Carbon nanowire / porous glassy carbon composite material and preparation method thereof

By depositing carbon nanowires on the porous glass carbon surface, the problem of poor thermal conductivity of existing porous glass carbon is solved, its thermal conductivity and compressive strength are improved, and it is suitable for thermal management and structural materials in the high-tech field.

CN118791322BActive Publication Date: 2024-11-15湖南德智新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411274011.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-15
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The existing porous glass carbon prepared with phenolic resin as the carbon source precursor has poor thermal conductivity and poor mechanical properties in the application of thermal management materials, which limits its further application in the field of high-tech.

Method used

Under alkaline conditions, a phenol derivative containing a nitrogen-doped element is reacted with a boron-doped element-doped element to prepare a phenolic resin, and a porous glass carbon is obtained by foaming, curing, and carbonization treatment, and then passed through the surface of the body through Carbon nanowires were deposited by CVD method to form carbon nanowires/porous glass carbon composite material.

Benefits of technology

The thermal conductivity and compression strength of porous glass carbon are improved, and a carbon nanowire/porous glass carbon composite material with high thermal conductivity and high compression strength is suitable for thermal management and structural materials in the high-tech field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791322B_ABST
    Figure CN118791322B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of carbon nanowires / porous glassy carbon, and provides a carbon nanowire / porous glassy carbon composite material and a preparation method thereof, the preparation method comprising: under alkaline conditions, mixing a phenol derivative containing a first doping element and a formaldehyde derivative containing a second doping element, and reacting to obtain a phenolic resin; the first doping element includes nitrogen, and the second doping element independently includes boron, nitrogen, or boron and nitrogen; foaming the phenolic resin to obtain a foamed phenolic resin; mixing a thermosetting resin with the foamed phenolic resin and curing them to obtain a cured product; loading a metal ion catalyst onto the cured product to obtain a precursor; carbonizing the precursor to obtain porous glassy carbon; depositing carbon nanowires on the surface of the porous glassy carbon by a CVD method to obtain a carbon nanowire / porous glassy carbon composite material. The carbon nanowire / porous glassy carbon composite material provided by the preparation method of the present invention has high thermal conductivity and compressive resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon nanowire / porous glassy carbon, and in particular to a carbon nanowire / porous glassy carbon composite material and a preparation method thereof. Background Art

[0002] Porous carbon material is a lightweight porous material with a three-dimensional network structure. It has light weight, high specific surface area, excellent elasticity, high temperature stability, chemical corrosion resistance and excellent biocompatibility. It has great potential application value in aerospace, electronics, corrosion, high temperature, chemistry and biomedicine.

[0003] Porous glassy carbon (also known as hard carbon, hard carbon) derived from phenolic resin has high hardness and strength, excellent elasticity, chemical corrosion resistance, high temperature stability and excellent biocompatibility. It is very suitable for lightweight, high-strength and extreme environment material structures and can be widely used in various fields such as high temperature, corrosion, friction, chemistry and biomedicine.

[0004] However, the porous glassy carbon currently prepared using phenolic resin as a carbon source precursor has poor thermal conductivity and mechanical properties when used in thermal management materials, which limits its further application in high-tech fields.

[0005] Therefore, there is an urgent need to provide a method for preparing porous glassy carbon with high thermal conductivity using phenolic resin as a precursor. Summary of the invention

[0006] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide a carbon nanowire / porous glassy carbon composite material and a preparation method thereof. The carbon nanowire / porous glassy carbon composite material obtained by the preparation method of the present invention has high thermal conductivity and electrical conductivity.

[0007] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a method for preparing a carbon nanowire / porous glassy carbon composite material, the method comprising: (1) under alkaline conditions, mixing a phenol derivative containing a first doping element and a formaldehyde derivative containing a second doping element, and reacting them to obtain a phenolic resin; the first doping element comprises nitrogen, and the second doping element independently comprises boron, nitrogen, or boron and nitrogen; the molar ratio of the phenol derivative containing the first doping element to the formaldehyde derivative containing the second doping element is 1:0.5-2; (2) foaming the phenolic resin to obtain a foamed phenolic resin, the foaming method comprising: adding a foaming agent to the phenolic resin for foaming, the foaming agent and the phenolic resin The mass ratio of the thermosetting resin to the foamed phenolic resin is 1:3-8; (3) mixing a thermosetting resin with a foamed phenolic resin and curing them to obtain a cured product, wherein the mass ratio of the thermosetting resin to the foamed phenolic resin is 1:1-6; (4) loading a metal ion catalyst onto the cured product to obtain a precursor, wherein the mass ratio of the metal ion catalyst to the cured product is 1:10-50; (5) carbonizing the precursor to obtain porous glassy carbon; (6) depositing carbon nanowires on the surface of the porous glassy carbon by a CVD method to obtain a carbon nanowire / porous glassy carbon composite material; in step (1), the reaction conditions include: a temperature of 60°C-150°C, a reaction time of 5h-10h, and a pH of 8-12.

[0008] Preferably, in step (6), the flow ratio of the carbon-containing gas to the hydrogen is 1:4-16.

[0009] Preferably, the phenol derivative containing the first doping element includes at least one of 3-morpholinephenol, p-nitrophenol, o-aminophenol and p-aminophenol.

[0010] Preferably, the formaldehyde derivative containing the second doping element includes at least one of 3-formylfuran-2-boric acid, azole-2-carboxaldehyde, 5-pyrimidinecarboxaldehyde, 4-quinolinecarboxaldehyde, 2-formylphenylboronic acid methyliminodiacetate, 5-formylfuran-2-boric acid methyliminodiacetate, 4-formylphenylboric acid and 4-hydroxyphenylboronic acid-1,3-propylene glycol ester.

[0011] The second aspect of the present invention provides a carbon nanowire / porous glassy carbon composite material obtained by the preparation method described in the first aspect.

[0012] Preferably, the porosity of the carbon nanowire / porous glassy carbon composite material is 30%-85%, and the specific surface area of ​​the carbon nanowire / porous glassy carbon composite material is 3000-6000m 2 / g.

[0013] Preferably, the porous glassy carbon has a porosity of 50%-97% and a specific surface area of ​​2000-4000m2 / g.

[0014] Preferably, in the carbon nanowire / porous glassy carbon composite material, the content of carbon nanowires is 5wt%-45wt%, and the content of porous glassy carbon containing metal ion catalyst is 55wt%-95wt%.

[0015] Preferably, the thermal conductivity of the carbon nanowire / porous glassy carbon composite material is 50-200 W (mK).

[0016] Preferably, the carbon nanowire / porous glassy carbon composite material has a compressive strength of 30-60 MPa.

[0017] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0018] The present invention prepares a phenolic resin by reacting a phenol derivative containing a first doping element and a formaldehyde derivative containing a second doping element, and foams the phenolic resin. The foamed phenolic resin is then mixed with a thermosetting resin, and porous glassy carbon with high thermal conductivity and high compressive strength is obtained after carbonization. Furthermore, carbon nanowires are in situ grown on the porous glassy carbon to obtain a carbon nanowire / porous glassy carbon composite material with higher thermal conductivity and greater compressive strength.

[0019] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. DETAILED DESCRIPTION

[0020] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0021] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0022] A first aspect of the present invention provides a method for preparing a carbon nanowire / porous glassy carbon composite material, the method comprising:

[0023] (1) under alkaline conditions, mixing a phenol derivative containing a first doping element and a formaldehyde derivative containing a second doping element, and reacting them to obtain a phenolic resin; the first doping element includes nitrogen, and the second doping element independently includes boron, nitrogen, or boron and nitrogen; the molar ratio of the phenol derivative containing the first doping element to the formaldehyde derivative containing the second doping element is 1:0.5-2; (2) foaming the phenolic resin to obtain a foamed phenolic resin, wherein the foaming treatment comprises: adding a foaming agent to the phenolic resin for foaming, and the mass ratio of the foaming agent to the phenolic resin is 1:3-8; (3) mixing a thermosetting resin with a foaming agent; The phenolic resin is mixed and cured to obtain a cured product, wherein the mass ratio of the thermosetting resin to the foamed phenolic resin is 1:1-6; (4) a metal ion catalyst is loaded onto the cured product to obtain a precursor, wherein the mass ratio of the metal ion catalyst to the cured product is 1:10-50; (5) the precursor is carbonized to obtain porous glassy carbon; (6) carbon nanowires are deposited on the surface of the porous glassy carbon by a CVD method to obtain a carbon nanowire / porous glassy carbon composite material; in step (1), the reaction conditions include: a temperature of 60°C-150°C, a reaction time of 5h-10h, and a pH of 8-12.

[0024] In some embodiments, the phenol derivative containing the first doping element includes at least one of 3-morpholinephenol, p-nitrophenol, o-aminophenol, and p-aminophenol.

[0025] In some embodiments, the formaldehyde derivative containing the second doping element includes at least one of 3-formylfuran-2-boric acid, azole-2-carboxaldehyde, 5-pyrimidinecarboxaldehyde, 4-quinolinecarboxaldehyde, 2-formylphenylboronic acid methyliminodiacetate, 5-formylfuran-2-boric acid methyliminodiacetate, 4-formylphenylboronic acid and 4-hydroxyphenylboronic acid-1,3-propylene glycol ester.

[0026] In step (1), the reaction conditions include: a temperature of 60°C-150°C, such as 60°C, 70°C, 75°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, and 150°C; a reaction time of 5h-10h, such as 5h, 6h, 7h, 8h, 9h, and 10h; and a pH of 8-12, such as 8, 9, 10, 11, and 12. In the present invention, the pH may be adjusted to 8-12 by mixing a phenol derivative containing a first doping element and a formaldehyde derivative containing a second doping element, and then adding an alkaline solution thereto to adjust the pH of the mixed solution to 8-12.

[0027] In some embodiments, the preparation method of step (1) comprises: mixing a phenol derivative containing a first doping element and a formaldehyde derivative containing a second doping element, and then adding an alkaline solution thereto to adjust the pH of the mixed solution to 8-12.

[0028] In some embodiments, the mixed solution with a pH of 8-12 is heated to 60° C.-150° C. and reacted for 5 h-10 h to obtain a phenolic resin.

[0029] The solute of the alkaline solution in the present invention is not particularly limited, as long as the pH of the mixed solution can be adjusted to 8-12, for example, it can be NaOH or KOH.

[0030] The molar ratio of the phenol derivative containing the first doping element to the formaldehyde derivative containing the second doping element is 1:0.5-2, for example, 1:0.5, 1:0.8, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.5, 1:1.7, 1:1.9 and 1:2.

[0031] In step (2), the conditions for the foaming treatment include: a temperature of 150°C-200°C, for example, 150°C, 160°C, 170°C, 180°C, 190°C and 200°C, and a constant temperature time of 60min-360min, for example, 60min, 100min, 150min, 200min, 250min, 300min and 360min.

[0032] In some embodiments, the equipment for the foaming treatment is not particularly limited, and may be, for example, a high-temperature reactor.

[0033] In some embodiments, the foaming treatment conditions include heating to 150°C-200°C at a heating rate of (1-10)°C / min, maintaining the temperature for 60min-360min, and then cooling down. The cooling method may be natural cooling. The heating rate may be 1°C / min, 2°C / min, 4°C / min, 6°C / min, 8°C / min, and 10°C / min.

[0034] In some embodiments, the foaming treatment method includes: adding a foaming agent to the phenolic resin for foaming.

[0035] The mass ratio of the foaming agent to the phenolic resin is 1:3-8, for example, 1:3, 1:4, 1:5, 1:6, 1:7 and 1:8.

[0036] In some embodiments, the mass ratio of the foam leveling agent to the phenolic resin is 1:8-12, for example, 1:8, 1:9, 1:10, 1:11 and 1:12.

[0037] In some embodiments, the blowing agent includes n-pentane and / or isopentane.

[0038] In some embodiments, the foam leveling agent comprises Tween 80 and / or silicone oil.

[0039] In some embodiments, the foaming agent is n-pentane, and the foam leveling agent is Tween 80.

[0040] In some embodiments, before the phenolic resin is foamed, it is pretreated by keeping it at 50°C-80°C for 90min-180min, such as 50°C, 60°C, 70°C and 80°C, which is beneficial to remove impurities in the phenolic resin and improve the foaming efficiency.

[0041] In some embodiments, the foamed phenolic resin obtained after the foaming treatment is post-treated, such as being soaked and washed with distilled water and acetone for several times, so as to remove a small amount of foaming agent and foam leveling agent remaining in the foamed phenolic resin.

[0042] In step (3), the mass ratio of the thermosetting resin to the foamed phenolic resin is 1:1-6, for example, 1:1, 1:2, 1:3, 1:4, 1:5 and 1:6.

[0043] In some embodiments, the thermosetting resin includes at least one of furfural resin, epoxy resin, and furan resin.

[0044] In some embodiments, the thermosetting resin is mixed with the foamed phenolic resin and then cured.

[0045] In some embodiments, in step (4), the method of loading the metal ion catalyst onto the solidified product comprises: immersing the solidified product in a solution containing a metal catalyst.

[0046] The mass ratio of the metal ion catalyst to the cured product is 1:10-50, for example, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45 and 1:50.

[0047] In some embodiments, the metal ion catalyst includes at least one of a soluble salt of Fe, Co, Ni, Cu, Zn, Ti.

[0048] In some embodiments, the metal ion catalyst may be at least one of FeCl3, CoCl2, NiCl2, CuCl2, ZnCl2, TiCl2, and AgCl.

[0049] In some embodiments, in step (5), the conditions for carbonization treatment include: a temperature of 700°C-1600°C, for example, 700°C, 800°C, 900°C, 1000°C, 1200°C, 1400°C and 1600°C; a constant temperature time of 30min-540min, for example, 30min, 100min, 200min, 240min, 280min, 300min, 320min, 360min, 400min, 440min, 500min and 540min.

[0050] In some embodiments, the conditions of the carbonization treatment include: a heating rate of 2°C / h-30°C / h, for example, 2°C / h, 4°C / h, 8°C / h, 10°C / h, 14°C / h, 18°C / h, 20°C / h, 24°C / h, 28°C / h and 30°C / h.

[0051] In some embodiments, the equipment for the carbonization treatment is not particularly limited, as long as the carbonization purpose can be achieved, for example, it can be a tubular furnace.

[0052] In some embodiments, the carbonization treatment conditions include: placing the precursor in a tubular furnace, introducing nitrogen, heating to 700°C-1600°C, such as 700°C, 800°C, 1000°C, 1200°C, 1400°C and 1600°C, keeping the temperature constant for 30min-540min, and finally cooling to room temperature to obtain porous glassy carbon.

[0053] In some embodiments, in step (6), the deposition conditions include: a deposition temperature of 800°C-1600°C, for example, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C and 1600°C; a deposition pressure of 5kPa-16kPa, for example, 5kPa, 8kPa, 9kPa, 10kPa, 12kPa, 14kPa and 16kPa; and a deposition time of 180min-900min, for example, 180min, 200min, 300min, 360min, 400min, 420min, 500min, 540min, 600min, 700min, 800min and 900min.

[0054] In some embodiments, the gas used in the deposition process includes a carbon-containing gas and hydrogen.

[0055] In some embodiments, the flow ratio of the carbon-containing gas to the hydrogen is 1:4-16, for example, 1:4, 1:6, 1:8, 1:10, 1:12, 1:14 and 1:16.

[0056] In some embodiments, the carbon-containing gas includes at least one of methane, ethylene, acetylene, and vinyl acetate.

[0057] In some embodiments, the deposition equipment is not particularly limited as long as it can meet actual needs, for example, it can be a tubular furnace.

[0058] In some embodiments, before depositing carbon nanowires on the surface of porous glassy carbon, the porous glassy carbon is pretreated by placing the porous glassy carbon in a tubular furnace, introducing nitrogen, and heating the furnace to 800° C.-1600° C. to remove impurities in the porous glassy carbon.

[0059] In some embodiments, the preparation method of carbon nanowires deposited on the surface of porous glassy carbon includes: heating the deposition furnace containing the porous glassy carbon to 800°C-1600°C, and after the deposition pressure is 5kPa-16kPa, stopping the introduction of nitrogen, and introducing carbon-containing gas and hydrogen so that the flow ratio of the carbon-containing gas and hydrogen is 1:4-16, and after maintaining the temperature for 30min-300min, a carbon nanowire / porous glassy carbon composite material is obtained.

[0060] The second aspect of the present invention provides a carbon nanowire / porous glassy carbon composite material obtained by the preparation method described in the first aspect.

[0061] In some embodiments, the carbon nanowire / porous glassy carbon composite material has a porosity of 30%-85%, such as 30%, 40%, 50%, 60%, 70%, 80% and 85%, and a specific surface area of ​​the carbon nanowire / porous glassy carbon composite material of 3000-6000m 2 / g, such as 3000m 2 / g、3500m 2 / g, 4000m 2 / g, 4500m 2 / g、5000m 2 / g、5500m 2 / g and 6000m 2 The porosity test method of the carbon nanowire / porous glassy carbon composite material is GB / T 25995-2010 fine ceramic density and apparent porosity test method for testing bulk density and porosity, and the specific surface area test method is GB / T 19587-2004 gas adsorption BET method for determining the specific surface area of ​​solid substances.

[0062] In some embodiments, the porous glassy carbon has a porosity of 50%-97%, for example, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90% and 97%, and a specific surface area of ​​2000-4000m 2 / g, such as 2000m 2 / g、2500m 2 / g、3000m 2 / g、3500m 2 / g and 4000m 2 The porous glassy carbon porosity test method is GB / T 25995-2010 fine ceramic density and apparent porosity test method to test bulk density and porosity, and the specific surface area test method is GB / T 19587-2004 gas adsorption BET method to determine the specific surface area of ​​solid substances to test the specific surface area.

[0063] In some embodiments, in the carbon nanowire / porous glassy carbon composite material, the content of carbon nanowires is 5wt%-45wt%, such as 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt% and 45wt%, and the content of porous glassy carbon containing metal ion catalyst is 55wt%-95wt%, such as 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, 85wt%, 90wt% and 95wt%.

[0064] In some embodiments, the thermal conductivity of the carbon nanowire / porous glassy carbon composite material is 50-200 W / mK, for example, 50 W / mK, 70 W / mK, 90 W / mK, 100 W / mK, 120 W / mK, 140 W / mK, 150 W / mK, 170 W / mK, 190 W / mK and 200 W / mK. The thermal conductivity is tested by GB / T 22588-2008 flash method for measuring thermal diffusivity or thermal conductivity for measuring thermal conductivity.

[0065] In some embodiments, the carbon nanowire / porous glassy carbon composite material has a compressive strength of 30-60 MPa, such as 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, 55 MPa and 60 MPa. The compressive strength is tested by GB / T 8489-2006 Fine Ceramics Compressive Strength Test Method to test compressive strength.

[0066] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0067] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0068] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0069] Example 1

[0070] This example is used to illustrate the preparation method of the carbon nanowire / porous glassy carbon composite material of the present invention.

[0071] (1) Preparation of phenolic resin: p-Aminophenol and 3-formylfuran-2-boric acid in a molar ratio of 1:1 were added into a three-necked flask and mixed evenly. NaOH was added to adjust the pH value of the solution to 10. The reaction mixture was heated to 90°C and stirred for 7 h to obtain phenolic resin.

[0072] (2) Preparation of foamed phenolic resin: Take 100 parts of phenolic resin, heat it to 180°C at a heating rate of 1°C / h to obtain a pretreated phenolic resin, then add 20 parts of n-pentane and 10 parts of Tween 80, stir evenly, place it in a high-pressure reactor, keep the temperature constant for 120 minutes, then cool it naturally and release the pressure to normal pressure to obtain a foamed phenolic resin, and then soak and wash it with distilled water and acetone to remove impurities.

[0073] (3) Preparation of a cured product: 24 parts of furan resin and 96 parts of foamed phenolic resin were mixed and placed in a mold for curing to obtain a cured product.

[0074] (4) Preparation of precursor: The cured product is immersed in a FeCl3 solution and dried to obtain a precursor. The mass ratio of the metal ion catalyst to the cured product is 1:35.

[0075] (5) Preparation of porous glassy carbon: Place the precursor in a tubular furnace, introduce nitrogen, raise the temperature to 1100°C, keep the temperature constant for 300 min, and then cool down to obtain porous glassy carbon.

[0076] (6) Preparation of carbon nanowire / porous glassy carbon composite material: Porous glassy carbon was placed in a tubular furnace and nitrogen was introduced. After the temperature was raised to 1100°C, the introduction of nitrogen was stopped and ethylene and hydrogen were introduced at a pressure of 10.5 kPa. After maintaining the temperature for 420 minutes, a carbon nanowire / porous glassy carbon composite material was obtained, wherein the gas flow ratio of ethylene to hydrogen was 1:8.

[0077] Example 2

[0078] This example is used to illustrate the preparation method of the carbon nanowire / porous glassy carbon composite material of the present invention.

[0079] (1) Preparation of phenolic resin: p-nitrophenol and 2-formylphenylboronic acid methyliminodiacetate in a molar ratio of 1:0.8 were added into a three-necked flask and mixed evenly. NaOH was added to adjust the pH value of the solution to 9. The reaction mixture was heated to 70°C and stirred for 6 hours to obtain phenolic resin.

[0080] (2) Preparation of foamed phenolic resin: Take 100 parts of phenolic resin, heat it to 160°C at a heating rate of 1°C / h to obtain a pretreated phenolic resin, then add 30 parts of n-pentane and 12 parts of Tween 80, stir evenly, place it in a high-pressure reactor, keep the temperature constant for 80 minutes, then cool it naturally and release the pressure to normal pressure to obtain a foamed phenolic resin, and then soak and wash it with distilled water and acetone to remove impurities.

[0081] (3) Preparation of a cured product: 40 parts of furan resin and 80 parts of foamed phenolic resin were mixed and placed in a mold for curing to obtain a cured product.

[0082] (4) Preparation of precursor: The cured product is immersed in a AgCl2 solution and dried to obtain a precursor. The mass ratio of the metal ion catalyst to the cured product is 1:30.

[0083] (5) Preparation of porous glassy carbon: Place the precursor in a tubular furnace, introduce nitrogen, raise the temperature to 950°C, maintain the temperature for 240 min, and then cool down to obtain porous glassy carbon.

[0084] (6) Preparation of carbon nanowire / porous glassy carbon composite material: Porous glassy carbon was placed in a tubular furnace and nitrogen was introduced. After the temperature was raised to 950°C, the introduction of nitrogen was stopped and ethylene and hydrogen were introduced at a pressure of 9 kPa. After maintaining the temperature for 360 minutes, a carbon nanowire / porous glassy carbon composite material was obtained. The gas flow ratio of ethylene to hydrogen was 1:6.

[0085] Example 3

[0086] This example is used to illustrate the preparation method of the carbon nanowire / porous glassy carbon composite material of the present invention.

[0087] (1) Preparation of phenolic resin: 3-morpholinephenol and 4-hydroxyphenylboronic acid-1,3-propylene glycol ester in a molar ratio of 1:1.2 were added into a three-necked flask and mixed evenly. NaOH was added to adjust the pH value of the solution to 11. The reaction mixture was heated to 120°C and stirred for 9 hours to obtain phenolic resin.

[0088] (2) Preparation of foamed phenolic resin: Take 100 parts of phenolic resin, heat it to 190°C at a heating rate of 1°C / h to obtain a pretreated phenolic resin, then add 13 parts of n-pentane and 9 parts of Tween 80, stir evenly, place it in a high-pressure reactor, keep the temperature constant for 300 minutes, then cool it naturally and release the pressure to normal pressure to obtain a foamed phenolic resin, and then soak and wash it with distilled water and acetone to remove impurities.

[0089] (3) Preparation of a cured product: 20 parts of furan resin and 100 parts of foamed phenolic resin were mixed and placed in a mold for curing to obtain a cured product.

[0090] (4) Preparation of precursor: The cured product is immersed in a NiCl2 solution and dried to obtain a precursor. The mass ratio of the metal ion catalyst to the cured product is 1:40.

[0091] (5) Preparation of porous glassy carbon: Place the precursor in a tubular furnace, introduce nitrogen, raise the temperature to 1200°C, and keep the temperature constant for 360 min. After cooling, porous glassy carbon can be obtained.

[0092] (6) Preparation of carbon nanowire / porous glassy carbon composite material: Porous glassy carbon was placed in a tubular furnace and nitrogen was introduced. After the temperature was raised to 1300°C, the introduction of nitrogen was stopped and ethylene and hydrogen were introduced at a pressure of 12 kPa. After maintaining the temperature for 540 minutes, a carbon nanowire / porous glassy carbon composite material was obtained, wherein the gas flow ratio of ethylene to hydrogen was 1:10.

[0093] Example 4

[0094] This example is used to illustrate the preparation of carbon nanowire / porous glassy carbon composite materials when the molar ratio of the phenol derivative containing the first doping element to the formaldehyde derivative containing the second doping element in step (1) is different.

[0095] Example 4-1

[0096] The operation was carried out according to the method described in Example 1, except that the molar ratio of the phenol derivative containing the first doping element to the formaldehyde derivative containing the second doping element was 1:0.5.

[0097] Example 4-2

[0098] The operation was carried out according to the method described in Example 1, except that the molar ratio of the phenol derivative containing the first doping element to the formaldehyde derivative containing the second doping element was 1:2.

[0099] Example 4-3

[0100] The operation was carried out according to the method described in Example 1, except that the molar ratio of the phenol derivative containing the first doping element to the formaldehyde derivative containing the second doping element was 1:3.

[0101] Example 5

[0102] This example is used to illustrate the preparation of carbon nanowire / porous glassy carbon composite materials when the mass ratio of thermosetting resin to foamed phenolic resin in step (3) is different.

[0103] Example 5-1

[0104] The method described in Example 1 was followed, except that 60 parts of furan resin and 60 parts of foamed phenolic resin were mixed and placed in a mold for curing to obtain a cured product.

[0105] Example 5-2

[0106] The method described in Example 1 was followed, except that 18 parts of furan resin and 102 parts of foamed phenolic resin were mixed and placed in a mold for curing to obtain a cured product.

[0107] Example 5-3

[0108] The method described in Example 1 was followed, except that 80 parts of furan resin and 40 parts of foamed phenolic resin were mixed and placed in a mold for curing to obtain a cured product.

[0109] Example 6

[0110] This example is used to illustrate the preparation of carbon nanowire / porous glassy carbon composite materials when the mass ratio of the metal ion catalyst to the cured product in step (3) is different.

[0111] Example 6-1

[0112] The operation was carried out according to the method described in Example 1, except that the mass ratio of the metal ion catalyst to the cured product was 1:13.

[0113] Example 6-2

[0114] The operation was carried out according to the method described in Example 1, except that the mass ratio of the metal ion catalyst to the cured product was 1:48.

[0115] Example 6-3

[0116] The operation was carried out according to the method described in Example 1, except that the mass ratio of the metal ion catalyst to the cured product was 1:5.

[0117] Example 7

[0118] This example is used to illustrate the preparation of carbon nanowire / porous glassy carbon composite materials under different deposition conditions in step (6).

[0119] Example 7-1

[0120] The operation was carried out in accordance with the method described in Example 1, except that the porous glassy carbon was placed in a tubular furnace, nitrogen was introduced, and after the temperature was raised to 850°C, the introduction of nitrogen was stopped, and ethylene and hydrogen were introduced at a pressure of 5.5 kPa to obtain a carbon nanowire / porous glassy carbon composite material, wherein the gas flow ratio of ethylene to hydrogen was 1:4.5.

[0121] Example 7-2

[0122] The operation was carried out in accordance with the method described in Example 1, except that the porous glassy carbon was placed in a tubular furnace, nitrogen was introduced, and after the temperature was raised to 1550°C, the introduction of nitrogen was stopped, and ethylene and hydrogen were introduced at a pressure of 15.5 kPa to obtain a carbon nanowire / porous glassy carbon composite material, wherein the gas flow ratio of ethylene to hydrogen was 1:15.

[0123] Example 7-3

[0124] The operation was carried out in accordance with the method described in Example 1, except that the porous glassy carbon was placed in a tubular furnace, nitrogen was introduced, and after the temperature was raised to 600°C, the introduction of nitrogen was stopped, and ethylene and hydrogen were introduced at a pressure of 18 kPa to obtain a carbon nanowire / porous glassy carbon composite material, wherein the gas flow ratio of ethylene to hydrogen was 1:20.

[0125] Comparative Example 1

[0126] This comparative example is used to illustrate the preparation of a carbon nanowire / porous glassy carbon composite material when the raw material for preparing a phenolic resin is not doped with boron and nitrogen elements.

[0127] The process described in Example 1 is followed, except that the raw materials for preparing the phenolic resin in step (1) are phenol and formaldehyde.

[0128] Comparative Example 2

[0129] This comparative example is used to illustrate the preparation of the carbon nanowire / porous glassy carbon composite material when no thermosetting resin is doped in step (3).

[0130] The method described in Example 1 was followed, except that the thermosetting resin in Example 1 was replaced by a foamed phenolic resin.

[0131] Comparative Example 3

[0132] This comparative example is used to illustrate the material prepared when carbon nanowires are not deposited on porous glassy carbon.

[0133] The difference from Example 1 is that step (6) is not performed.

[0134] The content of carbon nanowires, the content of porous glassy carbon containing metal ion catalysts (the content of porous glassy carbon before depositing carbon nanowires, the porous glassy carbon containing metal catalysts), the porosity of porous glassy carbon, the specific surface area of ​​porous glassy carbon, the porosity of carbon nanowire / porous glassy carbon composite materials, and the specific surface area of ​​carbon nanowire / porous glassy carbon composite materials in the above embodiments and comparative examples were measured. The specific results are shown in Table 1.

[0135]

[0136] Test Case

[0137] The carbon nanowire / porous glassy carbon composite materials obtained in the above examples and comparative examples were respectively subjected to the following tests:

[0138] (1) Thermal conductivity:

[0139] GB / T 22588-2008 flash method is used to measure thermal diffusivity or thermal conductivity. The results are shown in Table 2.

[0140] (2) Compression strength:

[0141] GB / T 8489-2006 Fine Ceramics Compression Strength Test Method Test compressive strength, the results are shown in Table 2.

[0142]

[0143] Example 4 is used to illustrate the preparation of carbon nanowire / porous glassy carbon composite materials when the molar ratios of the phenol derivative containing the first doping element and the formaldehyde derivative containing the second doping element are different. When the molar ratios of the reaction raw materials containing the phenol derivative containing the first doping element and the formaldehyde derivative containing the second doping element are different, the porosity and specific surface area of ​​the porous glassy carbon are different, and the thermal conductivity of the prepared carbon nanowire / porous glassy carbon composite materials is different.

[0144] Example 5 is used to illustrate the preparation of carbon nanowire / porous glass carbon composite materials when the mass ratio of thermosetting resin to foamed phenolic resin is different. The porosity and specific surface area of ​​the porous glass carbon prepared when the mass ratio of thermosetting resin to foamed phenolic resin is different are different, so that the porosity and specific surface area of ​​the carbon nanowire / porous glass carbon composite material finally obtained are also greatly different. Therefore, when the mass ratio of thermosetting resin to foamed phenolic resin is within the protection scope of the present invention, the thermal conductivity of the carbon nanowire / porous glass carbon composite material is better.

[0145] Example 6 is used to illustrate the preparation of carbon nanowire / porous glassy carbon composite materials when the mass ratio of metal ion catalyst to cured product is different. The content of carbon nanowires generated when the mass ratio of metal ion catalyst to cured product is different. When the mass ratio of metal ion catalyst to cured product is within the protection scope of the present invention, the thermal conductivity of the carbon nanowire / porous glassy carbon composite material obtained is better.

[0146] Example 7 is used to illustrate the preparation of carbon nanowire / porous glassy carbon composite materials under different deposition conditions. When the deposition conditions are within the scope of the present invention, the obtained carbon nanowire / porous glassy carbon composite materials have better thermal conductivity and compressive strength.

[0147] Comparative Example 1 is used to illustrate the preparation of carbon nanowire / porous glassy carbon composite materials when the raw materials for preparing phenolic resin are not doped with boron and nitrogen. The carbon nanowire / porous glassy carbon composite materials obtained when the reaction raw materials are not doped with impurity elements have poor thermal conductivity and compressive strength.

[0148] Comparative Example 2 is used to illustrate the preparation of the carbon nanowire / porous glassy carbon composite material without doping with thermosetting resin. The carbon nanowire / porous glassy carbon composite material obtained without doping with thermosetting resin has poor thermal conductivity and compressive strength.

[0149] Comparative Example 3 is used to illustrate the porous glassy carbon composite material obtained when no carbon nanowires are deposited. In this case, the thermal conductivity of the composite material obtained is poor.

[0150] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0151] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a carbon nanowire / porous glassy carbon composite material, characterized in that: The method includes: (1) under alkaline conditions, mixing a phenol derivative containing a first doping element and a formaldehyde derivative containing a second doping element, and reacting them to obtain a phenolic resin; the first doping element includes nitrogen, and the second doping element independently includes boron, nitrogen, or boron and nitrogen; the molar ratio of the phenol derivative containing the first doping element to the formaldehyde derivative containing the second doping element is 1:0.5-2; (2) foaming the phenolic resin to obtain a foamed phenolic resin, wherein the foaming treatment comprises: adding a foaming agent to the phenolic resin for foaming, wherein the mass ratio of the foaming agent to the phenolic resin is 1:3-8; (3) mixing a thermosetting resin and a foamed phenolic resin and curing the mixture to obtain a cured product, wherein the mass ratio of the thermosetting resin to the foamed phenolic resin is 1:1-6; (4) loading a metal ion catalyst onto the cured product to obtain a precursor, wherein the mass ratio of the metal ion catalyst to the cured product is 1:10-50; (5) Carbonizing the precursor to obtain porous glassy carbon; (6) depositing carbon nanowires on the surface of porous glassy carbon by a CVD method to obtain a carbon nanowire / porous glassy carbon composite material; In step (1), the reaction conditions include: temperature of 60°C-150°C, reaction time of 5h-10h, and pH of 8-12.

2. The method according to claim 1, characterized in that In step (2), the conditions for the foaming treatment include: a temperature of 150°C-200°C and a constant temperature time of 60min-360min.

3. The method according to claim 1, characterized in that In step (5), the carbonization treatment conditions include: a temperature of 700°C-1600°C and a constant temperature time of 30min-540min; and / or, In step (6), the gas used in the deposition process includes carbon-containing gas and hydrogen.

4. The method according to claim 3, characterized in that In step (6), the deposition conditions include: a deposition temperature of 800° C. to 1600° C., a deposition pressure of 5 kPa to 16 kPa, and a deposition time of 180 min to 900 min; and / or, The flow ratio of the carbon-containing gas to the hydrogen is 1:4-16.

5. The method according to claim 4, characterized in that The carbon-containing gas includes at least one of methane, ethylene, acetylene and vinyl acetate.

6. The method according to any one of claims 1 to 5, characterized in that: The phenol derivative containing the first doping element includes at least one of 3-morpholinephenol, p-nitrophenol, o-aminophenol and p-aminophenol; and / or, The formaldehyde derivative containing the second doping element includes at least one of 3-formylfuran-2-boric acid, azole-2-carboxaldehyde, 5-pyrimidinecarboxaldehyde, 4-quinolinecarboxaldehyde, 2-formylphenylboronic acid methyliminodiacetate, 5-formylfuran-2-boronic acid methyliminodiacetate, 4-formylphenylboric acid and 4-hydroxyphenylboronic acid-1,3-propylene glycol ester; and / or, The blowing agent comprises n-pentane and / or isopentane; and / or, The thermosetting resin includes at least one of furfural resin, epoxy resin and furan resin; and / or, The metal ion catalyst includes at least one of soluble salts of Fe, Co, Ni, Cu, Zn, and Ti.

7. A carbon nanowire / porous glassy carbon composite material prepared by the method according to any one of claims 1 to 6.

8. The carbon nanowire / porous glassy carbon composite material according to claim 7, characterized in that: The porosity of the carbon nanowire / porous glass carbon composite material is 30%-85%, and the specific surface area of ​​the carbon nanowire / porous glass carbon composite material is 3000-6000m 2 / g; and / or, The porosity of porous glassy carbon is 50%-97% and the specific surface area is 2000-4000m 2 / g.

9. The carbon nanowire / porous glassy carbon composite material according to claim 7, characterized in that: In the carbon nanowire / porous glassy carbon composite material, the content of the carbon nanowire is 5wt%-45wt%, and the content of the porous glassy carbon containing the metal ion catalyst is 55wt%-95wt%.

10. The carbon nanowire / porous glassy carbon composite material according to claim 7, characterized in that: The thermal conductivity of the carbon nanowire / porous glassy carbon composite material is 50-200 W / mK; and / or, The compression strength of the carbon nanowire / porous glassy carbon composite material is 30-60 MPa.