Method for manufacturing steel component

By combining carburizing and quenching processes in the manufacturing of steel parts, the carbon concentration is controlled at the hypoeutectoid composition level, which solves the problems of excessive hardness and low toughness, achieving a balanced improvement in hardness and toughness and improving the comprehensive performance of steel parts. .

CN118786227APending Publication Date: 2024-10-15AISIN CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023388.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-24
Filing Date
2023-01-17
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing manufacturing methods of steel parts, after carbon penetrates into the austenitized state, it is easy to cause the hardness to be too high and the toughness to be too low, affecting the impact resistance of the steel parts.

Method used

Using a combination method of carburizing process and quenching process, by heating the steel parts to above the austenitizing transformation end temperature, and performing slow cooling and rapid cooling, the carbon concentration is controlled at the hypoeutectoid composition level to avoid excessive carbon concentration. Thereby improving hardness and toughness in a balanced manner.

Benefits of technology

It achieves a balanced improvement in the hardness and toughness of steel parts, improves the bending fatigue strength and impact strength, and ensures the comprehensive performance of steel parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786227A_ABST
    Figure CN118786227A_ABST
Patent Text Reader

Abstract

This method for manufacturing a steel component comprises: a carburizing step in which carbon is permeated into the steel component at a carbon concentration at which the steel component and carbon form a hypoeutectoid composition in a state in which the steel component is austenitized by being heated to a temperature equal to or higher than an austenitizing transition completion temperature; and a quenching step in which, after the carburizing step, the steel component is reheated to a temperature equal to or higher than the austenitizing transition completion temperature, and the heated steel component is rapidly cooled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a steel component. Background Art

[0002] Conventionally, there is known a method for manufacturing a steel part, which includes a carburizing step of infiltrating carbon into a steel part in an austenitized state. For example, Japanese Patent Application Laid-Open No. 2019-127624 discloses such a method for manufacturing a steel part.

[0003] Japanese Patent Application Publication No. 2019-127624 discloses a method for manufacturing a steel component, which includes a carburizing step of infiltrating carbon into a steel component in an austenitized state. In the method for manufacturing a steel component described in Japanese Patent Application Publication No. 2019-127624, in the carburizing step, carbon is infiltrated into the steel component in an austenitized state at a carbon concentration such that the steel component and carbon form a hypereutectoid composition. Patent Literature

[0004] Patent Document 1: Japanese Patent Application Publication No. 2019-127624 Summary of the invention

[0005] However, in the manufacture of the steel parts described in Japanese Patent Publication 2019-127624, due to the carbon concentration of the hypereutectoid composition formed by the steel parts and carbon, carbon is infiltrated into the steel parts in the state of austenitization, so the carbon concentration infiltrated into the steel parts tends to become too high. Here, the hardness of the steel parts is generally roughly proportional to the carbon concentration of the surface (carburized layer) of the steel parts. In addition, the hardness of the steel parts is generally roughly inversely proportional to the toughness of the steel parts. That is, in the manufacture of the steel parts described in Japanese Patent Publication 2019-127624, it is easy to occur that the hardness of the steel parts becomes too high and the toughness of the steel parts becomes too low. Once the toughness of the steel parts becomes low, the ability of the steel parts to cope with the impact will weaken. Therefore, it is expected to find a method for manufacturing a steel part that can improve the hardness and toughness of the steel parts in a balanced manner.

[0006] The present invention has been made to solve the above-mentioned technical problems, and one object of the present invention is to provide a method for manufacturing a steel part capable of improving the hardness and toughness of the steel part in a balanced manner.

[0007] In order to achieve the above-mentioned object, a method for manufacturing a steel part in one embodiment of the present invention comprises a carburizing step and a quenching step. The carburizing step is to heat the steel part to a temperature higher than the austenitizing transformation finish temperature so that the steel part is in a state of being austenitized, infiltrate carbon into the steel part at a carbon concentration such that the steel part and carbon form a hypoeutectoid composition, and slowly cool the steel part infiltrated with carbon. The quenching step is to heat the steel part again to a temperature higher than the austenitizing transformation finish temperature after the carburizing step, and rapidly cool the heated steel part.

[0008] In a method for manufacturing a steel part in one embodiment of the present invention, as described above, in the carburizing process, carbon is infiltrated into a steel part in a state where austenitization has occurred at a carbon concentration such that the steel part and carbon form a hypoeutectoid composition. Thus, unlike the case where carburization is performed in which carbon is infiltrated into a steel part in a state where austenitization has occurred at a carbon concentration such that the steel part and carbon form a hypereutectoid composition, the carbon concentration infiltrated into the steel part will not become too high. Thus, the hardness of the steel part will not become too high, and the toughness of the steel part will not become too low. As a result, the hardness and toughness of the steel part can be improved in a balanced manner. Thus, the bending fatigue strength can be improved by improving the hardness, and the strength to impact can also be improved by improving the toughness.

[0009] According to the present invention, as described above, it is possible to provide a method for manufacturing a steel part capable of improving the hardness and toughness of the steel part in a balanced manner. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] [ Figure 1 ] A schematic diagram of a manufacturing process for a steel component according to an embodiment of the present invention. [ Figure 2 ]A diagram showing temperature changes of a steel part in a method for manufacturing a steel part according to an embodiment of the present invention. [ Figure 3 ]State diagram of S20C as an example of a steel component. [ Figure 4 ]A diagram showing temperature changes of a steel component in a method for manufacturing a steel component according to Comparative Example 1. [ Figure 5 ]A diagram showing temperature changes of a steel component in a method for manufacturing a steel component according to Comparative Example 2. [ Figure 6 ] Graphs showing the bending fatigue strength and toughness of steel parts in a method for manufacturing steel parts based on an embodiment of the present invention, a method for manufacturing steel parts based on a first variant example, a method for manufacturing steel parts based on a second variant example, and a method for manufacturing steel parts based on comparison example 1. [ Figure 7 ]A graph showing the bending fatigue strength of a steel part in a method for manufacturing a steel part according to an embodiment of the present invention, a steel part in a method for manufacturing a steel part according to a first variant example, and a steel part in a method for manufacturing a steel part according to a comparison example 2. [ Figure 8 ]A graph showing the torsional fatigue strength of a steel part in a method for manufacturing a steel part according to an embodiment of the present invention, a steel part in a method for manufacturing a steel part according to a first variant example, and a steel part in a method for manufacturing a steel part according to Comparative Example 3. [ Fig. 9 ] shows graphs of surface hardness, surface hardened layer depth, surface carbon concentration, etc. of steel parts in a method for manufacturing steel parts based on an embodiment of the present invention, a method for manufacturing steel parts based on a first variant example, and a method for manufacturing steel parts based on a comparison example 2. [ Fig.10 ] A graph showing the grain boundary oxidation depth and average crystal grain size of a steel part in a method for manufacturing a steel part according to an embodiment of the present invention and a steel part in a method for manufacturing a steel part according to Comparative Example 2. DETAILED DESCRIPTION

[0011] Hereinafter, embodiments of the present invention will be described based on the drawings.

[0012] [Method for manufacturing steel parts] Reference Figure 1 to Figure 3 , a method for manufacturing a steel component according to an embodiment of the present invention will be described. It should be noted that the method for manufacturing a steel component according to an embodiment of the present invention can be applied to steel components such as gears, bearings, and shafts.

[0013] (Cold forging process) First, if Figure 1 As shown, in step S1, a cold forging process is performed. The cold forging process (S1) is a process of forging a steel part into a desired shape (e.g., a gear, a bearing, a shaft, etc.) at room temperature. For the steel part, case hardened steel (e.g., SCM420) is used in which a hardened layer is formed by heat treatment on the surface.

[0014] (Carburizing process) Next, in step S2, a carburizing process is performed. Figure 2 As shown in FIG. 1 , the carburizing step (S2) is a step of infiltrating carbon into the steel part in a state where the steel part is austenitized by heating the steel part to a temperature T1 (e.g., about 1000° C.) above the austenitizing transformation end temperature A3, and then slowly cooling the steel part infiltrated with carbon. Figure 3As shown in FIG. 1 , the steel part in the state of being austenitized refers to a steel part composed of austenite (γ iron). The austenitization transformation completion temperature A3 is the temperature at which the steel part is heated and the austenitization transformation of the steel part is completed. Specifically, Figure 2 As shown, the steel part is arranged in the first heat treatment chamber. Then, the steel part is heated to a temperature T1 so that the steel part is austenitized. Then, while the steel part is maintained at a temperature T1 (i.e., the steel part is austenitized), a carburizing gas (e.g., C2H2) is introduced into the interior of the first heat treatment chamber. Then, on the surface of the steel part in the austenitized state, the carburizing gas decomposes to generate carbon. Then, since the generated carbon diffuses from the surface of the steel part to the inside, a carburized layer is formed on the surface of the steel part. Then, the steel part is slowly cooled so that the steel part is pearlitized. The steel part is slowly cooled at a cooling rate at which the steel part is pearlitized. That is, the steel part is slowly cooled at a cooling rate at which the steel part is not martensited. In addition, in order to prevent the formation of an oxide film on the steel part, the steel part is slowly cooled by an inert gas (e.g., Ar, N2, HE, etc.) atmosphere. It should be noted that the carburizing step ( S2 ) is performed while the interior of the first heat treatment chamber is depressurized by a vacuum pump.

[0015] like Figure 3 As shown, when the carbon concentration is a carbon concentration at which the steel part forms a hypoeutectoid composition with carbon (a concentration less than about 0.77%), the steel part is in a state composed of ferrite (α iron) and pearlite at a temperature lower than the austenitizing transformation start temperature A1. In addition, when the concentration does not reach the carbon concentration at which the steel part forms a hypoeutectoid composition with carbon, the steel part is in a state composed of austenite (γ iron) and ferrite (α iron) at a temperature higher than the austenitizing transformation start temperature A1 and lower than the austenitizing transformation end temperature A3. In addition, when the carbon concentration does not reach the carbon concentration at which the steel part forms a hypoeutectoid composition with carbon, the steel part is in a state composed of austenite (γ iron) at a temperature higher than the austenitizing transformation end temperature A3.

[0016] like Figure 2As shown, in the carburizing process (S2), carbon is infiltrated into the steel part in a state where austenitization has occurred with a carbon concentration at which the steel part and carbon form a hypoeutectoid composition. Specifically, by continuously introducing carburizing gas into the interior of the first heat treatment chamber, the carbon concentration on the surface (carburized layer) of the steel part will rise. In addition, the time for introducing carburizing gas is adjusted so that the carbon concentration on the surface (carburized layer) of the steel part becomes a carbon concentration that does not reach the carbon concentration at which the steel part and carbon form a eutectoid composition (for example, about 0.77% when the steel part is carburizing steel SCM420). Here, the hardness of the steel part is generally roughly proportional to the carbon concentration on the surface (carburized layer) of the steel part. In addition, the hardness of the steel part is generally roughly inversely proportional to the toughness of the steel part. Thus, unlike the carburizing of the steel part in a state where austenitization has occurred with a carbon concentration (concentration of about 0.77% or more) at which the steel part and carbon form a hypereutectoid composition, the carbon concentration infiltrated into the steel part will not become too high. Thus, the hardness of the steel part does not become too high, and the toughness of the steel part does not become too low. As a result, the hardness and toughness of the steel part can be improved in a balanced manner. Thus, the bending fatigue strength can be improved by improving the hardness, and the strength against impact can be improved by improving the toughness.

[0017] (Nitriding process) Then, if Figure 1 As shown, in step S3, a nitriding process is performed. Figure 2 As shown, the nitriding process (S3) is a process for infiltrating nitrogen into a steel part in a state where the steel part is heated to a temperature T2 (for example, about 810°C) that does not reach the austenitizing transformation end temperature A3. Specifically, the steel part is arranged in the second heat treatment chamber. Then, the steel part in the state where pearlitization has occurred in the carburizing process (S2) is heated to a temperature T2. At this time, the steel part becomes a state in which ferrite (α iron) and austenite (γ iron) are mixed. Then, while the steel part is maintained at a temperature T2 (that is, the steel part is in a state in which ferrite (α iron) and austenite (γ iron) are mixed), a specified amount (for example, 0.8 m 3 / hour) of nitriding gas (for example, NH3). Then, on the surface of the steel part, the nitriding gas decomposes to generate nitrogen. Then, since the generated carbon diffuses from the surface of the steel part to the inside, the nitrogen penetrates into the carburized layer of the surface part of the steel part, thereby forming a carburized nitrided layer. It should be noted that in order to prevent the carbon concentration of the carburized layer from decreasing, the carbon concentration inside the second heat treatment chamber is adjusted while the nitriding process (S3) is performed. Here, the amount of nitrogen infiltrated into the surface part of the steel part is generally inversely proportional to the temperature of the steel part at a temperature above the austenitizing transformation start temperature A1 (described later). In addition, in the case of infiltrating nitrogen into the carburized layer of the surface part of the steel part, generally the higher the carbon concentration of the carburized layer, the easier it is to generate voids in the steel part. In addition, the higher the temperature of the steel part becomes, the easier it is to form a grain boundary oxide layer in the steel part. In addition, the more the amount of nitrogen infiltrated into the surface part of the steel part increases, the harder the steel part will be. Thus, compared with the case of nitriding the steel part in a state where the steel part is heated to a temperature T3 (e.g., about 850° C.) above the austenitizing end temperature A3 for nitrogen infiltration, the amount of nitrogen infiltrated into the steel part can be increased, and the generation of cavities or the formation of a grain boundary oxide layer in the steel part can be suppressed. As a result, the hardness of the steel part can be effectively increased, and therefore, even in the case where the toughness of the steel part is increased in the carburizing step (S2) and the hardness of the steel part is reduced accordingly, sufficient hardness of the steel part can be ensured.

[0018] In the nitriding step (S3), the time for introducing the nitriding gas and the amount of the nitriding gas are adjusted so that the nitrogen concentration on the surface (carburized and nitrided layer) of the steel part becomes a specified concentration. That is, the nitriding step (S3) is a step for infiltrating nitrogen into the steel part so that the nitrogen concentration on the surface of the steel part becomes a specified concentration. The specified concentration is at least about 0.5% or less. The specified concentration is preferably about 0.05% or more and 0.35% or less. Thus, nitriding can be performed in a manner that improves the hardness and toughness of the steel part in a balanced manner.

[0019] The nitriding step (S3) is a step of infiltrating nitrogen into a steel part at a temperature T2 (for example, about 810°C) that is above the austenitizing start temperature A1 and below the austenitizing end temperature A3. The austenitizing start temperature A1 is the temperature at which the steel part begins to undergo austenitizing. Here, when nitriding is performed to infiltrate nitrogen into the steel part at a temperature that does not reach the austenitizing start temperature A1, the amount of nitrogen infiltrated into the steel part is generally significantly reduced compared to the case where nitriding is performed to infiltrate nitrogen into the steel part at a temperature above the austenitizing start temperature A1. As a result, the amount of nitrogen infiltrated into the steel part can be increased compared to the case where nitriding is performed to infiltrate nitrogen into the steel part at a temperature that does not reach the austenitizing start temperature A1.

[0020] As described above, a cold forging process is performed in step S1. That is, the carburizing process (S2) is performed on the steel part after cold forging. Thus, in the carburizing process (S2), by heating the steel part and slowly cooling it, the residual stress generated in the steel part due to cold forging can be eliminated from the steel part. As a result, in the subsequent process (the quenching process (S4) described later, etc.), the grain coarsening of the steel part caused by the residual stress can be suppressed. That is, the strength reduction of the steel part caused by the grain coarsening can be suppressed. In addition, the grain coarsening can be suppressed, and the dimensional change of each part of the steel part can be suppressed from becoming larger in the subsequent process. In addition, there is no need to use a special steel part to which Nb, TI, V, etc. are added in order to suppress the grain coarsening that occurs in the steel part after cold forging. As a steel part, a generally used carburizing steel (for example, SCM420) can be used.

[0021] (Quenching process) Then, if Figure 1 As shown, in step S4, a quenching process is performed. Figure 2 As shown, the quenching process (S4) is a process of reheating the steel part to a temperature T3 (for example, about 850°C) above the austenitizing transformation end temperature A3, and rapidly cooling the heated steel part. Specifically, the steel part is arranged in the second heat treatment chamber. Then, the steel part is reheated to a temperature T3 so that the steel part is austenitized. Then, after briefly maintaining the state of the steel part at a temperature T3 (that is, the state in which the steel part is austenitized), the steel part is transported from the heat treatment chamber to the inside of the cooling device, and the steel part is rapidly cooled so that the steel part is martensited. The steel part is rapidly cooled at a cooling rate at which the steel part will undergo martensite transformation. That is, the steel part is rapidly cooled at a cooling rate at which the steel part does not undergo pearlite transformation. In addition, water or oil is used to rapidly cool the steel part.

[0022] The quenching step (S4) is a step of heating the steel part from a temperature T2 (e.g., about 810°C) that does not reach the austenitizing transformation end temperature A3 to a temperature T3 (e.g., about 850°C) that is higher than the austenitizing transformation end temperature A3 immediately after the nitriding step (S3), and rapidly cooling the heated steel part. That is, the nitriding step (S3) and the quenching step (S4) are performed continuously in this order. Thus, the steel part that has been heated to a temperature T2 (e.g., about 810°C) that does not reach the austenitizing transformation end temperature A3 in the nitriding step (S3) can be heated from the temperature T2 (e.g., about 810°C) to a temperature T3 (e.g., about 850°C) that is higher than the austenitizing transformation end temperature A3, and thus, compared with the case where the quenching step (S4) is not performed immediately after the nitriding step (S3), the energy consumption in heating the steel part can be suppressed.

[0023] (Tempering process) Then, if Figure 1 As shown, in step S5, a tempering process is performed. The tempering process (S5) is a process of heating the martensitic steel part again and cooling it. Thus, the steel part in a state where the hardness becomes too high and the toughness decreases excessively due to martensiticization is changed to a state with appropriate fatigue strength and toughness by tempering.

[0024] [Example] Reference Figures 4 to 10 , an example of the method for manufacturing a steel component according to the above-mentioned embodiment will be described while being compared with a method for manufacturing a steel component according to Comparative Example 1 and a method for manufacturing a steel component according to Comparative Example 2.

[0025] (Manufacturing of Steel Parts Based on the Aforesaid Embodiment) According to the manufacturing method of the steel part based on the above-mentioned embodiment, the steel part is set as a gear, and a steel part is manufactured (Example 1). Specifically, first, a cold forging process of cold forging the steel part is carried out. For the steel part, carburizing steel SCM420 is used. Then, a carburizing process is carried out, and the carburizing process is to infiltrate carbon into the steel part in a state where the steel part is austenitized by heating it to a temperature T1 (1000°C) above the austenitizing transformation end temperature A3, and the steel part infiltrated with carbon is slowly cooled. In the carburizing process, carbon is infiltrated into the steel part in a state where austenitization occurs at a carbon concentration (less than 0.77%) at which the steel part and carbon form a hypoeutectoid composition. The carburizing process is carried out while decompressing the interior of the first heat treatment chamber by a vacuum pump. Then, a nitriding process is carried out, and the nitriding process is to infiltrate nitrogen into the steel part in a state where the steel part is heated to a temperature T2 (810°C) that does not reach the austenitizing transformation end temperature A3. Then, immediately after the nitriding step, a quenching step is performed, in which the steel part is heated again to a temperature T3 (850°C) above the austenitization end temperature A3 and the heated steel part is rapidly cooled. Then, a tempering step is performed, in which the martensitic steel part is heated again and cooled.

[0026] (Manufacturing of Steel Parts Based on the First Modification and the Second Modification) As a first modification of the above embodiment, a steel component was manufactured by omitting the nitriding step in the method for manufacturing a steel component based on the above embodiment (Example 2). In addition, as a second modification of the above embodiment, a steel component was manufactured by omitting the nitriding step in the method for manufacturing a steel component based on the above embodiment and replacing the steel component in the method for manufacturing a steel component based on the above embodiment with a sintered material instead of a carburized steel (Example 3).

[0027] (Manufacturing of other steel parts based on the above-mentioned embodiment and first modified example) According to the manufacturing method of the steel component based on the above embodiment, the steel component was used as a shaft to manufacture a steel component (Example 4). In addition, according to the manufacturing method of the steel component based on the first modified example, the steel component was used as a shaft to manufacture a steel component (Example 5).

[0028] (Manufacturing of Steel Parts Based on Comparative Example 1) according to Figure 4 The method for manufacturing a steel component based on Comparative Example 1 shown in the figure sets the steel component as a gear and manufactures the steel component. Specifically, first, a cold forging process is performed as in the method for manufacturing a steel component based on the above-mentioned embodiment. As for the steel component, carburizing steel SCM420 is used as in the method for manufacturing a steel component based on the above-mentioned embodiment. Then, as in the method for manufacturing a steel component based on the above-mentioned embodiment, a carburizing process is performed, in which carbon is infiltrated into the steel component in a state where the steel component is heated to a temperature T1 (1000°C) above the austenitizing transformation end temperature A3 to make it austenitized, and the steel component infiltrated with carbon is slowly cooled. Unlike the method for manufacturing a steel component based on the above-mentioned embodiment, in the carburizing process, during the slow cooling of the steel component, the steel component is kept at a temperature T4 (710°C) that does not reach the austenitizing transformation start temperature A1, and is maintained in this state for a specified time so that only a part of the austenite is pearlitized. That is, the time for which the steel part is kept at a temperature of T4 (710°C) is correspondingly longer than that of the method for manufacturing a steel part according to the above-mentioned embodiment. In addition, unlike the method for manufacturing a steel part according to the above-mentioned embodiment, in the carburizing step, carbon is infiltrated into the steel part in a state where austenitization has occurred, with a carbon concentration (0.77% or more) such that the steel part and carbon form a hypereutectoid composition. It should be noted that, as in the method for manufacturing a steel part according to the above-mentioned embodiment, the carburizing step is performed while decompressing the interior of the heat treatment chamber by a vacuum pump. Then, a quenching step is performed, in which the steel part is heated to a temperature of T3 (850°C) above the austenitization transformation end temperature A3, and the steel part is briefly maintained at the temperature of T3 (850°C), and then the steel part is rapidly cooled. It should be noted that in the quenching step, when the steel part is kept at a temperature T3 (850° C.) for a short time (i.e., the steel part is austenitized), a nitriding step for infiltrating nitrogen into the steel part is also performed. Then, a tempering step is performed as in the method for manufacturing a steel part according to the above embodiment.

[0029] (Manufacturing of Steel Parts Based on Comparative Example 2) according to Figure 5 The manufacturing method of the steel component based on the comparative example 2 shown in the figure sets the steel component as a gear and manufactures the steel component. Specifically, first, a cold forging process is performed as in the manufacturing method of the steel component based on the above-mentioned embodiment. For the steel component, carburizing steel SCM420 is used as in the manufacturing method of the steel component based on the above-mentioned embodiment. Then, as in the manufacturing method of the steel component based on the above-mentioned embodiment, a carburizing process is performed, in which carbon is infiltrated into the steel component in a state where the steel component is austenitized by heating the steel component to a temperature T1 (1000°C) above the austenitizing transformation end temperature A3, and the steel component infiltrated with carbon is slowly cooled. It should be noted that the slow cooling in the carburizing process is performed until the temperature of the steel component reaches the temperature T3 (850°C) for the quenching process. In addition, unlike the manufacturing method of the steel component based on the above-mentioned embodiment, in the carburizing process, carbon is infiltrated into the steel component in a state where austenitization has occurred at a carbon concentration (0.77%) at which the steel component and carbon form a eutectic composition. It should be noted that, unlike the method for manufacturing a steel component based on the above-mentioned embodiment, in the carburizing process, the carburizing process is performed without decompressing the interior of the heat treatment chamber. Then, a quenching process is performed, in which the steel component is rapidly cooled after briefly maintaining the steel component at a temperature T3 (850°C) above the austenitizing transformation end temperature A3. That is, unlike the method for manufacturing a steel component based on the above-mentioned embodiment, the steel component is not pearlitized after the carburizing process, but the quenching process is performed immediately after the carburizing process. It should be noted that, unlike the method for manufacturing a steel component based on the above-mentioned embodiment, a nitriding process is not performed. And, as in the method for manufacturing a steel component based on the above-mentioned embodiment, a tempering process is performed.

[0030] (Manufacturing of Steel Parts Based on Comparative Example 3) As Comparative Example 3, a steel component was manufactured by replacing the gear with a shaft in the method for manufacturing a steel component according to Comparative Example 2.

[0031] (Test results of steel component performance) Hereinafter, test results of the performance of steel parts using the method for manufacturing steel parts based on the above-mentioned embodiment (steel parts of Example 1 and steel parts of Example 4), steel parts using the method for manufacturing steel parts based on the above-mentioned first variant (steel parts of Example 2 and steel parts of Example 5), steel parts using the method for manufacturing steel parts based on the above-mentioned second variant (steel parts of Example 3), steel parts using the method for manufacturing steel parts based on Comparative Example 1 (steel parts of Comparative Example 1), steel parts using the method for manufacturing steel parts based on Comparative Example 2 (steel parts of Comparative Example 2), and steel parts using the method for manufacturing steel parts based on Comparative Example 3 (steel parts of Comparative Example 3) will be described.

[0032] like Figure 6 As shown, the crack generation energy E during the impact test of any of the steel parts of Example 1 (SCM (with nitriding) in the figure), the steel parts of Example 2 (SCM (without nitriding) in the figure), and the steel parts of Example 3 (sintered material (without nitriding) in the figure) i (J / cm 2 ) and bending fatigue strength σ (MPa) are greater than those of the steel component of Comparative Example 1 (SCM420 (Comparative Example 1) in the figure). Specifically, the crack generation energy E of the steel component of Example 1 is i The crack generation energy E of the steel component of Comparative Example 1 is i The crack generation energy E of the steel component of Example 2 is greater. i Energy E generated by cracking of steel parts i The crack generation energy E of the steel component of Example 3 is greater. i The crack generation energy E of the steel part of Example 2 is i The bending fatigue strength σ of the steel part of Example 3 is greater than the bending fatigue strength σ of the steel part of Comparative Example 1. The bending fatigue strength σ of the steel part of Example 2 is greater than the bending fatigue strength σ of the steel part of Example 3. The bending fatigue strength σ of the steel part of Example 1 is greater than the bending fatigue strength σ of the steel part of Example 2. It should be noted that the crack generation energy E during the impact test i The size of is roughly proportional to the size of toughness. In addition, the bending fatigue strength σ means the size of the strength relative to bending. The bending fatigue strength σ is generally roughly proportional to the hardness. The crack generation energy E during the impact test is measured using the Charpy impact test i In addition, the bending fatigue strength σ was measured using the Ono-type rotating bending fatigue test.

[0033] like Figure 7As shown, the bending fatigue strength σ (MPa) of any of the steel parts of Example 1 (SCM (with nitriding) in the figure) and the steel parts of Example 2 (SCM (without nitriding) in the figure) is greater than that of the steel parts of Comparative Example 2 (SCM420 (Comparative Example 2) in the figure).

[0034] like Figure 8 As shown, the torque amplitude T of the steel component of Example 4 (SCM (with nitriding) in the figure) and the steel component of Example 5 (SCM (without nitriding) in the figure) is a (N·m) are larger than those of the steel component of Comparative Example 3 (SCM420 (Comparative Example 3) in the figure). a It is an indicator of torsional fatigue strength. The torque amplitude T is measured using the torsional fatigue test. a .

[0035] like Fig. 9 As shown, the surface hardness of the steel component of Comparative Example 2 (SCM420 (Comparative Example 2) in the figure) is 760 HV, while the surface hardness of the steel component of Example 1 (SCM (with nitriding) in the figure) is 770, and the surface hardness of the steel component of Example 2 (SCM (without nitriding) in the figure) is 771. That is, the steel component of Example 1 and the steel component of Example 2 have a higher surface hardness than the steel component of Comparative Example 2. It should be noted that the surface hardness was measured using the Vickers hardness test in accordance with JIS Z 2244.

[0036] The surface hardened layer depth of the steel component of Comparative Example 2 (SCM420 (Comparative Example 2) in the figure) is 0.77 mm, while the surface hardened layer depth of the steel component of Example 1 (SCM (with nitriding) in the figure) is 0.82 mm, and the surface hardened layer depth of the steel component of Example 2 (SCM (without nitriding) in the figure) is 0.80 mm. That is, the surface hardened layer depths of the steel components of Example 1 and Example 2 are greater than those of the steel component of Comparative Example 2.

[0037] The carbon concentration on the surface of the steel part of Comparative Example 2 (SCM420 (Comparative Example 2) in the figure) is 0.70 wt %, whereas the carbon concentration on the surface of the steel part of Example 1 (SCM (with nitriding) in the figure) is 0.54 wt %, and the carbon concentration on the surface of the steel part of Example 2 (SCM (without nitriding) in the figure) is 0.57 wt %. That is, the carbon concentration on the surface of the steel part of Example 1 and the steel part of Example 2 is significantly lower than that of the steel part of Comparative Example 2. This is considered to be caused by the fact that in the carburizing process, carbon is infiltrated into the steel part in a state where the steel part and carbon form an eutectoid composition (0.77%), while in the carburizing process, carbon is infiltrated into the steel part in a state where the steel part and carbon form an hypoeutectoid composition (less than 0.77%).

[0038] The total case depth of the steel part of Example 1 (SCM (with nitriding) in the figure), the total case depth of the steel part of Example 2 (SCM (without nitriding) in the figure), and the total case depth of the steel part of Comparative Example 2 (SCM420 (Comparative Example 2) in the figure) are all 1.4 mm. This is considered to be caused by the fact that carbon is infiltrated into the steel part that has been heated to temperature T1 (1000°C) and austenitized in all the steel parts of Example 1, Example 2, and Comparative Example 2.

[0039] The nitrogen concentration at the surface of the steel part of Example 1 (SCM (nitrided) in the figure) is 0.34 wt%. That is, in the steel part of Example 1, the nitrogen concentration at the surface is lower than the carbon concentration at the surface. In addition, the total nitriding depth of the steel part of Example 1 (SCM (nitrided) in the figure) is 0.3 mm. That is, in the steel part of Example 1, the total nitriding depth is lower than the total carburizing depth at the surface.

[0040] like Fig.10 As shown in the figure, the grain boundary oxidation depth of the steel part of Comparative Example 2 (SCM420 (Comparative Example 2) in the figure) is 14 μm, while the grain boundary oxidation depth of the steel part of Example 1 (SCM (with nitriding) in the figure) is 5 μm. That is, the grain boundary oxidation depth of the steel part of Example 1 is smaller than that of the steel part of Comparative Example 2. Therefore, in the steel part of Example 1, the formation of the grain boundary oxidation layer in the manufacturing process is greatly suppressed.

[0041] The minimum value of the crystal grain size of the steel part of Example 1 (MIN in the figure) and the minimum value of the crystal grain size of the steel part of Comparative Example 2 are both 10μm. On the other hand, the maximum value of the crystal grain size of the steel part of Comparative Example 2 (MAX in the figure) is 170μm, while the maximum value of the crystal grain size of the steel part of Example 1 is 22μm. Furthermore, the average crystal grain size of the steel part of Comparative Example 2 is 38μm, while the average crystal grain size of the steel part of Example 1 is 14μm. That is, the steel part of Example 1 has a smaller average crystal grain size than the steel part of Comparative Example 2. Therefore, in the steel part of Example 1, the coarsening of the crystal grain size in the manufacturing process is greatly suppressed.

[0042] As described above, the steel parts of the examples (Examples 1 to 5) showed high toughness, bending fatigue strength, surface hardness, surface hardened layer depth, etc. Therefore, the method for manufacturing a steel part based on the above embodiment, the method for manufacturing a steel part based on the first modified example of the above embodiment, and the method for manufacturing a steel part based on the second modified example of the above embodiment are suitable as a method for manufacturing steel parts (e.g., gears, bearings, shafts, etc.) that require both high hardness and high toughness.

[0043] [Modifications] It should be noted that the embodiments disclosed this time are illustrative in all aspects and should not be considered restrictive. The scope of the present invention is indicated by the claims rather than the description of the embodiments above, and further includes all changes (modifications) within the meaning and scope equivalent to the claims.

[0044] For example, in the above embodiment, the example of performing the carburizing step (S2) on the cold-forged steel part is shown, but the present invention is not limited thereto. In the present invention, the carburizing step may be performed on the hot-forged steel part.

[0045] In addition, in the above embodiment, the nitriding step (S3) is an example of a step of infiltrating nitrogen into the steel part at a temperature T2 that is higher than the austenitizing start temperature A1 and lower than the austenitizing end temperature A3, but the present invention is not limited thereto. In the present invention, the nitriding step may also be a step of infiltrating nitrogen into the steel part at a temperature lower than the austenitizing start temperature.

[0046] In addition, in the above-mentioned embodiment, an example is shown in which the nitriding step (S3) is a step of infiltrating nitrogen into the steel part in a state where the steel part is heated to a temperature T2 that does not reach the austenitizing transformation end temperature A3, but the present invention is not limited thereto. In the present invention, the nitriding step may be a step of infiltrating nitrogen into the steel part in a state where the steel part is heated to a temperature higher than the austenitizing transformation end temperature, as in Comparative Example 1. In this case, the nitriding step may be performed while heating in the quenching step, as in Comparative Example 1.

[0047] In addition, in the above embodiment, an example of performing the nitriding step (S3) of infiltrating nitrogen into the steel part is shown, but the present invention is not limited thereto. In the present invention, the nitriding step of infiltrating nitrogen into the steel part may not be performed as in the above first and second modified examples.

[0048] In addition, in the above embodiment, an example of using carburized steel for steel parts is shown, but the present invention is not limited to this. In the present invention, a sintered material may be used for the steel parts as in the above second modification. Explanation of symbols

[0049] Austenitizing start temperature ... A1, austenitizing end temperature ... A3, temperatures (higher than the austenitizing end temperature) ... T1, T3, temperatures (less than the austenitizing end temperature) ... T2.

Claims

1. A method for manufacturing a steel component, comprising: a carburizing step of heating a steel part to a temperature not lower than an austenitizing transformation end temperature so as to cause carbon to penetrate into the steel part at a carbon concentration such that the steel part and the carbon form a hypoeutectoid composition, and slowly cooling the steel part penetrated with the carbon; and A quenching step is performed after the carburizing step, wherein the steel component is heated again to a temperature equal to or higher than the austenite transformation end temperature, and the heated steel component is rapidly cooled.

2. The method for manufacturing a steel component according to claim 1, wherein: After the carburizing step and before the quenching step, a nitriding step is further provided in which nitrogen is infiltrated into the steel part in a state where the steel part is heated to a temperature that does not reach the austenitizing end temperature.

3. The method for manufacturing a steel component according to claim 2, wherein: The quenching step is a step of heating the steel member from a temperature that has not reached the austenitizing end temperature to a temperature equal to or higher than the austenitizing end temperature immediately after the nitriding step, and rapidly cooling the heated steel member.

4. The method for manufacturing a steel component according to claim 2, wherein: The nitriding step is a step of infiltrating nitrogen into the steel part at a temperature not lower than the austenitizing start temperature and lower than the austenitizing end temperature.

5. The method for manufacturing a steel component according to claim 2, wherein: The nitriding step is a step of allowing nitrogen to penetrate into the steel component so that the nitrogen concentration on the surface of the steel component becomes 0.5% or less.

6. The method for manufacturing a steel component according to claim 1, wherein: The carburizing step is performed on the cold-forged steel component.