A method for preparing a doped silicon-carbon composite negative electrode material

By using porous carbon to deposit silicon oxide in the negative electrode material of lithium-ion battery and forming a silicon-carbon composite material filled with doped silicon oxide, the first time silicon-based materials are solved in lithium-ion batteries, the low efficiency, poor cycle stability and rate performance of silicon-based materials in lithium-ion batteries are solved. The problem of insufficient results has achieved higher electrochemical performance and stability.

CN118800896BActive Publication Date: 2024-11-15BEIJING IAMETAL NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411280752.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-15
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The existing silicon-based anode materials have problems such as low Coulomb efficiency, poor cycle stability and insufficient rate performance in lithium-ion batteries, especially in fast-charging battery applications, which are difficult to meet high performance needs.

Method used

Porous carbon deposits silicon oxide and vacuum evaporation method to form a silicon-carbon composite material filled with doped silicon oxide on the porous carbon substrate. Metal elements are uniformly distributed in the silicate bonding network to enhance the structure of the material Stability and conductivity.

Benefits of technology

It significantly improves the first-time Coulomb efficiency, rate performance and cycle stability of the negative electrode material of lithium-ion battery, extends the battery life, and simplifies the production process, suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800896B_ABST
    Figure CN118800896B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a doped silicon-carbon composite negative electrode material, which is based on porous carbon, uniformly coated on the inner wall of a deposition collection device, and heated in a vacuum evaporation furnace connected to the collection device to form steam, diffused to the collection device, and silicon deposition and doping of the porous carbon material are performed, and then sintered, and finally carbon coated to obtain the doped silicon-carbon composite negative electrode material. The doped metal element is uniformly distributed in the silicon-carbon material in the form of a silicate bonding network. After metal in-situ doping, an inert bonding network is formed inside the silicon oxide, which plays a role in improving the first coulomb efficiency and reducing irreversible lithium loss, and has better cycle stability and higher first efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery negative electrodes, and in particular relates to a method for preparing a doped silicon-carbon composite negative electrode material. Background Art

[0002] With the rapid development of new energy technologies, lithium-ion batteries and other secondary batteries are increasingly used in electric vehicles, wearable devices and other fields. However, as consumers' expectations for battery performance continue to rise, traditional graphite negative electrode materials can no longer meet the stringent requirements of high-performance batteries, especially fast-charging batteries. In the process of promoting battery technology, fast charging function has become an urgent need of the public. Therefore, the development of negative electrode materials that can meet the fast charging needs of high-performance batteries has become a key challenge currently facing the battery industry.

[0003] At present, the precursors of silicon-based negative electrode materials are mainly silicon and silicon oxide. Compared with silicon oxide, although silicon has a higher capacity (up to 4200 mAh / g), its volume expansion rate is greater (~300%), which is not conducive to the improvement of the cycle stability and safety of lithium-ion batteries. Silicon oxide will irreversibly generate lithium oxide and lithium silicate with lithium ions during the charge and discharge process, which plays a role in buffering the volume expansion of lithium-silicon alloys during the cycle process, and has a longer cycle life and higher safety. However, silicon oxide also has a large volume expansion problem (~150%). The drastic volume expansion will cause the active material to break and pulverize, and then fall off the current collector and lose electrical contact, and will also cause the SEI film to break and regenerate continuously. This process will consume a large amount of active lithium and electrolyte, thereby accelerating the capacity decay and aging of the battery, seriously affecting the battery life, safety and cycle stability. In addition, silicon oxide will generate electrochemically inert lithium oxide and lithium silicate during the first lithium insertion process. This irreversible lithium consumption seriously reduces the first coulomb efficiency of silicon oxide as a negative electrode material, so that the advantages of silicon-based negative electrode materials cannot be effectively exerted.

[0004] At present, the volume expansion and first coulombic efficiency of silicon-based negative electrode materials are mainly improved by element doping and carbon coating. Carbon-coated silicon oxide negative electrode materials combine the advantages of silicon and carbon, aiming to overcome some challenges of silicon materials in lithium-ion batteries. The composite material prepared by compounding silicon and carbon reserves expansion space for the volume expansion of silicon, while at the same time making up for the shortcomings of poor conductivity of silicon and instability of solid electrolyte interface (SEI) film to a certain extent. Although carbon-coated silicon oxide negative electrode materials have high specific capacity and small volume expansion in theory, there are still some shortcomings in practical applications. First, the first efficiency of carbon-coated silicon oxide negative electrode materials is usually low, which means that the number of lithium ions that can effectively participate in the reaction during the first charge and discharge process is small. Secondly, although carbon coating can alleviate the volume expansion of silicon to a certain extent, the carbon coating layer may break during long-term cycling, resulting in a decrease in material performance. The existing technology also includes coating by coating carbon fiber, but the preparation cost of carbon fiber is high, and the processing of silicon oxide layer may affect its fiber structure, which is not conducive to large-scale production.

[0005] Element doping is a commonly used strategy for silicon oxide modification. This method usually involves doping metal elements into silicon oxide materials to improve the performance of silicon oxide negative electrode materials in lithium-ion batteries. By doping a small amount of metal elements into the silicon oxide structure, the irreversible lithium loss can be reduced, thereby improving the first coulombic efficiency of the battery. At the same time, the metal silicates uniformly dispersed in the silicon oxide structure can inhibit the volume expansion of the material to a certain extent. In the existing doping technology, some doping elements can stabilize the structure of the material and reduce the structural damage or phase change that may occur during the charging and discharging process. This stability is not only conducive to extending the cycle life of the battery, but also can improve the coulombic efficiency of the battery. However, due to the intrinsic defects of the material and the type and concentration of the doping elements, this improvement effect may not be significant, and it is difficult to meet the high requirements of fast-charging batteries for the performance of negative electrode materials, resulting in the failure of existing doping methods to fully stimulate and utilize the synergistic effects between doping elements.

[0006] Patent CN114906853A discloses a method for preparing an element-doped silicon oxide / carbon composite material. This method uses a doping source, silicon and silicon dioxide as raw materials to prepare element-doped silicon oxide; the crushed element-doped silicon oxide is coated with a carbon layer by vapor deposition to prepare an element-doped silicon oxide / carbon composite material. This method increases the lithium ion transfer rate of the material by doping silicon oxide with elements, thereby increasing the carrier concentration or introducing a highly conductive metal, so that the element-doped silicon oxide / carbon composite material has a high-rate charge and discharge performance, improves the disadvantage of low lithium ion transfer rate of traditional silicon oxide, and improves its rate performance. However, although element doping may improve electrochemical performance in this patent, it fails to effectively solve the problem of volume expansion of silicon oxide during charging and discharging. While pursuing high energy density, the cycle stability and life of the material may be sacrificed. In order to successfully promote silicon-based anode materials to practical applications, the key is to develop a solution that can effectively solve the three core challenges they face while maintaining the advantages of high energy density of silicon-based materials: low first coulombic efficiency, poor cycle stability and insufficient rate performance. Summary of the invention

[0007] The purpose of the present invention is to solve the problem that the existing silicon-based materials have poor electrochemical performance, and irreversible phases will be formed during the first charge and discharge process. At the same time, during the battery cycle, the agglomeration of the silicon crystal region will significantly reduce its rate performance, further leading to the problems of low first coulombic efficiency and low cycle life of the negative electrode material. Therefore, a porous carbon is provided to deposit silicon oxide, and then form a silicon-carbon negative electrode material filled with doped silicon oxide, and a preparation method and use thereof are provided to improve the first coulombic efficiency, rate performance and cycle performance of the current lithium-ion battery negative electrode material.

[0008] To achieve the above effects, the present invention provides a method for preparing a doped silicon-carbon composite negative electrode material, comprising the following steps:

[0009] (S1) preparing porous carbon, a binder and a solvent into a slurry, vacuum degassing, coating the slurry on the inner wall of a collecting device, and volatilizing and removing the solvent under heating conditions in an inert atmosphere, so that the porous carbon material adheres to the inner wall of the collecting device;

[0010] (S2) in a vacuum evaporation furnace connected to a collecting device, a mixture of a silicon source and a metal doping source is formed into steam under vacuum and high temperature conditions, the steam enters the collecting device by diffusion, the collecting device is maintained at 500-600° C., and silicon is deposited and doped on the porous carbon material adhered to the inner wall of the collecting device; the silicon source is a mixture of silicon and silicon oxides, the metal doping source is a metal element and / or a metal compound, and the metal is an alkali metal and / or an alkaline earth metal;

[0011] (S3) under an inert atmosphere, transferring the collecting device to a sintering furnace, heating the furnace for sintering, and cooling the furnace to obtain a doped silicon-carbon material;

[0012] (S4) The doped silicon-carbon material is carbon-coated to obtain a doped silicon-carbon composite negative electrode material.

[0013] The doped silicon-carbon composite negative electrode material obtained by the present invention uses porous carbon as a substrate, is uniformly coated inside a deposition collection device, and then subjected to vacuum vapor deposition to form a silicon-carbon composite material filled with doped silicon and silicon monoxide, wherein the metal is uniformly distributed in the silicon-carbon material in the form of a silicate bonding network; the metal element is selected from one or more of alkali metals or alkaline earth metals.

[0014] Compared with the existing simple mixing technology, this method coats porous carbon on the inner wall of the collection device, which can make the metal-doped silicon oxide uniformly deposited inside the porous carbon, so that the pore structure of the porous carbon is not destroyed in the subsequent treatment, thereby maintaining its high specific surface area, and enhancing the stability of the internal structure of the porous carbon, reducing the particle cracking of the Si crystal region during the electrochemical process, thereby improving the first coulomb efficiency; it can also make full use of the pore structure of the porous carbon, increase its contact area with the electrolyte, and improve the reaction activity; and provide a good support and conductive network for the metal-doped silicon oxide, which helps to improve its electrochemical performance. In addition, the preparation method of the present invention pre-coats the porous carbon inside the collection device to simplify the subsequent processing process, especially in a high vacuum environment, which can effectively reduce impurity contamination and ensure that the deposited silicon-carbon composite material has a high purity. Moreover, the vacuum evaporation method has the advantages of simple film forming method and easy operation, which is suitable for large-scale production applications.

[0015] Furthermore, in step (S1), the porous carbon is selected from one or more of activated carbon fibers, carbon nanotubes, carbon molecular sieves, and carbon aerogels, and the porous carbon has a particle size of 5-10 μm and a specific surface area of ​​1500-2500 m 2 / g, pore volume is 0.8-1.1cm 3 / g. The thickness of the slurry coating is 1-2cm, and the coating layer cannot be too thick, otherwise it may peel off from the collection device in the subsequent process. The porous structure rich in porous carbon reserves space for the volume expansion of silicon, greatly alleviating the volume expansion rate of silicon during the charging and discharging process. At the same time, the introduction of carbon effectively increases the conductivity of the silicon negative electrode and provides a large number of channels for the diffusion of lithium ions. The binder is selected from at least one of polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC), and polytetrafluoroethylene (PTFE); the solvent is selected from at least one of H2O, butyl acetate, N-methylpyrrolidone, and N,N-dimethylformamide. There is no special limitation on the preparation of slurry, and it is sufficient to mix all materials evenly, such as stirring for 1-5 hours at a rotation speed of 50-100 rpm; vacuum degassing is to evacuate the collection device, and when it is observed that the bubbles in the material have basically disappeared, continue to maintain the vacuum for 0.5-1 hour; the inert atmosphere is nitrogen and / or argon, and the volatilization and removal of solvent under the heating condition is drying at 60-90°C for 5-10 hours to volatilize and remove the solvent, so that the porous carbon material is firmly adhered to the inner wall of the collection device. There is no special limitation on the shape of the collection device, such as cylindrical or cubic.

[0016] Furthermore, in step (S1), the mass ratio of porous carbon, binder and solvent is 100:2-5:50-80,

[0017] Further, in step (S2), further, the alkali metal is lithium, sodium, potassium, and the alkaline earth metal is magnesium and calcium; the metal compound is at least one of metal oxides, hydroxides, carbonates, bicarbonates, and halides (such as metal chlorides, metal bromides, preferably metal chlorides); such as lithium carbonate, lithium hydroxide, lithium nitrate, sodium carbonate, sodium bicarbonate, sodium oxide, sodium chloride, magnesium oxide, magnesium carbonate, calcium oxide, calcium carbonate, calcium bicarbonate, and calcium hydroxide.

[0018] Furthermore, in step (S2), the particle size of silicon is 2-4 μm, the particle size of silicon oxide is 5-8 μm, and the particle size of silicon oxide is 1-5 μm larger than that of silicon, and the particle size of the metal doping source is 5-20 μm. Preferably, when the metal doping source is an alkali metal element and / or an alkali metal compound, the particle size is 15-20 μm; when the metal doping source is an alkaline earth metal element and / or an alkaline earth metal compound, the particle size is 7-12 μm. The size of the raw material particle size will affect the surface area, collision frequency, mass transfer rate and number of active sites per unit mass of the reaction material. Therefore, in the preparation process, controlling the particle size of the raw material is an important process parameter. The particle size is related to the reaction rate. If the particle size is too small, the reaction rate is too fast, resulting in too fast deposition, and the deposition cannot be uniformly deposited in the porous carbon coating, resulting in poor deposition effect. If the particle size is too large, the reaction rate is too slow, and the deposition amount is too small in the same time, and the reactants cannot be completely deposited. The appropriate particle size can make the reactants uniformly deposited in the porous carbon coating within the reaction time. The size of the particle size is related to the material, and different components have different optimal particle size ranges. After a large number of experiments, the inventor unexpectedly obtained a silicon source and a doping source within the above particle size range that can obtain a doped silicon-carbon composite material with the best electrochemical performance.

[0019] Furthermore, in step (S2), the mass ratio of the silicon source to the metal doping source is 3-5:1, such as 4-4.5:1; in the silicon source, the mass ratio of silicon to silicon oxide is 3-7:1, such as 3-4:1; the silicon oxide is silicon dioxide and / or silicon iodide; the mass ratio of the silicon source in step (S2) to the porous carbon in step (S1) is 1.2-2:1, preferably 1.6-1.8:1.

[0020] Furthermore, in step (S2), the vacuum high temperature condition is to raise the temperature to 1250-1450°C at 0.1-10Pa and keep the temperature for 10-20h to form silicon and metal vapor. The generated vapor diffuses into a collection device with a lower temperature, and the temperature of the collection device is maintained at 500-600°C to complete the deposition of silicon and the doping of the metal source.

[0021] Under high temperature and vacuum conditions, silicon and silicon oxide are evaporated from solid to gas and combined into SiO x , in which the metal oxide is reduced to its elemental form by silicon and reacts with SiO x Metal silicate is formed by in-situ doping and is uniformly deposited inside the porous carbon material adhered to the inner wall of the collection device under the drive of temperature difference.

[0022] Furthermore, in step (S3), the temperature is raised to 600-900° C. for sintering for 6-10 hours.

[0023] Further, in step (S4), the carbon coating process is well known in the art. Specifically, a carbon-containing process gas is introduced, and the carbon-containing process gas contacts the doped silicon-carbon material of step (S3) under heating conditions, and the carbon-containing process gas is pyrolyzed, and a carbon layer is deposited on the surface of the doped silicon-carbon material to form a dense carbon coating layer. Preferably, the carbon-containing process gas is selected from at least one of methane, ethane, propane, ethylene, and acetylene, the heating temperature is 800-950°C, the flow rate of the carbon-containing process gas is independently 5-15L / min, and the total amount of carbon-containing process gas introduced is such that the carbon in the carbon coating layer accounts for 3-5wt% of the total mass of the doped silicon-carbon composite negative electrode material.

[0024] The porous carbon substrate in the silicon-carbon composite negative electrode material obtained by the method of the present invention provides the space for volume expansion required for the lithium insertion process of the silicon-based negative electrode material, which can prevent the breakage and pulverization of silicon oxide micron particles, thereby improving the cycle stability of the material; in addition, the porous structure of carbon can also effectively shorten the transmission path of lithium ions and electrons in the battery, inhibiting the SiO x The crystal region agglomeration that occurs in the material during the cycle, and the appropriate stabilization treatment process, effectively improve the material's rate performance and cycle stability. After in-situ metal doping, an inert bonding network is formed inside the silicon oxide, which can directly improve the material's structural modulus and create pores in the particles to reduce the material's volume expansion rate, thereby inhibiting the capacity decay caused by volume change. Secondly, metal element doping can combine with irreversible O, which plays a role in improving the first coulomb efficiency and reducing irreversible lithium loss, and has better cycle stability and higher first efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic diagram of a device for preparing a doped silicon-carbon composite negative electrode material according to the present invention;

[0026] Figure 2 The X-ray diffraction spectrum of the doped silicon-carbon composite negative electrode material prepared in Example 1;

[0027] Figure 3 This is a scanning electron microscope photograph of the doped silicon-carbon composite negative electrode material prepared in Example 1;

[0028] Figure 4 This is the first charge and discharge diagram of the doped silicon-carbon composite negative electrode material prepared in Example 1. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.

[0030] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0031] Figure 1 It is a schematic diagram of the device for preparing doped silicon-carbon composite negative electrode material of the present invention, wherein: 1-vacuum evaporation furnace wall, 2-reaction zone, 3-collection zone, 4-collection device, 5-vacuum pipeline, 6-circulating water cooling chamber, 7-circulating water outlet pipe, 8-circulating water inlet pipe.

[0032] Example 1

[0033] (S1) Pretreatment: First, the inside of the cylindrical collection device was cleaned with anhydrous ethanol to ensure that the porous carbon material could be evenly coated on its surface. Then, a 6.5 μm particle size and a pore volume of 1 cm 3 / g, specific surface area 1800 m 2 / g porous carbon material 10kg, binder (CMC) 0.2kg, solvent H2O 6kg, add into the mixer and mix at 50 r / min for 2 h to form slurry, the slurry is transferred into the vacuum container and gradually evacuated to form a vacuum environment, and the degassing treatment is started. When it is observed that the bubbles in the material have basically disappeared, the vacuum state in the container is maintained for 60min to ensure thorough degassing, and then the slurry is evenly applied to the inner wall of the collecting device with a coating thickness of 2cm. The moisture is removed by drying at 80℃ for 6h in an argon atmosphere, so that the porous carbon is firmly attached to the inner layer of the collecting device.

[0034] (S2) 13.5 kg of silicon oxide with a particle size of 8.0 μm, 4.5 kg of silicon powder with a particle size of 4.0 μm, and 4 kg of lithium oxide powder with a particle size of 16.0 μm are mixed uniformly to obtain a mixture, which is added into a reactor in a vacuum evaporation furnace with a vacuum degree of less than 1 Pa, and the mixture is heated to 1300°C at a heating rate of 10°C / min and then kept warm for 20 hours, while the temperature of the deposition condensation collection zone is always controlled at 600°C. After the reaction is completed, the mixture is naturally cooled to room temperature to obtain a block-shaped porous carbon-deposited silicon oxide composite material.

[0035] (S3) The collection device after deposition is transferred to a sintering furnace under an inert atmosphere with a ventilation flow rate of 5-L / min, and the temperature is increased to 800°C at a rate of 1°C / min for sintering for 7 h. The device is naturally cooled to room temperature under the protection of the inert atmosphere to obtain a block-shaped porous carbon-deposited pre-lithium silicon oxide negative electrode material.

[0036] (S4) The material obtained in (S3) is crushed and added to the coating furnace, nitrogen is filled to exclude air, and the temperature is raised to 920°C at a rate of 10°C / min. After being kept stable for 1.5 hours, acetylene gas is introduced at a flow rate of 10 L / min for 3 hours. This process dehydrogenates acetylene and converts it into a dense carbon layer that coats the material. Then the acetylene gas is turned off, the heating is maintained for 2 hours, and the temperature is lowered and the material is discharged to obtain the product doped silicon-carbon composite negative electrode material. The carbon coating layer accounts for 3.6wt% of the total mass of the doped silicon-carbon composite negative electrode material.

[0037] Figure 2 This is the X-ray diffraction spectrum of the doped silicon-carbon composite negative electrode material prepared in Example 1.

[0038] Figure 3 This is a scanning electron microscope photograph of the doped silicon-carbon composite negative electrode material prepared in Example 1.

[0039] Figure 4 This is the first charge and discharge diagram of the doped silicon-carbon composite negative electrode material prepared in Example 1.

[0040] Example 2

[0041] Other conditions and operations were the same as those in Example 1, except that in step (S1), the binder was changed to PVDF in an amount of 0.5 kg, and the solvent was changed to N-methylpyrrolidone in an amount of 8 kg.

[0042] Example 3

[0043] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixture is changed to 12.8 kg of silicon oxide with a particle size of 5.0 μm, 3.2 kg of silicon powder with a particle size of 2.0 μm, and 4 kg of lithium carbonate powder with a particle size of 20 μm.

[0044] Example 4

[0045] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixture is changed to 12 kg of silicon oxide raw material with a particle size of 8.0 μm, 6 kg of silicon powder with a particle size of 4.0 μm, and 4 kg of lithium oxide powder with a particle size of 16 μm.

[0046] Example 5

[0047] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixture is changed to 15 kg of silicon oxide raw material with a particle size of 8.0 μm, 3 kg of silicon powder with a particle size of 4.0 μm, and 4 kg of lithium oxide powder with a particle size of 16 μm.

[0048] Example 6

[0049] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixture is changed to 13.5 kg of silicon monoxide raw material with a particle size of 8.0 μm, 4.5 kg of silicon powder with a particle size of 4.0 μm, and 6 kg of lithium oxide powder with a particle size of 16 μm.

[0050] Example 7

[0051] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixture is changed to 13.5 kg of silicon monoxide raw material with a particle size of 8.0 μm, 4.5 kg of silicon powder with a particle size of 4.0 μm, and 3 kg of lithium oxide powder with a particle size of 16 μm.

[0052] Example 8

[0053] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixture is changed to 13.5 kg of silicon monoxide with a particle size of 8.0 μm, 4.5 kg of silicon powder with a particle size of 4.0 μm, and 4 kg of magnesium oxide powder with a particle size of 10.0 μm.

[0054] Example 9

[0055] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixture is changed to 13.5 kg of silicon monoxide with a particle size of 4.0 μm, 4.5 kg of silicon powder with a particle size of 5.0 μm, and 4 kg of lithium oxide powder with a particle size of 16.0 μm.

[0056] Comparative Example 1

[0057] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixed material is changed to 18 kg of silicon oxide raw material with a particle size of 8.0 μm and 4 kg of lithium oxide powder with a particle size of 16 μm, that is, no silicon powder is added.

[0058] Comparative Example 2

[0059] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixed material is changed to 18 kg of silicon powder with a particle size of 3.6 μm and 4 kg of lithium oxide powder with a particle size of 16 μm, that is, silicon dioxide is not added.

[0060] Comparative Example 3

[0061] Other conditions and operations are the same as those in Example 1, except that in step (S2), the mixed material is changed to 13.5 kg of silicon oxide raw material with a particle size of 8.0 μm and 4.5 kg of silicon powder with a particle size of 3.6 μm, that is, no lithium oxide powder is added.

[0062] Application Examples

[0063] Performance test of silicon-carbon composite materials as negative electrode materials for lithium batteries

[0064] The doped silicon-carbon composite negative electrode materials prepared in the embodiments and comparative examples of the present invention were subjected to electrochemical performance tests according to the following method: the doped silicon-carbon composite negative electrode material, Super P, carboxymethyl cellulose and styrene-butadiene rubber composite binder were mixed in a mass ratio of 8:1:1 to form a slurry (the mass ratio of CMC and SBR was 1:1), and the slurry was evenly coated on a copper foil with a 200 μm thick scraper, and then vacuum dried for 12 h to prepare a silicon-carbon negative electrode plate; then a metal lithium sheet was used as a counter electrode, a polyolefin was used as a diaphragm, and 1 mol / L LiPF6 (the solvent was a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) was used as an electrolyte, 2% VC and 5% FEC were added to the electrolyte by volume, and button batteries were assembled in an argon atmosphere in a Braun inert gas glove box in Germany.

[0065] The battery assembled above was charged and discharged on a LAND charge and discharge tester, with a charge and discharge range of 50 mV to 1.5 V and a compaction density of 1.1 g / cm 3 After three charge and discharge cycles at a current density of 0.2 C (1 C = 1500 mA / g), the material was charged and discharged at a current density of 0.2C to obtain the capacity, first coulombic efficiency and cycle performance data of the material.

[0066] According to the same method, the silicon-based composite materials obtained in the examples of the present invention and the comparative examples were used as negative electrode materials to assemble button-type lithium batteries, and the electrochemical test results are listed in Table 1.

[0067] Table 1 Electrochemical performance test

[0068] .

[0069] In summary, the preparation method of the present invention is simple and efficient. It can be seen from the data of the embodiments and comparative examples that the preparation method of the present invention forms an inert bonding network inside the material to inhibit crack generation, silicon agglomeration, and reduce the internal expansion of the silicon-based material. The porous structure of the porous carbon substrate effectively buffers the volume expansion of the porous silicon oxide during the charge and discharge process, reduces the internal stress of the particles, and inhibits the SiO x The crystal regions of the material agglomerate during the cycle, so the material's first coulombic efficiency and cycle stability are more advantageous. When vacuum evaporation is performed, the raw materials of the gas source in the vacuum evaporation furnace include silicon powder, silicon oxide, and metal doping source.

Claims

1. A method for preparing a doped silicon-carbon composite negative electrode material, It is characterized in that The following steps are involved: (S1) preparing porous carbon, a binder and a solvent into a slurry, vacuum degassing, coating the slurry on the inner wall of a collecting device, volatilizing and removing the solvent under an inert atmosphere and heating conditions, so that the porous carbon material adheres to the inner wall of the collecting device; (S2) In a vacuum evaporation furnace connected to a collecting device, a mixture of a silicon source and a metal doping source is formed into steam under vacuum and high temperature conditions, and the steam enters the collecting device by diffusion, and the collecting device is maintained at 500-600°C, and silicon deposition and doping are performed on the porous carbon material adhered to the inner wall of the collecting device; the silicon source is a mixture of silicon and silicon oxides, the metal doping source is a metal element and / or a metal compound, and the metal is an alkali metal and / or an alkaline earth metal; the silicon has a particle size of 2-4 μm, and the silicon oxide has a particle size of 5-8 μm, and the silicon oxide particle size is 1-5 μm larger than the silicon particle size; when the metal doping source is an alkali metal element and / or an alkali metal compound, the particle size is 15-20 μm; when the metal doping source is an alkaline earth metal element and / or an alkaline earth metal compound, the particle size is 7-12 μm; (S3) under an inert atmosphere, transferring the collecting device to a sintering furnace, heating the furnace for sintering, and cooling the furnace to obtain a doped silicon-carbon material; (S4) The doped silicon-carbon material is carbon-coated to obtain a doped silicon-carbon composite negative electrode material.

2. The preparation method according to claim 1, It is characterized in that In step (S1), the porous carbon is selected from one or more of activated carbon fibers, carbon nanotubes, carbon molecular sieves, and carbon aerogels, and the porous carbon has a particle size of 5-10 μm and a specific surface area of ​​1500-2500 m 2 / g, pore volume is 0.8-1.1cm 3 / g; and / or the slurry coating thickness is 1-2 cm; and / or The binder is selected from at least one of polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC), and polytetrafluoroethylene (PTFE); the solvent is selected from H 2 O, butyl acetate, N-methylpyrrolidone, at least one of N,N-dimethylformamide.

3. The preparation method according to claim 1, It is characterized in that In step (S1), the mass ratio of porous carbon, binder and solvent is 100:2-5:50-80.

4. The preparation method according to claim 1, It is characterized in that In step (S2), the alkali metal is lithium, sodium, potassium, the alkaline earth metal is magnesium, calcium; the metal compound is metal oxide, hydroxide, carbonate, bicarbonate, halide.

5. The preparation method according to claim 4, It is characterized in that The metal compound is selected from at least one of lithium carbonate, lithium hydroxide, lithium nitrate, sodium carbonate, sodium bicarbonate, sodium oxide, sodium chloride, magnesium oxide, magnesium carbonate, calcium oxide, calcium carbonate, calcium bicarbonate, and calcium hydroxide.

6. The preparation method according to claim 1, It is characterized in that In step (S2), the mass ratio of the silicon source to the metal doping source is 3-5:1; in the silicon source, the mass ratio of silicon to silicon oxide is 3-7:1; the silicon oxide is silicon dioxide and / or silicon iodide; the mass ratio of the silicon source in step (S2) to the porous carbon in step (S1) is 1.2-2:

1.

7. The preparation method according to claim 1, It is characterized in that In step (S2), the vacuum high temperature condition is to raise the temperature to 1250-1450° C. at 0.1-10 Pa and keep it warm for 10-20 hours; and / or In step (S3), the temperature is raised to 600-900° C. for sintering for 6-10 hours.

8. A silicon-carbon negative electrode material, It is characterized in that It is prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Cited By

  • Multi-element synergistically doped nano silicon negative electrode material and preparation method and application thereof

    CN121839636A

  • A multi-element synergistically doped nano-silicon negative electrode material, a preparation method and application thereof

    CN121839636B