Semi-solid electrolyte precursor solution as well as preparation method and application thereof
By using a semi-solid electrolyte precursor copolymerized with ether monomers and fluorinated high-pressure solvents in lithium-ion batteries, the potential safety hazards and energy density bottlenecks of lithium-ion batteries are solved, and high room temperature ionic conductivity and electrochemical stability are achieved. and thermal stability, improving the overall performance and safety of the battery.
Patent Information
- Application Number
- CN202410720316.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-15
AI Technical Summary
Existing lithium-ion batteries have safety hazards and energy density bottlenecks, especially in the field of electric vehicles. The semi-solid electrolyte has low room temperature ionic conductivity, poor electrochemical stability, poor electrode/electrolyte compatibility, and the proportion of solid phase is too low. , it is difficult to meet the requirements of high safety and high energy density.
A semi-solid electrolyte precursor is used to form a macromolecular network structure through the copolymerization of the first ether monomer and the second ether monomer, and is compounded with a fluorinated high-pressure solvent. The semi-solid electrolyte is prepared through an in-situ curing process to ensure that the electrolyte Uniform contact and high voltage stability within the battery improve overall performance.
It significantly improves the room temperature ion conductivity, electrochemical stability and thermal stability of semi-solid batteries, improves the safety performance and energy density of the battery, and ensures efficient electrochemical performance and safety performance.
Smart Images

Figure CN118782895A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state lithium batteries, and specifically relates to a semi-solid electrolyte precursor solution and a preparation method and application thereof, and in particular to a semi-solid electrolyte and a semi-solid battery prepared based on an in-situ curing process. Background Art
[0002] Since its introduction, lithium-ion batteries have been widely used in consumer electronics and electric vehicles. Lithium-ion batteries contain a large amount of low-boiling organic solvents, which are extremely easy to burn or even explode when exposed to heat, making them carry a large safety hazard. In addition, the energy density of lithium-ion batteries based on traditional positive and negative electrode materials has reached a bottleneck, and it is difficult to exceed 300Wh / kg at a practical level. Especially in the field of electric vehicles, safety risks and low mileage have become the two main factors that hinder people from buying electric vehicles.
[0003] Based on the problems existing in the above-mentioned lithium-ion batteries, solidification of the electrolyte is considered to be the ultimate direction for solving the problem. Compared with inorganic solid electrolyte materials, organic polymer materials have the advantages of flexibility, easy processing, good interface contact, and low cost, and are currently a good choice for practical solid-state batteries. Among them, organic ether materials, in addition to the above-mentioned advantages, also have the characteristics of high compatibility with alkali metals and strong dissociation of the main chain to lithium salts, and have received extensive attention from the scientific community in recent years. In order to achieve a breakthrough in the application of ether-based materials in practical solid-state batteries, it is also necessary to solve the defects of limited room temperature ionic conductivity, poor high-voltage stability, and low thermal stability. For example, the results published by CN112701348B show that the invention improves the room temperature ionic conductivity to a certain extent by cross-linking, but it is still far from the practical level. The room temperature cycle performance of the polymer-based all-solid-state battery assembled therein can only be stably cycled for about 60 cycles, and it cannot adapt to high-voltage positive electrode materials. After assembling the battery, the energy density may even be much lower than that of a mature liquid system. By making an appropriate compromise between the polymer and the organic solvent, the performance of all aspects can be improved. By plasticizing the polymer chain segments with solvents and increasing the free volume, the room temperature ionic conductivity can be significantly improved, thereby improving the overall electrochemical performance of the battery. Since the overall solid-state characteristics are still maintained, the thermal stability can still be guaranteed. It should be pointed out that the amount of polymer and the amount of organic solvent need to be reasonably designed, and too high an amount of organic solvent deviates from the original intention of the solid state. For example, in CN117304467B, although the fluorinated semi-solid electrolyte design significantly improves the electrochemical performance, the amount of organic solvent reaches more than 90% by mass, which is obviously an unhealthy liquid phase ratio. In the case of thermal runaway, the safety performance is difficult to have a significant advantage over the pure liquid state.
[0004] Based on this, there is an urgent need to develop a semi-solid electrolyte with a high solid phase ratio, high room temperature ionic conductivity, and high electrochemical stability to meet the battery's requirements for high safety and high energy density. Summary of the invention
[0005] In order to solve one or more problems of semi-solid-state batteries, such as low polymer phase ionic conductivity, poor electrochemical stability, poor electrode / electrolyte compatibility, and too low solid phase ratio, the present invention provides a semi-solid electrolyte precursor solution and a preparation method and application thereof.
[0006] On the one hand, the present invention provides a semi-solid electrolyte precursor solution, comprising: a first ether monomer, a second ether monomer, a first plasticizer, a second plasticizer, a first lithium salt and a second lithium salt; the first ether monomer is a cyclic ether monomer, preferably at least one of 1,3-dioxolane (DOL), 1,3-dioxane (DOX), tetrahydrofuran (THF), and trioxymethylene (TXE), more preferably 1,3-dioxolane; the second ether monomer is an epoxy ether monomer, preferably comprising at least one of propylene triglycidyl ether (GTE), ethylene glycol diglycidyl ether (EGDE), and polyethylene glycol diglycidyl ether (PEGDE).
[0007] In the present invention, the macromolecular network structure formed by copolymerization of the first ether monomer and the second ether monomer has the advantages of high intrinsic ionic conductivity and high electrochemical stability. The advantage of GTE in the present invention is that DOL-GTE copolymerization is superior to simple DOL polymerization.
[0008] Preferably, based on the total volume of the semi-solid electrolyte precursor solution as 100 vol%, the content of the first ether monomer is 25-49 vol%; based on the total volume of the semi-solid electrolyte precursor solution as 100 vol%, the content of the second ether monomer is 1-25 vol%; preferably, the total volume of the first ether monomer and the second ether monomer accounts for ≥ 40 vol% of the total volume of the precursor solution.
[0009] Furthermore, preferably, the volume ratio of the first ether monomer to the second ether monomer is 50:50 to 98:2, and preferably 60:40 to 90:10.
[0010] Preferably, the first plasticizer is at least one of 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether (HFE), 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether, and bis(2,2,2-trifluoroethyl) ether, preferably HFE; the second plasticizer is at least one of fluoroethylene carbonate (FEC), methyl trifluoroethyl carbonate (FEMC), ethyl trifluoroethyl carbonate (FDEC), 2,2,2-trifluoro-N,N-dimethylacetamide (FDMA), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethylene carbonate (EC), propylene carbonate (PC), and ethylene glycol dimethyl ether (DME), preferably a binary mixture of FEC and EMC. In the present invention, the plasticizer solvent phase (first / second plasticizer) is mainly composed of a fluorinated high-pressure solvent, which can improve the system's ionic conductivity and high-pressure resistance while increasing the system's ionic conductivity. The volume ratio does not exceed 60% of the total volume of the precursor solution.
[0011] Preferably, based on the total volume of the semi-solid electrolyte precursor solution as 100 vol%, the content of the first plasticizer is 5 to 25 vol%; based on the total volume of the semi-solid electrolyte precursor solution as 100 vol%, the content of the second plasticizer is 25 to 45 vol%; preferably, the total volume of the first plasticizer and the second plasticizer does not exceed 60 vol% of the total volume of the precursor solution.
[0012] In addition, preferably, the volume ratio of the first plasticizer to the second plasticizer is 10:90 to 50:50, preferably 15:85 to 45:55. As for the content of the first plasticizer (HFE), since the first plasticizer is an inert solvent, it only improves the window but does not improve the ionic conductivity. Generally, it is controlled within a specific small range. Too high or too low will result in two extremes of no improvement in the window and very low ionic conductivity.
[0013] Preferably, the ratio of the total volume of the first ether monomer and the second ether monomer to the total volume of the first plasticizer and the second plasticizer is 30:70 to 70:30, preferably 40:60 to 60:40.
[0014] Preferably, the first lithium salt is at least one of lithium bis(trifluoromethanesulfonyl imide) (LiTFSI), lithium bis(pentafluoroethylsulfonyl imide) (LiPFSI), and lithium trifluoromethanesulfonate (LiOTF), preferably lithium bis(trifluoromethanesulfonyl imide) (LiTFSI); the concentration of the first lithium salt in the semi-solid electrolyte precursor solution is 0.5-3 mol / L, preferably 0.8-2 mol / L.
[0015] Preferably, the second lithium salt is at least one of lithium difluorooxalatoborate (LiDFOB), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), and lithium bis(fluorosulfonyl)imide (LiFSI), preferably a binary mixture of LiDFOB and LiBF4, more preferably a molar ratio of LiDFOB to LiBF4 of (3-5):1; The concentration of the second lithium salt in the semi-solid electrolyte precursor solution is 0.05-1 mol / L, preferably 0.1-0.6 mol / L.
[0016] In a second aspect, the present invention provides a method for preparing a semi-solid electrolyte, comprising: subjecting a semi-solid electrolyte precursor solution to in-situ curing to obtain the semi-solid electrolyte; preferably, the in-situ curing temperature is 25 to 80° C., preferably 30 to 60° C. Under certain conditions, the first monomer and the second monomer copolymerize to form a network structure, so that a semi-solid electrolyte without fluidity is formed as a whole.
[0017] In a third aspect, the present invention provides a semi-solid electrolyte prepared according to the above preparation method.
[0018] In a fourth aspect, the present invention provides a semi-solid-state battery, characterized in that it comprises: a semi-solid-state electrolyte.
[0019] Preferably, it also includes: a positive electrode, a separator and a negative electrode.
[0020] Preferably, the structure of the semi-solid battery includes, in sequence: positive electrode / semi-solid electrolyte / diaphragm / semi-solid electrolyte / negative electrode.
[0021] Preferably, the positive electrode comprises at least one of a lithium iron phosphate positive electrode (LFP), a nickel-cobalt-manganese ternary positive electrode (NCM), a lithium-rich manganese-based positive electrode, and a sulfur positive electrode; preferably, the positive electrode has a surface capacity of 0.5 to 5 mAh / cm 2 , preferably 3 to 4 mAh / cm 2 ; The diaphragm comprises at least one of a polyolefin diaphragm and a glass fiber diaphragm; The negative electrode lithium comprises at least one of a negative electrode, a graphite negative electrode, a hard carbon negative electrode, a silicon-carbon negative electrode, and a silicon negative electrode; preferably, the negative electrode surface capacity is 2 to 20 mAh / cm 2 , preferably 4 to 10 mAh / cm 2 .
[0022] In a fifth aspect, the present invention provides a method for preparing a semi-solid-state battery, comprising: injecting the semi-solid electrolyte precursor solution into a component comprising a positive electrode, a negative electrode, and a separator, and then in-situ curing to obtain the semi-solid-state battery; Preferably, the injection amount of the semi-solid electrolyte precursor solution is 1 to 4 g / Ah, preferably 1 to 2 g / Ah; Preferably, the in-situ curing temperature is 25 to 80°C, preferably 30 to 60°C; Preferably, the in-situ curing time may be 1 to 48 hours, preferably 6 to 36 hours.
[0023] The present invention achieves uniform and close contact of the electrolyte at various interfaces in the battery through an in-situ curing process, and ultimately improves various aspects of the performance of the semi-solid battery.
[0024] Compared with the prior art, the present invention can achieve the following beneficial effects: The present invention effectively improves the ionic conductivity and high-voltage stability of the ether-based polymer by cross-linking copolymerization, and further improves the ionic conductivity and high-voltage stability by compounding with a high-pressure resistant fluorinated solvent. It is injected into a battery and in-situ cured by an initiator, thereby achieving uniform and dense filling of the pores and interfaces of the electrode with a semi-solid electrolyte, thereby ensuring stable and efficient performance of the semi-solid battery. The network structure of the cross-linked polymer can effectively adsorb and fix small molecules of the plasticizer, maintaining the overall hard elastic texture, so that the electrolyte as a whole has good thermal stability, and the safety performance of the semi-solid battery can be effectively improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A schematic diagram of a semi-solid-state battery formed by solidifying the semi-solid-state electrolyte in the battery of the present invention; Figure 2 These are photos of the precursor solution of Example 4 before and after curing; Figure 3 This is a comparison diagram of conductivity impedance after curing of Example 4 and Comparative Example 1; Figure 4 This is a comparison diagram of the electrochemical windows after curing of Example 4, Comparative Example 1 and Comparative Example 2; Figure 5 This is a graph of the cycle performance of a semi-solid-state battery based on an LFP positive electrode, a polypropylene separator, and a lithium negative electrode in Example 4; Figure 6 These are photos of the semi-solid electrolyte of Example 4 before and after being heated at 110°C for 5 minutes; Figure 7 This is a picture of a small soft-pack battery prepared in Example 6; Figure 8 The figure is a comparison of the physical states of the semi-solid electrolyte after solidification of Example 4 and Comparative Example 1. DETAILED DESCRIPTION
[0026] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0027] In the present invention, the semi-solid electrolyte polymer phase is an ether polymer, the plasticizer phase is a high-pressure component mainly composed of a fluorinated solvent, and the monomer accounts for no less than 40% by volume in the precursor solution. Specifically, the electrolyte precursor solution components include: a first monomer, a second monomer, a first plasticizer, a second plasticizer, a first lithium salt, and a second lithium salt. The preparation method of the electrolyte precursor solution includes: weighing the first lithium salt and the second lithium salt, adding the first plasticizer, the second plasticizer, the first monomer, and the second monomer in sequence, and stirring at room temperature until the lithium salt is completely dissolved.
[0028] In the present invention, the semi-solid electrolyte is composed of a polymer, a plasticizer, and a lithium salt, wherein the polymer is formed by in-situ copolymerization of an ether monomer and a cross-linking agent. Among them, the plasticizer is mainly composed of a composite fluorinated solvent, and the cross-linked ether-based polymer has the advantages of high lithium stability, high ionic conductivity, high electrochemical stability, high thermal stability, etc. The composite fluorinated solvent further improves the electrochemical stability and ionic conductivity. The specific preparation method includes: first weighing the first lithium salt and the second lithium salt in a container, adding the first plasticizer, the second plasticizer, the first monomer, and the second monomer in turn, stirring until the lithium salt is completely dissolved, and then under certain conditions, the first monomer and the second monomer copolymerize to form a network structure, so that the whole forms a semi-solid electrolyte without fluidity.
[0029] In the present invention, lithium salt, monomer and plasticizer are sequentially added into a container and stirred until the lithium salt is completely dissolved, and then injected into a basic component mainly composed of a positive electrode, a separator and a negative electrode, and left at room temperature. The precursor liquid will slowly infiltrate all pores of the electrode. At the same time, under the initiation of the second lithium salt, the first monomer and the second monomer will open the ring to copolymerize. Over time, the precursor liquid as a whole will slowly change from a liquid state to a hard elastic solid state without fluidity, that is, the construction of a semi-solid battery is completed. The cross-linking copolymerization improves the ionic conductivity and electrochemical stability of the polymer phase, and the fluorinated plasticizer further improves the overall ionic conductivity and electrochemical window. This combined effect will significantly improve the electrochemical performance of the battery. At the same time, a higher proportion of copolymers will also effectively improve the safety of the battery.
[0030] More specifically, the first monomer may be one or more cyclic ethers such as 1,3-dioxolane (DOL), 1,3-dioxane (DOX), tetrahydrofuran (THF), trioxymethylene (TXE), etc., preferably DOL. The function of the first monomer is to constitute a component of the long chain of the polymer network structure, and its function is to form a flexible framework. It should be pointed out that the first monomer does not only refer to the only monomer, but can also be composed of two or more mixed monomers. The criterion is whether a long chain structure can be formed after polymerization.
[0031] More specifically, the second monomer is glycerol triglycidyl ether (GTE). The role of the second monomer is to constitute the connection point of the polymer network structure. The presence of the connection point can disrupt the regular arrangement of the long-chain structure, inhibit crystallization, increase the free volume, improve the intrinsic ionic conductivity of the polymer, and reduce the hydroxyl end-capping at the same time, and improve the electrochemical stability. It should be pointed out that the second monomer in the present invention does not only refer to the only monomer, but can also be composed of two or more mixed monomers, and the criterion is whether the network connection point can be formed after polymerization. For example, two kinds of glycerol triglycidyl ether (GTE) and ethylene glycol diglycidyl ether (EGDE), or two kinds of glycerol triglycidyl ether (GTE) and polyethylene glycol diglycidyl ether (PEGDE).
[0032] More specifically, the first plasticizer can be one or more of 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether (HFE), 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether, and bis(2,2,2-trifluoroethyl) ether, preferably HFE. The first plasticizer mainly plays a role in improving the high pressure window, and has no dissociation effect on the lithium salt, so the added amount should not be too high, generally not more than 50% of the total plasticizer volume.
[0033] More specifically, the second plasticizer can be one or more of fluoroethylene carbonate (FEC), methyl trifluoroethyl carbonate (FEMC), ethyl trifluoroethyl carbonate (FDEC), 2,2,2-trifluoro-N,N-dimethylacetamide (FDMA), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethylene carbonate (EC), propylene carbonate (PC), and ethylene glycol dimethyl ether (DME), preferably a binary mixture of FEC and EMC. The second plasticizer mainly dissociates lithium salts, increases the free volume of the polymer, and improves the overall ionic conductivity. It preferably contains a portion of fluorinated solvents and a portion of non-fluorinated solvents. The high pressure window of the fluorinated solvent is higher than that of the non-fluorinated solvent, and the non-fluorinated solvent has a higher dissociation effect on the lithium salt than the fluorinated solvent, so the combination of the two is preferred.
[0034] More specifically, the first lithium salt may be one or more of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(pentafluoroethylsulfonyl)imide (LiPFSI), and lithium trifluoromethanesulfonate (LiOTF), preferably LiTFSI. The first lithium salt has a high degree of dissociation in the solvent and does not participate in the polymerization reaction. It is the main source of lithium ions and is an important guarantee for the semi-solid electrolyte to have high ionic conductivity.
[0035] More specifically, the second lithium salt may be one or more of lithium difluorooxalatoborate (LiDFOB), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), and lithium bis(fluorosulfonyl)imide (LiFSI), preferably a binary mixture of LiDFOB and LiBF4. On the one hand, the second lithium salt provides a portion of lithium ions like the first lithium salt, but the dissociation degree of the second lithium salt is weaker than that of the first lithium salt. Another function of the second lithium salt is to act as an initiator, which can dissociate and form Lewis acidic groups with catalytic activity, initiate the polymerization reaction, and form a semi-solid electrolyte. For example, LiBF4 can dissociate into BF3, which reacts with trace amounts of water to form catalytically active H + (BF3) - , which in turn triggers the ring-opening polymerization of DOL.
[0036] More specifically, the components of the precursor solution have the following proportions: the first ether monomer 25-49% volume ratio (liquid phase); the second ether monomer 1-25% volume ratio (liquid phase); the first plasticizer 5-25% volume ratio (liquid phase); the second plasticizer 25-45% volume ratio (liquid phase); the first lithium salt 0.5-3 mol / L; the second lithium salt 0.05-1 mol / L.
[0037] The volume ratio of the first ether monomer (referred to as the first monomer) in the monomer is not lower than that of the second ether monomer (referred to as the second monomer), the volume ratio of the first plasticizer in the liquid phase is not higher than that of the second plasticizer, the volume ratio of the total monomer in the liquid phase is approximately the same as the volume of the plasticizer, the volume ratio of the first monomer to the second monomer is 50:50 to 98:2, preferably 60:40 to 90:10, the volume ratio of the first plasticizer to the second plasticizer is 10:90 to 50:50, preferably 15:85 to 45:55, and the total volume ratio of the monomers to the plasticizers is 30:70 to 70:30, preferably 40:60 to 60:40.
[0038] In the present invention, the semi-solid battery may be mainly composed of a positive electrode, a separator, a negative electrode, and a semi-solid electrolyte. The positive electrode may be one or more of a lithium iron phosphate positive electrode (LFP), a nickel-cobalt-manganese ternary positive electrode (NCM), a lithium-rich manganese-based positive electrode, and a sulfur positive electrode, preferably an LFP positive electrode or an NCM positive electrode. The positive electrode surface capacity may be 0.5-5 mAh / cm 2 , preferably 3-4 mAh / cm 2 The separator is a polyolefin separator or a glass fiber separator, preferably a polyolefin separator. The negative electrode can be one or more of a lithium negative electrode, a graphite negative electrode, a hard carbon negative electrode, a silicon carbon negative electrode, and a silicon negative electrode, preferably a lithium negative electrode. The negative electrode surface capacity can be 2-10 mAh / cm 2 , preferably 4-8 mAh / cm 2 .
[0039] The semi-solid battery provided by the present invention is prepared by in-situ curing. The formation of the semi-solid electrolyte can occur after the precursor solution is injected into the battery and completely infiltrates the pores, and the electrolyte can fully infiltrate the pores. The present invention ensures that the interfaces inside the battery are in close and stable contact through the in-situ curing process, thereby obtaining a highly safe and high-performance semi-solid battery.
[0040] In the present invention, the curing temperature of the semi-solid battery or the semi-solid electrolyte may be 25-80° C., preferably 30-60° C. The curing time may be 1-48 hours, preferably 6-36 hours.
[0041] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0042] Example 1 The precursor solution is prepared according to the parameters in Table 1 below.
[0043] In an argon glove box, based on 1 ml of liquid, weigh 1 M-LiTFSI and 0.5 M-LiBF4, add a magnet, and use a high-precision pipette to add 0.4 ml-DOL, 0.1 ml-GTE, 0.2 ml-HFE, and 0.3 ml-FEC in sequence, that is, the volume ratio of monomer to plasticizer is 1:1. Stir at room temperature until the lithium salt is completely dissolved, the process takes about 1-2 hours, and an electrolyte precursor solution is obtained.
[0044] The precursor solution was injected into the CR2025 button cell with an injection volume of 50 μl. Regarding the injection volume, it should be pointed out that due to the large inactive space inside the button cell, in addition to being adsorbed into the pores of the diaphragm and the electrode, a large part of the precursor solution is in the free space. Therefore, there is no accurate g / Ah injection coefficient. The injection volume of the button cell can be the conventional injection volume. The positive electrode in the battery has a surface capacity of 0.5 mAh / cm 2 The LFP electrode is Celgard2400 polypropylene diaphragm, and the negative electrode has a surface capacity of 10 mAh / cm 2 The lithium metal is packaged and the battery is placed at room temperature of 30°C for 30 hours to cure to obtain a semi-solid-state battery.
[0045] Example 2 The precursor solution is prepared according to the parameters in Table 1 below.
[0046] In an argon glove box, based on 1 ml of liquid, 1 M-LiTFSI and 0.5 M-LiBF4 were weighed, a magnet was added, and 0.4 ml-DOL, 0.1 ml-GTE, 0.2 ml-HFE, 0.2 ml-FEC, and 0.1 ml-EMC were added in sequence with a high-precision pipette. The volume ratio of the monomer to the plasticizer was 1:1. The mixture was stirred at room temperature until the lithium salt was completely dissolved. The process took about 30 minutes to obtain an electrolyte precursor solution. Compared with Example 1, the second plasticizer in Example 2 was designed as a binary solvent. The addition of a small amount of EMC can accelerate the dissolution of the lithium salt and improve the conductivity.
[0047] The precursor solution was injected into the CR2025 button battery. The injection volume was consistent with the conventional injection volume, which was 50 μl. The surface capacity of the positive electrode in the battery was 0.5 mAh / cm 2 The LFP electrode is Celgard2400 polypropylene diaphragm, and the negative electrode has a surface capacity of 10 mAh / cm 2 The lithium metal is packaged and the battery is placed at room temperature of 30°C for 30 hours to cure to obtain a semi-solid-state battery.
[0048] Example 3 The precursor solution is prepared according to the parameters in Table 1 below.
[0049] In an argon glove box, based on 1 ml of liquid, 1 M-LiTFSI, 0.5 M-LiBF4, and 0.1 M-LiDFOB were weighed, a magnet was added, and 0.4 ml-DOL, 0.1 ml-GTE, 0.2 ml-HFE, and 0.3 ml-FEC were added in sequence with a high-precision pipette. The volume ratio of the monomer to the plasticizer was 1:1. The mixture was stirred at room temperature until the lithium salt was completely dissolved. The process took about 30 minutes to obtain an electrolyte precursor solution. Compared with Example 1, Example 3 designed the second lithium salt as a binary lithium salt. LiDFOB can dissociate LiBF4 to become an initiator, but this process is slow and belongs to a weak initiation effect. In addition, the decomposition of LiDFOB at the positive electrode is more serious. However, LiDFOB can be used as an additive to participate in the positive electrode film formation and improve the positive electrode stability. At the same time, LiDFOB and LiBF4 can inhibit the decomposition of each other, and they are a pair of better lithium salt combinations.
[0050] The precursor solution was injected into the CR2025 button battery. The injection volume was consistent with the conventional injection volume, which was 50 μl. The surface capacity of the positive electrode in the battery was 0.5 mAh / cm 2 The LFP electrode is Celgard2400 polypropylene diaphragm, and the negative electrode has a surface capacity of 10 mAh / cm 2 The lithium metal is packaged and the battery is placed at room temperature of 30°C for 30 hours to cure to obtain a semi-solid-state battery.
[0051] Example 4 The precursor solution is prepared according to the parameters in Table 1 below.
[0052] In an argon glove box, based on 1 ml of liquid, 1 M-LiTFSI, 0.5 M-LiBF4, and 0.1 M-LiDFOB were weighed, a magnet was added, and 0.4 ml-DOL, 0.1 ml-GTE, 0.2 ml-HFE, 0.2 ml-FEC, and 0.1 ml-EMC were added in sequence with a high-precision pipette, the volume ratio of the monomer to the plasticizer was 1:1, and the mixture was stirred at room temperature until the lithium salt was completely dissolved. The process took about 30 minutes to obtain an electrolyte precursor solution. Compared with Examples 1, 2, and 3, Example 4 designed the second plasticizer as a binary solvent and the second lithium salt as a binary lithium salt. The addition of a small amount of EMC can promote the dissolution of the lithium salt and improve the conductivity. The addition of a small amount of LiDFOB can form a film on the positive electrode while participating in the initiation effect, which can comprehensively improve the capacity and cycle life of the battery.
[0053] Figure 2 The glass bottle is used to visually display the state characteristics of the precursor liquid before and after solidification. Figure 3 and Figure 4 It is the ionic conductivity and electrochemical window of the semi-solid electrolyte. The ionic conductivity test method is as follows: 50 μl of the precursor solution is injected into a CR2025 button cell composed of stainless steel / diaphragm / stainless steel. After curing at 30°C for 30 hours, the ionic conductivity is calculated using the following formula: Conductivity (σ) = L / (R*S), where S is the contact area between the original sheet stainless steel electrode and the diaphragm, R is the impedance value measured by the electrochemical workstation, and L is the thickness of the diaphragm. The diameter of the original stainless steel sheet can be 14-16 cm, and the thickness of the diaphragm can be 10-30 μm. The electrochemical window test method is as follows: the precursor solution is injected into a CR2025 button cell composed of stainless steel / diaphragm / lithium metal. After curing at 30°C for 30 hours, the electrochemical window is measured using linear sweep voltammetry, where the voltage range is OCV-6V, and the sweep rate can be set to 0.1-2mV. After that, the semi-solid battery was assembled and the precursor solution was injected into the CR2025 button battery. The injection volume was consistent with the conventional injection volume, which was 50 μl. The surface capacity of the positive electrode in the battery was 0.5 mAh / cm 2 The LFP electrode is Celgard2400 polypropylene diaphragm, and the negative electrode has a surface capacity of 10 mAh / cm 2 The lithium metal is packaged and then placed at room temperature of 30°C for 30 hours to obtain a semi-solid-state battery. The capacity retention rate of the semi-solid-state battery is greater than 90% after 500 cycles at 1C rate at room temperature. Figure 5 ), Figure 6 The thermal stability of the semi-solid electrolyte was verified, and it was found that the solidified electrolyte still maintained good solid characteristics after being heated at 110°C for 5 minutes, showing good thermal stability.
[0054] Example 5 The precursor solution is prepared according to the parameters in Table 1 below.
[0055] In an argon glove box, based on 1 ml of liquid, 1 M-LiTFSI, 0.5 M-LiBF4, and 0.1 M-LiDFOB were weighed, a magnet was added, and 0.48 ml-DOL, 0.12 ml-GTE, 0.16 ml-HFE, 0.16 ml-FEC, and 0.08 ml-EMC were added in sequence with a high-precision pipette. The volume ratio of the monomer to the plasticizer was 6:4, and the mixture was stirred at room temperature until the lithium salt was completely dissolved. The process took about 30 minutes to obtain an electrolyte precursor solution. Compared with Example 4, Example 5 increased the monomer component from 50% to 60%, that is, the overall proportion of the polymer after curing was further increased, which can further improve the solid-state characteristics of the semi-solid electrolyte, that is, on the basis of ensuring the electrochemical performance, the thermal stability can be further improved, and the risk of plasticizer leakage can be reduced to ensure better battery safety.
[0056] The precursor solution was injected into the CR2025 button battery. The injection volume was consistent with the conventional injection volume, which was 50 μl. The surface capacity of the positive electrode in the battery was 0.5 mAh / cm 2 The LFP electrode is Celgard2400 polypropylene diaphragm, and the negative electrode has a surface capacity of 10 mAh / cm 2 The lithium metal is packaged and the battery is placed at room temperature of 30°C for 30 hours to cure to obtain a semi-solid-state battery.
[0057] Example 6 The precursor solution is prepared according to the parameters in Table 1 below.
[0058] In an argon glove box, based on 1 ml of liquid, weigh 1M-LiTFSI, 0.5M-LiBF4, and 0.1M-LiDFOB, add a magnet, and then use a high-precision pipette to add 0.4ml-DOL, 0.1ml-GTE, 0.2ml-HFE, 0.2ml-FEC, and 0.1ml-EMC in sequence. The volume ratio of monomer to plasticizer is 1:1. Stir at room temperature until the lithium salt is completely dissolved. The process takes about 30 minutes to obtain an electrolyte precursor solution.
[0059] The precursor solution is injected into a small soft pack battery with an injection amount of 2g / Ah. The battery contains two sheets with a surface capacity of 1.5mAh / cm 2 NCM811 electrode sheet, total capacity 50mAh, Celgard2400 polypropylene diaphragm, negative electrode surface capacity 10mAh / cm 2After the injection is completed, the soft-pack battery is packaged, two glass plates are added to the surface of the battery, and a dovetail clip is added to the outside. The battery is placed at room temperature of 30°C for 30 hours to obtain a 50mAh semi-solid-state battery ( Figure 7 ), compared with Example 4, Example 6 enlarges the battery from a CR2025 button battery based on LFP positive electrode to a 50mAh soft-pack battery based on NCM811 positive electrode, verifying the feasibility of practical application of semi-solid electrolytes.
[0060] Comparative Example 1 The precursor solution is prepared according to the parameters in Table 1 below.
[0061] In an argon glove box, based on 1 ml of liquid, 1 M-LiTFSI, 0.5 M-LiBF4, and 0.1 M-LiDFOB were weighed, a magnet was added, and 0.5 ml-DOL, 0.2 ml-HFE, 0.2 ml-FEC, and 0.1 ml-EMC were added in sequence with a high-precision pipette, the volume ratio of monomer to plasticizer was 1:1, and the mixture was stirred at room temperature until the lithium salt was completely dissolved. The process took about 30 minutes to obtain an electrolyte precursor solution. Unlike Example 4, the comparative example contained only the first monomer but did not contain the second monomer.
[0062] CR2025 button cells were assembled according to the method of Example 4, and after curing at 30°C for 3 days, ionic conductivity and electrochemical window tests were performed in the same manner as in Example 4. Compared with Example 4, the polymer phase in the electrolyte of Comparative Example 1 formed a long chain structure, but did not form a network structure, and the curing time was greatly prolonged. The overall ionic conductivity, electrochemical stability and curing characteristics of the electrolyte were poor ( Figure 3 , Figure 4 and Figure 8 ).
[0063] Comparative Example 2 The precursor solution is prepared according to the parameters in Table 1 below.
[0064] In an argon glove box, based on 1 ml of liquid, 1 M-LiTFSI, 0.5 M-LiBF4, and 0.1 M-LiDFOB were weighed, a magnet was added, and 0.5 ml-DOL, 0.3 ml-FEC, and 0.2 ml-EMC were added in sequence with a high-precision pipette. The volume ratio of the monomer to the plasticizer was 1:1. The mixture was stirred at room temperature until the lithium salt was completely dissolved. The process took about 30 minutes to obtain an electrolyte precursor solution. Unlike Example 4, Comparative Example 2 only contained the second plasticizer but did not contain the first plasticizer.
[0065] The CR2025 button cell was assembled according to the method of Example 4, and after curing at 30°C for 30 hours, an electrochemical window test was performed. The test method was the same as that of Example 4. Compared with Example 4, the electrolyte of Comparative Example 2 did not contain the first plasticizer, and the electrochemical stability decreased ( Figure 4 ).
[0066] Table 1 shows the composition of the precursor solution:
[0067] In the present invention, DOL-GTE copolymerization has advantages over simple DOL polymerization, which can be reflected in Comparative Example 1. Example 4 has improved conductivity and electrochemical window (window represents stability) compared with Comparative Example 1. Moreover, the optical photograph of Example 4 heated at 110°C is used as proof ( Figure 8 ), this resistance to thermal deformation is unmatched by the electrolyte in comparative document 1, which has a liquid content of 90%.
Claims
1. A semi-solid electrolyte precursor solution, characterized in that: include: A first ether monomer, a second ether monomer, a first plasticizer, a second plasticizer, a first lithium salt and a second lithium salt; the first ether monomer is a cyclic ether monomer, preferably at least one of 1,3-dioxolane (DOL), 1,3-dioxane (DOX), tetrahydrofuran (THF), and trioxymethylene (TXE), more preferably 1,3-dioxolane; the second ether monomer is an epoxy ether monomer, preferably including at least one of glycerol triglycidyl ether (GTE), ethylene glycol diglycidyl ether (EGDE), and polyethylene glycol diglycidyl ether (PEGDE).
2. The semi-solid electrolyte precursor solution according to claim 1, characterized in that Based on the total volume of the semi-solid electrolyte precursor solution being 100 vol%, the content of the first ether monomer is 25 to 49 vol%; Based on the total volume of the semi-solid electrolyte precursor solution being 100 vol%, the content of the second ether monomer is 1 to 25 vol%; Preferably, the total volume of the first ether monomer and the second ether monomer accounts for ≥ 40 vol% of the total volume of the precursor solution.
3. The semi-solid electrolyte precursor solution according to claim 2, characterized in that: The volume ratio of the first ether monomer to the second ether monomer is 50:50 to 98:2, preferably 60:40 to 90:
10.
4. The semi-solid electrolyte precursor solution according to any one of claims 1 to 3, characterized in that: The first plasticizer is at least one of 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether (HFE), 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether, and bis(2,2,2-trifluoroethyl) ether, preferably HFE; The second plasticizer is at least one of fluoroethylene carbonate (FEC), methyl trifluoroethyl carbonate (FEMC), ethyl trifluoroethyl carbonate (FDEC), 2,2,2-trifluoro-N,N-dimethylacetamide (FDMA), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethylene carbonate (EC), propylene carbonate (PC), and ethylene glycol dimethyl ether (DME), preferably a binary mixture of FEC and EMC.
5. The semi-solid electrolyte precursor solution according to any one of claims 1 to 4, characterized in that: Based on the total volume of the semi-solid electrolyte precursor solution being 100 vol%, the content of the first plasticizer is 5 to 25 vol%; Based on the total volume of the semi-solid electrolyte precursor solution being 100 vol%, the content of the second plasticizer is 25 to 45 vol%; Preferably, the total volume of the first plasticizer and the second plasticizer does not exceed 60 vol% of the total volume of the precursor solution.
6. The semi-solid electrolyte precursor solution according to claim 5, characterized in that: The volume ratio of the first plasticizer to the second plasticizer is 10:90 to 50:50, preferably 15:85 to 45:
55.
7. The semi-solid electrolyte precursor solution according to any one of claims 1 to 6, characterized in that: The ratio of the total volume of the first ether monomer and the second ether monomer to the total volume of the first plasticizer and the second plasticizer is 30:70 to 70:30, preferably 40:60 to 60:
40.
8. The semi-solid electrolyte precursor solution according to any one of claims 1 to 7, characterized in that: The first lithium salt is at least one of lithium bis(trifluoromethanesulfonyl imide) (LiTFSI), lithium bis(pentafluoroethylsulfonyl imide) (LiPFSI), and lithium trifluoromethanesulfonate (LiOTF), preferably lithium bis(trifluoromethanesulfonyl imide) (LiTFSI); the concentration of the first lithium salt in the semi-solid electrolyte precursor solution is 0.5 to 3 mol / L, preferably 0.8 to 2 mol / L.
9. The semi-solid electrolyte precursor solution according to any one of claims 1 to 8, characterized in that: The second lithium salt is at least one of lithium difluorooxalatoborate (LiDFOB), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), and lithium bis(fluorosulfonyl)imide (LiFSI), preferably a binary mixture of LiDFOB and LiBF4, more preferably a molar ratio of LiDFOB to LiBF4 of (3-5):1; The concentration of the second lithium salt in the semi-solid electrolyte precursor solution is 0.05 to 1 mol / L, preferably 0.1 to 0.6 mol / L.
10. A method for preparing a semi-solid electrolyte, characterized in that: include: The semi-solid electrolyte precursor solution according to any one of claims 1 to 9 is subjected to in-situ curing to obtain the semi-solid electrolyte; preferably, the in-situ curing temperature is 25 to 80°C, preferably 30 to 60°C.
11. A semi-solid electrolyte prepared by the preparation method according to claim 10, characterized in that: include: A macromolecular network structure formed by copolymerization of the first ether monomer and the second ether monomer.
12. A semi-solid battery, characterized in that: include: The semi-solid electrolyte according to claim 11.
13. The semi-solid-state battery according to claim 12, characterized in that: Also includes: Positive electrode, separator and negative electrode.
14. The semi-solid battery according to claim 12, characterized in that: The structure of the semi-solid battery includes: positive electrode / semi-solid electrolyte / separator / semi-solid electrolyte / negative electrode in sequence.
15. The semi-solid-state battery according to any one of claims 12 to 14, characterized in that: The positive electrode comprises at least one of a lithium iron phosphate positive electrode (LFP), a nickel-cobalt-manganese ternary positive electrode (NCM), a lithium-rich manganese-based positive electrode, and a sulfur positive electrode; preferably, the positive electrode has a surface capacity of 0.5 to 5 mAh / cm 2 , preferably 3 to 4 mAh / cm 2 ; The diaphragm comprises at least one of a polyolefin diaphragm and a glass fiber diaphragm; The negative electrode lithium comprises at least one of a negative electrode, a graphite negative electrode, a hard carbon negative electrode, a silicon-carbon negative electrode, and a silicon negative electrode; preferably, the negative electrode surface capacity is 2 to 20 mAh / cm 2 , preferably 4 to 10 mAh / cm 2 .
16. A method for preparing a semi-solid battery, characterized in that: include: Injecting the semi-solid electrolyte precursor solution according to any one of claims 1 to 9 into a component comprising a positive electrode, a negative electrode, and a separator, and then curing the component in situ to obtain the semi-solid battery; Preferably, the injection amount of the semi-solid electrolyte precursor solution is 1 to 4 g / Ah, preferably 1 to 2 g / Ah; Preferably, the in-situ curing temperature is 25 to 80°C, preferably 30 to 60°C; Preferably, the in-situ curing time may be 1 to 48 hours, preferably 6 to 36 hours.