some embodiments, as the positive electrode active material for a secondary battery, a composite metal oxide containing one or more selected from the group consisting of cobalt, manganese, and nickel and lithium, or a lithium-containing olivine-type phosphate containing one or more selected from iron, cobalt, nickel, and manganese is used. These positive electrode active materials can be used alone or in combination of two or more.

[0041] Exemplarily, in some embodiments, as such a lithium composite metal oxide, for example, those selected from LiCoO2, LiMn2O4, LiNiO2, LiCo 1-x Ni x O2 (0.01 < x < 1), LiNi x Mn y Co z O2 (x + y + z = 1), a solid solution of Li2MnO3 and LiMO2 (M is a transition metal such as Co, Ni, Mn, Fe, etc.), LiNi 1 / 2 Mn 3 / 2 O4, LiFePO4, LiMnPO4, and LiMn 1- x FexPO4 (0.01 < x < 1) and more preferably two or more. A part of these composite metal oxides with lithium or lithium-containing olivine-type phosphates can be replaced by other elements, or a part of cobalt, nickel, manganese, and iron can be replaced by one or more elements selected from Co, Mn, Ni, Mg, Al, B, Ti, V, Nb, Cu, Zn, Mo, Ca, Sr, W, and Zr, or coated with a compound or carbon material containing these other elements.

[0042] Exemplarily, in some embodiments, as such a lithium composite metal oxide, a first element is further included, and the first element includes at least one of lanthanum, iridium, cerium, tungsten or strontium. From the viewpoint of improving the low temperature initial resistance characteristics of the lithium ion battery, based on the mass of the lithium composite metal oxide, the content of any one of the first elements is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, and further preferably 0.05% by mass or more. In addition, as the upper limit of the content of the first element, the content of any one of the first elements is 1% by mass or less, preferably 0.5% by mass or less, more preferably 0.3% by mass or less, further preferably 0.15% by mass or less, and particularly preferably 0.1% by mass or less.

[0043] As the voltage during charging, from the viewpoint of increasing the voltage, the positive electrode potential is preferably 4.4 V (vs. Li / Li + ) or more, more preferably 4.5V (vs.Li / Li + ) or more, particularly preferably 4.6V (vs.Li / Li + )above.

[0044] The conductive agent of the positive electrode of the present application is not particularly limited as long as it is an electronic conductive material that does not cause chemical changes. Examples include graphites such as natural graphite (flake graphite, etc.), artificial graphite, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black, etc. Carbon black. In addition, graphite and carbon black can also be appropriately mixed for use. The amount of the conductive agent added to the positive electrode mixture is preferably 1 to 10% by mass, particularly preferably 1.5 to 5% by mass.

[0045] For example, in some embodiments, the positive electrode binder includes at least one of polyvinylidene fluoride, polyacrylonitrile, and polyacrylic acid. From the viewpoint of improving lithium ion acceptance and low-temperature initial resistance of the secondary battery, polyacrylonitrile is preferred.

[0046] Exemplarily, in some embodiments, from the perspective of improving lithium ion acceptance, the positive electrode binder may further include a dispersant, the dispersant including at least one of sodium salt, potassium salt and ammonium salt of dioctyl sulfosuccinate, dipentyl sulfosuccinate and dicyclopentyl sulfosuccinate.

[0047] Exemplarily, in some embodiments, from the perspective of improving low-temperature initial resistance, the metal element in the inorganic additive contained in the positive electrode includes at least one of aluminum, magnesium, titanium, zirconium, niobium, indium, tungsten, tin, zinc or antimony.

[0048] For example, in some embodiments, the inorganic additive may be at least one of an inorganic metal oxide and an inorganic metal hydroxide, such as aluminum oxide, aluminum hydroxide, boehmite, magnesium oxide, magnesium hydroxide, titanium dioxide, zirconium dioxide, niobium monoxide, niobium dioxide, niobium trioxide, niobium pentoxide, indium trioxide, tungsten trioxide, tin dioxide, zinc oxide, or antimony trioxide.

[0049] The inorganic additive may be contained in any one or more of the active material layer, the undercoat layer or the edge layer. For example, in some embodiments, from the viewpoint of improving the initial resistance at low temperature, it is preferably contained in the undercoat layer or the edge layer. From the viewpoint of improving the resistance after high temperature storage, it is preferably contained in the active material layer.

[0050] For example, in some embodiments, the density of the positive electrode active material layer is generally 3.5 g / cm 3 In order to further increase the capacity of the battery, it is preferably 3.8 g / cm 3 More preferably 4 g / cm 3 More preferably, 4.1 g / cm 3 In addition, the upper limit is preferably 4.6 g / cm 3 the following.

[0051] For example, in some embodiments, examples of the positive electrode current collector may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and carbon materials such as carbon cloth or carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum foil. There is no particular limitation on the type of the positive electrode current collector of the present application, and it may be any material known to be suitable for use as a positive electrode current collector.

[0052] Example

[0053] There are three ways to make the positive electrode:

[0054] Method 1: Inorganic additives are included in the positive electrode active material layer

[0055] The above-mentioned positive electrode active material, inorganic additives, conductive agents such as acetylene black, carbon black, and binders such as polyvinylidene fluoride or polyacrylonitrile are mixed, and a high boiling point solvent such as 1-methyl-2-pyrrolidone is added and kneaded to form a slurry, which is then coated on the aluminum foil of the current collector, dried, and pressed to form a positive electrode.

[0056] Method 2: Inorganic additives are included in the base coat

[0057] The inorganic additives are mixed with conductive agents such as acetylene black and carbon black, and binders such as polyvinylidene fluoride or polyacrylonitrile, deionized water is added thereto and mixed evenly to form a slurry, which is then coated on the aluminum foil of the current collector and dried to form a primer layer.

[0058] The above-mentioned positive electrode active material is mixed with a conductive agent such as acetylene black, carbon black, and a binder such as polyvinylidene fluoride or polyacrylonitrile, and a high boiling point solvent such as 1-methyl-2-pyrrolidone is added and kneaded to form a slurry, which is then applied to the base coating, dried, and pressed to form a positive electrode.

[0059] Method 3: Inorganic additives are included in the edge layer

[0060] The inorganic additive is mixed with a conductive agent such as acetylene black, carbon black, and a binder such as polyvinylidene fluoride or polyacrylonitrile, and deionized water is added thereto and mixed evenly to prepare a slurry 1.

[0061] The above-mentioned positive electrode active material is mixed with a conductive agent such as acetylene black, carbon black, and a binder such as polyvinylidene fluoride or polyacrylonitrile, and a high boiling point solvent such as 1-methyl-2-pyrrolidone is added thereto and kneaded to prepare slurry 2 .

[0062] Slurry 1 and slurry 2 are coated in parallel on the aluminum foil of the current collector, with slurry 1 located at one or two outer edges of slurry 2 (along the coating direction), and then dried and pressed to form a positive electrode.

[0063] negative electrode

[0064] The negative electrode of this embodiment includes a negative electrode current collector and a negative electrode mixture layer disposed on the surface of the negative electrode current collector, wherein the negative electrode mixture layer contains a negative electrode active material. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being accidentally precipitated on the negative electrode during charging.

[0065] The present application does not particularly limit the negative electrode active material, and examples thereof include carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials in combination thereof. Carbon-based negative electrode active materials refer to active materials with carbon as the main skeleton that can be inserted with lithium, and examples of carbon-based negative electrode active materials include carbonaceous materials and graphite materials.

[0066] Exemplarily, in some embodiments, as carbonaceous materials, for example, graphitizable carbon, non-graphitizable carbon with a similar amorphous structure represented by glassy carbon, etc. can be cited. Here, as graphitizable carbon, for example, carbon materials obtained from petroleum or coal using tar pitch as raw material can be cited. When specific examples are cited, coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fibers, and pyrolysis vapor-grown carbon fibers can be cited. In addition, as non-graphitizable carbon, for example, phenolic resin sintered bodies, polyacrylonitrile-based carbon fibers, quasi-isotropic carbon, furfuryl alcohol resin sintered bodies (PFA), hard carbon, etc. can be cited.

[0067] For example, in some embodiments, as graphite materials, for example, natural graphite, artificial graphite, etc. can be cited. Among them, as artificial graphite, for example: artificial graphite obtained by heat treating carbon containing graphitized carbon mainly at above 2800°C, graphite MCMB obtained by heat treating MCMB at above 2000°C, graphite mesophase pitch-based carbon fiber obtained by heat treating mesophase pitch-based carbon fiber at above 2000°C, etc. can be cited. In addition, in the present application, as a carbon-based negative electrode active material, natural graphite (amorphous coated natural graphite) in which at least a portion of its surface is coated with amorphous carbon can be used.

[0068] Exemplarily, in some embodiments, the metal-based negative electrode active material is an active material containing a metal, generally referring to an active material having an element capable of inserting lithium or alloying with lithium in the structure, and an active material having a theoretical current capacity of 500 mAh / g or more per unit mass when inserting lithium or alloying with lithium. As a metal-based negative electrode active material, for example, lithium metal, a single metal that can form a lithium alloy (such as Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn or Ti, etc.) and its alloy, and their oxides, sulfides, nitrides, silicides, carbides, phosphides, etc. can be used. Among them, as a metal-based negative electrode active material, an active material containing silicon (silicon-based negative electrode active material) is preferably used. This is because the secondary battery can be made high-capacity by using a silicon-based negative electrode active material.

[0069] For example, in some embodiments, as a silicon-based negative electrode active material, for example, silicon (Si), an alloy containing silicon, silicon oxide, a silicon-containing material coated with conductive carbon or a composite of a silicon-containing material and conductive carbon can be cited. From the viewpoint of improving the battery capacity, a silicon-carbon material is preferred, such as a composite material of porous carbon loaded with silicon. In addition, the negative electrode active material can be used alone or in combination of two or more in any ratio.

[0070] Exemplarily, in some embodiments, the negative electrode mixture layer may further include a negative electrode binder. The negative electrode binder may improve the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the solvent used in the manufacture of the electrolyte or electrode. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, and the like.

[0071] For example, in some embodiments, as a current collector for holding the negative electrode active material, any known current collector can be used. Examples of negative electrode current collectors include, but are not limited to, metal materials such as copper, nickel, stainless steel, and nickel-plated steel. In some embodiments, the negative electrode current collector is copper foil.

[0072] Exemplarily, in some embodiments, the negative electrode can be prepared by the following method: a negative electrode mixture slurry comprising a negative electrode active material, a resin binder, etc. is coated on a negative electrode current collector, and after drying, the negative electrode mixture slurry is rolled to form a negative electrode mixture layer on both sides of the negative electrode current collector, thereby obtaining a negative electrode.

[0073] Isolation film

[0074] In order to prevent short circuit, a separator is provided between the positive electrode and the negative electrode of this embodiment, and the electrolyte is used by infiltrating the separator.

[0075] This embodiment has no particular restrictions on the material and shape of the isolation membrane, as long as it does not significantly impair the effect of the present application. For example, in some embodiments, the isolation membrane may be a resin, glass fiber, inorganic material, etc. formed by a material that is stable to the electrolyte of the present application. In some embodiments, the isolation membrane includes a porous sheet or a non-woven fabric-like material with excellent liquid retention. Examples of materials for resin or glass fiber isolation membranes may include, but are not limited to, polyolefins, aromatic polyamides, polytetrafluoroethylene, polyether sulfone, etc. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The materials of the above isolation membranes can be used alone or in any combination.

[0076] Illustratively, in some embodiments, the isolation film may also be a material formed by laminating the above materials, examples of which include, but are not limited to, a three-layer isolation film formed by laminating polypropylene, polyethylene, and polypropylene in this order.

[0077] For example, in some embodiments, examples of inorganic materials in the isolation film may include, but are not limited to, oxides such as aluminum oxide and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates (e.g., barium sulfate, calcium sulfate, etc.). The form of the inorganic material may include, but is not limited to, granular or fibrous.

[0078] Exemplarily, in some embodiments, the separator may be in the form of a thin film, examples of which include, but are not limited to, nonwoven fabrics, woven fabrics, microporous films, and the like. In the thin film form, the separator has a pore size of 0.01 μm to 1 μm and a thickness of 5 μm to 50 μm. In addition to the above-mentioned independent thin film separators, the following separators may also be used: a separator formed by forming a composite porous layer containing the above-mentioned inorganic particles on the surface of the positive electrode and / or the negative electrode using a resin-based adhesive, for example, a separator formed by using a fluororesin as an adhesive to form a porous layer on both sides of the positive electrode with 90% of the aluminum oxide particles having a particle size less than 1 μm.

[0079] The thickness of the isolation film of the present application is arbitrary, as long as it does not significantly damage the effect of the present application. For example, in some embodiments, the thickness of the isolation film is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the isolation film is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the isolation film is within the above range, the insulation and mechanical strength can be ensured, and the DC resistance characteristics and energy density of the secondary battery can be ensured.

[0080] Electronic Devices

[0081] A second aspect of the embodiments of the present application provides an electronic device, which includes the secondary battery described in the present application.

[0082] The use of the secondary battery of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the secondary battery of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.

[0083] The preparation of the secondary battery is described below in conjunction with specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.

[0084] (I) Preparation of secondary batteries

[0085] <Production of positive electrode>

[0086] Method 1: Inorganic additives are included in the positive electrode active material layer

[0087] The positive electrode active material in Table 1-1: 97 mass%, the inorganic additive in Table 1-1: 0.5 mass%, and acetylene black: 1.0 mass% are mixed, and added to a solution obtained by dissolving the binder and dispersant in Table 1-1: 1.5 mass% (if there is no dispersant, the binder is 1.5 mass%. If there is a dispersant, the binder is 1.2 mass% and the dispersant is 0.3 mass%) in 1-methyl-2-pyrrolidone in advance and mixed to prepare a positive electrode slurry. The positive electrode slurry is applied on both sides of an aluminum foil, dried, pressurized, and cut into a specified size to make a positive electrode.

[0088] Method 2: Inorganic additives are included in the base coat

[0089] Mix 65 mass % of the inorganic additive in Table 1-1, 20 mass % of acetylene black, and 15 mass % of the binder and dispersant in Table 1-1 (if there is no dispersant, the binder is 15 mass %. If there is a dispersant, adjust it to: 12 mass % of the binder in Table 1-1, 3 mass % of the dispersant in Table 1-1), add deionized water and mix evenly, make a slurry, apply it on both sides of the aluminum foil, dry it, and form a primer layer.

[0090] Mix the positive electrode active material in Table 1-1: 97 mass % and acetylene black: 1.5 mass %, add to the solution obtained by dissolving the binder and dispersant in Table 1-1: 1.5 mass % (if there is no dispersant, the binder is 1.5 mass %. If there is a dispersant, the binder is 1.2 mass % and the dispersant is 0.3 mass %) in 1-methyl-2-pyrrolidone in advance, and mix to prepare a positive electrode slurry. Apply the positive electrode slurry on the surface of the primer layer, dry and pressurize it, and then cut it into a specified size to make a positive electrode. Method three: Inorganic additives are included in the edge layer

[0091] Mix 65 mass % of the inorganic additive in Table 1-1, 20 mass % of acetylene black, and 15 mass % of the binder and dispersant in Table 1-1 (if there is no dispersant, the binder is 15 mass %. If there is a dispersant, adjust it to: 12 mass % of the binder in Table 1-1, 3 mass % of the dispersant in Table 1-1), add deionized water and mix evenly to make positive electrode slurry 1, apply it on the edge of the aluminum foil with the pole ear side, dry it, and form an edge layer.

[0092] The positive electrode active material in Table 1-1: 97 mass % and acetylene black: 1.5 mass % are mixed, and added to the solution obtained by dissolving the binder and dispersant in Table 1-1: 1.5 mass % (if there is no dispersant, the binder is 1.5 mass %. If there is a dispersant, the binder is 1.2 mass % and the dispersant is 0.3 mass %) in 1-methyl-2-pyrrolidone in advance, and mixed to prepare positive electrode slurry 2. The positive electrode slurry is applied on both sides of an aluminum foil, dried, pressurized, and cut into a specified size to make a positive electrode. Among them, slurry 1 and slurry 2 are applied on the aluminum foil in parallel, and slurry 1 is located at an outer edge of slurry 2 (along the running direction of coating).

[0093] <Production of negative electrode>

[0094] The negative electrode active material artificial graphite and silicon carbon (mass ratio 90:10): 96 mass%, styrene butadiene rubber: 2 mass% are mixed, added to a solution obtained by dissolving 2 mass% of lithium carboxymethyl cellulose in deionized water in advance and mixed to prepare a negative electrode mixture paste. The negative electrode mixture paste is applied to one side of a copper foil (current collector), dried, pressurized, and then cut into a specified size to make a negative electrode.

[0095] <Preparation of Electrolyte>

[0096] The electrolyte was prepared by dissolving LiPF6 as a supporting electrolyte in a solution containing: (I) fluoroethylene carbonate (II) nitrogen-containing lithium salt (III) propyl propionate and ethylene carbonate and propylene carbonate (mass ratio 1:1). Based on 100 parts by mass of the total mass of the non-aqueous electrolyte: the parameters of fluoroethylene carbonate, nitrogen-containing lithium salt and propyl propionate, and other additives are shown in Table 1-2, and the content of LiPF6 is 12%.

[0097] <Production of Secondary Battery>

[0098] The positive electrode and negative electrode prepared as above were connected to a lead wire respectively. The layers were stacked via a polypropylene porous film having a thickness of 10 μm. The stack was then placed in an aluminum laminated housing together with 3.2 g of electrolyte. The opening of the housing was heat-sealed, and a secondary battery was prepared by steps such as formation and capacity.

[0099] Table 1-1 shows the raw material components and contents of the positive electrodes used in the examples and comparative examples of the present application, and Table 1-2 shows the components and contents of the electrolytes used in the examples and comparative examples of the present application. The electrolyte prepared with the preparation parameters of the electrolyte numbered 1-35 in the above steps is matched with the prepared positive electrodes, and secondary batteries are made respectively to obtain Examples 1-29, Comparative Examples 1-8, Examples 2-29, Comparative Examples 2-8, Examples 3-29 and Comparative Examples 3-8. Then, the following test methods are used to respectively carry out the lithium ion acceptance test of the secondary battery at low temperature, the initial resistance test of the secondary battery at low temperature, and the resistance test of the secondary battery after high temperature storage. The test results are shown in Tables 2-1, 2-2 and 2-3 below.

[0100] (II) Test methods

[0101] (1) Lithium ion acceptance test of secondary batteries at low temperatures

[0102] After the secondary battery is allowed to stand for 24 hours at 25°C, it is charged at a constant current of 1.0C for 1 hour at 25°C to measure the normal temperature charge capacity (C0). Then, at 25°C, the discharge is stopped at a constant current of 0.1C until it reaches 3V. Next, at -20°C, the charge is performed at a constant current of 1.0C for 1 hour to measure the low temperature charge capacity (C1). Then, the ratio of C1 to C0 (C1 / C0) is calculated and evaluated according to the following criteria. The larger the value of C1 / C0, the better the lithium ion acceptance of the secondary battery at low temperatures.

[0103] A: C1 / C0 is 0.65 or more and 1 or less.

[0104] B: C1 / C0 is 0.5 or more and less than 0.65.

[0105] C: C1 / C0 is less than 0.5.

[0106] (2) Low temperature initial resistance test of secondary batteries

[0107] After the secondary battery is left to stand for 24 hours at 25°C, it is charged at 4.6V and 0.2C and discharged to 3.0V at 0.2C. Then, it is charged at 4.6V and 0.2C at -20°C, and the voltage V0 at this time is measured. Then, the discharge operation is performed at an initial discharge resistance of 1C at -20°C, and the voltage V1 is measured 10 seconds after the start of discharge. The resistance characteristics are evaluated by the voltage change represented by ΔV=V0-V1. The smaller the value of ΔV, the better the resistance characteristics of the secondary battery, and the more the increase in the initial resistance at low temperature is suppressed.

[0108] A: 10<ΔV(mV)≤12.

[0109] B: 12<ΔV(mV)≤15.

[0110] C: 15<ΔV(mV)≤20.

[0111] D: 20<ΔV(mV).

[0112] (3) Resistance test of secondary batteries after high temperature storage

[0113] The manufactured secondary battery is charged at a constant current of 0.2CmA at 25°C until the battery voltage becomes 4.6V, and then charged at a constant voltage of 4.6V until the charging current becomes 0.02C. Next, the constant current discharge is performed at 0.2C until the battery voltage becomes 3.0V. The capacity at the end of the constant current discharge is set as the initial capacity. Then, at 25°C, the battery voltage is charged to 3.82V according to the constant current method of 0.2C, and left in this state for 5 hours, and the voltage Vini0 is measured. Furthermore, a 3C discharge operation is performed, and the voltage Vini20 is measured 20 seconds after the start of the discharge. The voltage change shown by ΔVini=Vini0-Vini20 defines the resistance before high-temperature storage.

[0114] After the above measurement, the secondary battery was charged at a constant current of 0.2 C until the battery voltage reached 4.6 V. Then, after being stored in a thermostatic chamber at 60° C. for 20 days, it was discharged at a constant current of 0.2 C until the battery voltage reached 3.0 V in an environment of 25° C.

[0115] Next, the battery was charged at 25°C and 0.1C constant current method until the battery voltage reached 4.6V, and left in this state for 5 hours, and the voltage Vfin0 was measured. Furthermore, a 3C discharge operation was performed, and the voltage Vfin20 was measured 20 seconds after the start of discharge. The resistance after high temperature storage was defined as the voltage change shown by ΔVfin=Vfin0-Vfin20.

[0116] Then, the value calculated from ΔVfin / ΔVini×100(%) was regarded as the resistance increase rate after high-temperature storage, and was evaluated according to the following criteria: The smaller the value of the resistance increase rate, the better the resistance increase was suppressed after high-temperature storage.

[0117] A: The resistance increase rate is less than 120%.

[0118] B: The resistance increase rate is 120% or more and less than 130%.

[0119] C: The resistance increase rate is 130% or more and less than 140%.

[0120] D: The resistance increase rate is 140% or more.

[0121] Table 1-1 Positive electrode

[0122]

[0123]

[0124] *The values ​​in the above table are all in mass %. The abbreviations are as follows: PVDF: polyvinylidene fluoride, PAN: polyacrylonitrile, PAA: polyacrylic acid, A1: dioctyl sulfosuccinate sodium salt, A2: dipentyl sulfosuccinate sodium salt, A3: dicyclopentyl sulfosuccinate sodium salt, A4: dioctyl sulfosuccinate potassium salt, A5: dipentyl sulfosuccinate ammonium salt.

[0125] Table 1-2 Electrolyte

[0126]

[0127]

[0128] *In the above table, (I) is fluoroethylene carbonate, (II) is nitrogen-containing lithium salt, and (III) is propyl propionate. The values ​​in () are all mass %, (I) is fluoroethylene carbonate, (II) is nitrogen-containing lithium salt, and (III) is propyl propionate. The corresponding abbreviations and numbers of the remaining items are: FEC: fluoroethylene carbonate, PP: propyl propionate N1: LiN(FSO2)2, N2: LiN(FSO2)(CF3SO2), N3: LiN(CF3SO2)2, N4: LiN(FCO)(FSO2), N5: LiN(C2F5SO2)2, N6: LiN(FCO)2, N7: LiN(CF3SO2) (C4F9SO2), N8: 4,5-dicyano-2-trifluoromethylimidazole lithium salt, N9: 2,4,5-tricyanoimidazole lithium salt, N10: 2,5,6-tricyanobenzimidazole lithium salt, C1: succinonitrile, C2: adiponitrile, C3: 1,3,6-hexanetricarboxylic acid nitrile, C4: 1,2,3-tris(2-cyanoethoxy)propane, C5: vinyl sulfate, C6: compound of formula 1, C7: compound of formula 2.

[0129] Table 2-1

[0130]

[0131]

[0132] Table 2-2

[0133]

[0134]

[0135] Table 2-3

[0136]

[0137]

[0138] Results Analysis

[0139] It can be seen from Tables 2-1, 2-2 and 2-3 above that the positive electrode includes a lithium composite metal oxide, a binder and any inorganic additive containing aluminum, magnesium, titanium, zirconium, niobium, indium, tungsten, tin, zinc or antimony. The total content of fluoroethylene carbonate and nitrogen-containing lithium salt in the electrolyte is within the specific range provided in the present application, and when the electrolyte contains a specific content of fluoroethylene carbonate, nitrogen-containing lithium salt and propyl propionate, the lithium ion acceptance of the secondary battery at low temperature (ambient temperature below -20°C) can be improved, and the initial resistance increase at low temperature can be suppressed, thereby improving the low temperature performance of the secondary battery, and taking into account the improvement of the high temperature performance of the secondary battery, especially suppressing the resistance increase of the secondary battery after storage at high temperature (ambient temperature greater than 45°C).

[0140] In particular, the total content of fluoroethylene carbonate and nitrogen-containing lithium salt and the content of propyl propionate in the electrolyte are within the preferred range provided in the present application, which can significantly improve the lithium ion acceptance of the secondary battery at low temperatures, inhibit its initial resistance increase at low temperatures, and thus improve the low temperature performance of the secondary battery, while taking into account the improvement of the high temperature performance of the secondary battery, especially inhibiting the resistance increase of the secondary battery after high-temperature storage.

[0141] In particular, adding other additives to the electrolyte can improve the stability of the film formed on the surface of the positive electrode material by the propionate compounds in the inorganic additive-catalyzed electrolyte at high temperatures, and increase the ion conduction rate of lithium ions, thereby further improving the resistance characteristics after high-temperature storage.

[0142] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.

Claims

1. A secondary battery, characterized in that: The secondary battery comprises a positive electrode, a negative electrode and an electrolyte; The positive electrode comprises a lithium composite metal oxide, a binder and an inorganic additive, wherein the metal element in the inorganic additive comprises at least one of aluminum, magnesium, titanium, zirconium, niobium, indium, tungsten, tin, zinc or antimony; The electrolyte contains fluoroethylene carbonate, nitrogen-containing lithium salt and propyl propionate. Based on the mass of the electrolyte, the sum of the mass percentages of the fluoroethylene carbonate and the nitrogen-containing lithium salt is greater than 0.76 mass% and less than 10.17 mass%, and the mass percentage of the propyl propionate is greater than 12 mass% and less than 65 mass%.

2. The secondary battery according to claim 1, characterized in that: The sum of the mass percentages of the fluoroethylene carbonate and the nitrogen-containing lithium salt is greater than or equal to 4.89 mass % and less than or equal to 10.17 mass %.

3. The secondary battery according to claim 1, characterized in that: The mass percentage content of the propyl propionate is greater than or equal to 22 mass % and less than or equal to 47 mass %.

4. The secondary battery according to claim 1, characterized in that: The binder includes at least one of polyvinylidene fluoride, polyacrylonitrile and polyacrylic acid.

5. The secondary battery according to claim 1, characterized in that: The positive electrode further contains a dispersant, and the dispersant includes at least one of sodium salt, potassium salt and ammonium salt of dioctyl sulfosuccinate, dipentyl sulfosuccinate and dicyclopentyl sulfosuccinate.

6. The secondary battery according to any one of claims 1 to 4, characterized in that: The nitrogen-containing lithium salt is selected from LiN(FCO)2, LiN(FCO)(FSO2), LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,2-perfluoroethane disulfonyl imide lithium, cyclic 1,3-perfluoropropane disulfonyl imide lithium, LiN(CF3SO2)(C4F9SO2), 4,5-dicyano-2-trifluoromethyl imidazole lithium salt, 4,5-dicyano-2-pentafluoroethyl imidazole lithium salt, 2,4,5-tricyanoimidazole At least one of lithium salt, 5,6-dicyano-2-trifluoromethylbenzimidazole lithium salt, 5,6-dicyano-2-pentafluoroethylbenzimidazole lithium salt, 2,5,6-tricyanobenzimidazole lithium salt, 4,7-dicyano-2-trifluoromethylbenzimidazole lithium salt, 4,7-dicyano-2-pentafluoroethylbenzimidazole lithium salt, 2,4,7-tricyanobenzimidazole lithium salt, 4,5,6,7-tetracyano-2-trifluoromethylbenzimidazole lithium salt, 4,5,6,7-tetracyano-2-pentafluoroethylbenzimidazole lithium salt or 2,4,5,6,7-pentacyanobenzimidazole lithium salt.

7. The secondary battery according to any one of claims 1 to 4, characterized in that: Based on the mass of the electrolyte, the mass percentage of the fluoroethylene carbonate is greater than 0.53 mass % and less than 8.95 mass %, or the mass percentage of the nitrogen-containing lithium salt is greater than 0.23 mass % and less than 3.45 mass %, or the mass percentage of the propyl propionate is greater than 24 mass % and less than 39 mass %.

8. The secondary battery according to any one of claims 1 to 4, characterized in that: The electrolyte includes other additives, and the other additives include at least one of 1,2-bis(difluorophosphine)ethane, a compound of formula 1, a compound of formula 2, vinylene carbonate, lithium fluorosulfonate, succinonitrile, adiponitrile, 1,3,6-hexanetricarboxylate, 1,2,3-tris(2-cyanoethoxy)propane, vinyl sulfate, fluorobenzene, cyclohexylbenzene, biphenyl, tris(trimethylsilyl)phosphate or tris(trimethylsilyl)borate; 9. The secondary battery according to any one of claims 1 to 4, characterized in that: The lithium composite metal oxide contains a first element, wherein the first element includes at least one of lanthanum, yttrium, cerium, tungsten or strontium; A mass percentage content of any one of the first elements is 0.01 mass % or more and 1 mass % or less based on the mass of the lithium mixed metal oxide.

10. The secondary battery according to any one of claims 1 to 4, characterized in that: The positive electrode includes a primer layer and an active material layer disposed on a current collector, and the inorganic additive is contained in the active material layer and / or the primer layer.

11. The secondary battery according to any one of claims 1 to 4, characterized in that: The positive electrode includes an edge layer and an active material layer disposed on a current collector, and the inorganic additive is contained in the edge layer. 12 . An electronic device comprising the secondary battery according to claim 1 .

Citation Information

Cited By

  • Secondary battery and electronic apparatus

    WO2025256204A1