Preparation method of controllable degradation magnesium alloy material

The gradient structure is formed on the surface of magnesium alloy through copper ion implantation technology, which solves the problems of controlled degradation and insufficient antibacterial performance of magnesium alloy materials in the existing technology, and realizes the effective mechanical support and infection prevention of magnesium alloy materials in gastrointestinal staplers. suppression, reducing the risk of anastomotic leakage.

CN118808360AActive Publication Date: 2024-10-22CHINA WEAPON SCI ACADEMY NINGBO BRANCH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410877233.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-22
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

It is difficult to realize magnesium alloy materials with controllable degradation and antibacterial properties using existing technology, and the coating preparation process involves the use of toxic solvents and substrate peeling problems, which cannot meet the needs of gastrointestinal staples for mechanical support and infection suppression.

Method used

Copper ion implantation technology is used to form a structural defect layer, a nano-fine-grained layer and a strained coarse-grained layer on the surface of the magnesium alloy. The infection is inhibited and the degradation rate is controlled through the release of copper ions. It is prepared by combining ultrasonic cleaning, inert atmosphere smelting and extrusion preparation methods. Magnesium alloy material with controlled degradation and antibacterial properties.

Benefits of technology

It achieves controllable degradation and antibacterial properties of magnesium alloy materials, meets the mechanical support requirements of gastrointestinal staples, inhibits local infection during the healing process, reduces the incidence of anastomotic leakage, and avoids side effects caused by implant residues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808360A_ABST
    Figure CN118808360A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a controllable degradation magnesium alloy material. The preparation method comprises the following steps: cleaning: removing an oxide film on the surface of a magnesium alloy, and then carrying out ultrasonic cleaning; the magnesium alloy cleaned in the first step is molten under inert atmosphere protection to obtain molten alloy, and the molten alloy is cooled to obtain as-cast magnesium alloy; the as-cast alloy obtained in the second step is subjected to homogenizing heat treatment and extruded, and the extruded magnesium alloy is obtained; wire material preparation: annealing the extruded alloy obtained in the step 3, and then performing multi-pass drawing to obtain a magnesium alloy wire material; and ion implantation: cutting the wire, grinding and cleaning the wire, and performing copper ion implantation on a metal ion implanter equipped with a copper cathode arc source to obtain the controllable degradation magnesium alloy material. Compared with the prior art, the prepared magnesium alloy material provides mechanical support and antibacterial performance in the early stage of healing, is properly and slowly degraded in the middle stage and is degraded at a high rate in the later stage so as to avoid inflammation induction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of biometal materials, and in particular to a method for preparing a controllably degradable magnesium alloy material. Background Art

[0002] In gastrointestinal anastomosis, the use of staplers can shorten the operation time of gastrointestinal anastomosis, reduce postoperative complications, and relieve the pain of patients. However, the surgical staples commonly used in surgery cannot be degraded and will exist permanently in the human body, which is easy to cause adverse reactions such as allergic reactions, foreign body reactions and tissue adhesion. Magnesium and magnesium alloys are considered to be one of the potential candidates for degradable staple materials due to their good biocompatibility and mechanical properties, as well as their ability to be degraded and absorbed in the human environment. It usually takes 30 to 40 days for gastrointestinal anastomosis to heal completely after surgery. From a histological point of view, the gastrointestinal healing process is roughly divided into three stages: the early postoperative period (1 to 3 days) is the mechanical healing stage, the middle period (4 to 15 days) is the biochemical healing stage, and the late period (after 15 days) is the wound maturation stage. In the mechanical healing stage, that is, from the time the gastrointestinal tissue is cut, an inflammatory response of the wound tissue is induced, and the microorganisms around the wound are cleared. At the same time, macrophages induce lymphocytes to release interleukins and interferons, produce vascular endothelial growth factor to promote angiogenesis, and the wound begins to heal. At this time, the wound mainly relies on staples to provide mechanical support. In the biochemical healing stage, the interstitial cells around the blood vessels secrete the matrix and nutrients needed for wound healing, and fibroblasts and smooth muscles migrate to the wound. About 2 weeks after the anastomosis, the proliferation of fibroblasts reaches its peak, new capillaries are generated, and the tension resistance of the wound increases rapidly. In the postoperative wound maturation stage, the connective tissue at the wound gradually matures, the number of macrophages and fibroblasts at the wound decreases, the intestinal epithelial layer is basically restored, and the tension resistance of the wound is further strengthened. Three weeks after the operation, the tension resistance of the wound is restored to about 70% of the original.

[0003] The gastrointestinal tract has different mechanical demands on implanted staples at different healing stages. Therefore, the implanted staples are required to have controlled degradation, that is, they are required to slowly degrade in the early stage of healing of injured tissue to provide sufficient mechanical support; they are required to degrade evenly at an appropriate rate in the middle stage of implantation, and promote endothelial cell proliferation, synthesis and new blood vessel formation at the wound by releasing beneficial ions, so that the wound has a certain pressure tolerance; in the late stage of implantation, the morphological healing of the wound has been completed, and the staples need to be degraded quickly and evenly at an appropriate speed to avoid the occurrence of side effects such as anterior rectal resection syndrome caused by residual implanted staples.

[0004] In addition, clinical studies have found that the probability of anastomotic leakage after colorectal resection is 3% to 20%, and the incidence of anastomotic leakage in low rectal or colon anus is as high as 24%. Severe peritonitis caused by anastomotic leakage may even be life-threatening. Factors leading to anastomotic leakage include: surgical anastomosis technique, local infection of the anastomosis, and excessive tension after anastomosis. Among them, local infection is one of the most common factors causing anastomotic leakage, and it will affect the healing of gastrointestinal anastomosis in the middle and late stages. Studies have found that commensal bacteria in the human intestine, such as Enterococcus faecalis, Pseudomonas aeruginosa, and Serratia marcescens, will transform into highly toxic pathogens due to the inflammatory environment created by the inflammatory response after anastomosis, and dissolve the extracellular matrix by producing proteases, thereby causing anastomotic leakage. Therefore, inhibiting some of the flora at the anastomosis can significantly reduce the incidence of anastomotic leakage.

[0005] The above problems put forward the requirements of controlled degradation and resistance to local infection for the anastomotic staple implants in the body, that is, the implants are required to slowly degrade in the early stage of wounded tissue healing to provide sufficient mechanical support, uniformly degrade in the middle stage to promote tissue healing, and uniformly and rapidly degrade in the late stage to match the degradation rate with the tissue healing rate, and the implants are completely degraded when the tissue is completely healed. In addition, during the healing process of the wound, some bacterial colonies at the anastomosis can be suppressed to avoid anastomotic leakage.

[0006] The disclosed Chinese invention patent "A biodegradable antibacterial magnesium alloy staple and its preparation method" (publication number: CN 117018300 A) obtains a magnesium alloy wire with antibacterial and acid-base resistance by preparing a mixed coating of biopolysaccharides and their derivatives and black phosphorus on the surface of Mg-xCa-yM wire by dipping, spraying or hydrothermal synthesis. However, the organic solvent N-dimethylformamide is used in the coating preparation process. The solvent is toxic and long-term contact will affect the nerves, liver and skin, and even cause cancer. The preparation process of this coating does not meet the current market pursuit of green and environmental protection. In addition, the tail of the staple is bent under stress during use, and the coating on the surface of the staple is prone to bulge or even rupture and fail. This patent does not take into account the problem of the coating peeling off from the substrate when it is under stress.

[0007] The Chinese invention patent "A magnesium alloy surface coating material and its application" (application publication number CN114481074A) deposits a DLC coating on a magnesium alloy through a magnetron sputtering coating device under an argon atmosphere, and then anneals the coating material and places it in an ion implantation device for titanium element implantation to improve the corrosion resistance of medical magnesium alloys in simulated body fluids. This patent prepares a corrosion-resistant coating through two depositions, which has high production costs, slow production efficiency, and complex operations. The degradation rate of the prepared magnesium and magnesium alloys is single, which cannot meet the requirements of human implants for graded degradation of implanted devices. It is necessary to develop an ion implantation surface modification process technology with simple operating steps and that can achieve graded degradation of magnesium and magnesium alloys.

[0008] The Chinese invention patent "A method for preparing antibacterial coating on magnesium and magnesium alloy surface" (application publication number CN114369808A) uses double-layer glow plasma infiltration equipment to deposit Cu elements on the surface of magnesium / magnesium alloy substrates, so that the Mg2Cu gradient distribution in the alloy surface diffusion layer is achieved, and the Cu ion gradient release is achieved to solve different stages of infection such as early postoperative infection and delayed infection. High temperature is one of the characteristics of double-layer glow plasma infiltration technology, which is suitable for the process technology of alloying the surface of high-melting-point metals such as iron-based metals. However, magnesium and magnesium alloys have low melting points, and the structural properties of the substrate are easily changed at such high temperatures. If sputtering is performed at a lower temperature, the infiltration effect is often poor, the infiltration layer is thinner, and generally a deposition layer and a thin diffusion layer are formed on the alloy surface. However, the thin Cu ion diffusion layer has limited ability to inhibit microbial infection.

[0009] Methods for regulating the degradation behavior of medical magnesium alloy staples and imparting them with biomedical functions include severe plastic deformation of the surface layer and preparation of surface coatings. However, there is still much controversy about the effect of severe plastic deformation of magnesium alloys on the corrosion behavior of magnesium and magnesium alloys, and it is necessary to explore process parameters to achieve the optimal degradation rate and mechanical properties. Coating is one of the commonly used methods for surface modification. Currently, the main methods for preparing coatings on the surface of staples are dipping, spraying or hydrothermal synthesis. However, the above methods have poor interfacial bonding properties with the substrate, and the problems of peeling and degradation under stress need to be solved. In addition, due to the addition of organic solvents, long-term contact can easily cause adverse effects on nerves, liver and skin, and the coating is prepared through a solution medium, which does not meet the current market pursuit of green and environmentally friendly production. Summary of the invention

[0010] The technical problem to be solved by the present invention is to provide a method for preparing a controllably degradable magnesium alloy material in response to the above-mentioned technical status quo. The method has simple steps, and the prepared magnesium alloy material is degradable, has good antibacterial properties and can be used in the field of gastrointestinal anastomosis staples, meeting the requirements for controllable degradation of medical metal materials for in vivo implantation.

[0011] The technical solution adopted by the present invention to solve the above technical problems is: a method for preparing a controllably degradable magnesium alloy material, characterized in that it comprises the following steps:

[0012] Step 1: Cleaning: Use phosphoric acid solution to remove the surface oxide film of magnesium alloy and then perform ultrasonic cleaning;

[0013] Step 2, alloy smelting: melting the magnesium alloy cleaned in step 1 under inert atmosphere to obtain a molten alloy, and cooling to obtain a cast magnesium alloy;

[0014] Step 3: Preparation of extruded alloy: firstly subject the cast alloy obtained in step 2 to homogenization heat treatment, and then extrude to obtain extruded magnesium alloy;

[0015] Step 4: Wire preparation: annealing the extruded alloy obtained in step 3, and then performing multiple drawing to obtain magnesium alloy wire;

[0016] Step 5, ion implantation: cutting the wire, grinding and cleaning the wire, and implanting copper ions on a metal ion implanter equipped with a copper cathode arc source to obtain a controllably degradable magnesium alloy material; the controllably degradable magnesium alloy material has a modified layer on its surface, and the modified layer is provided with a structural defect layer, a nano-fine crystal layer, and a strained coarse crystal layer in sequence from the surface to the inside.

[0017] Cu 2+ The concentration of Cu in the range of 65-650 mg / L can kill 99% of Staphylococcus aureus and Pseudomonas aeruginosa, and has no cytotoxicity to fibroblasts. 2+ Concentration ≥10 -5 mol / L, it has a bactericidal effect on Pseudomonas aeruginosa and Enterococcus faecalis. Therefore, if Cu is introduced into gastrointestinal anastomotic staples to release Cu ions during wound healing, the incidence of anastomotic leakage caused by local infection caused by common intestinal bacteria such as Pseudomonas aeruginosa and Enterococcus faecalis can be greatly reduced.

[0018] Preferably, the magnesium alloy wire implanted with copper ions in step 5 is placed on a water-cooled target of a metal ion implanter, the ion implantation angle is 7-10°, the acceleration voltage is 40-50 kV, and the vacuum chamber pressure is 2.0-6.0×10 -4 pa, the injection beam current is 1.0-2.0 mA; the copper ion injection dose is 0.8-3×10 17 ion / cm 2 .

[0019] Placing the wire on a water-cooled target is to ensure that the sample deposition temperature is relatively low, avoiding changes in the sample substrate structure and properties caused by excessively high temperatures during ion implantation.

[0020] The purpose of tilting the ion injection angle is to make the incident direction of the ions not aligned with the lattice channel, reduce the channeling effect, and make the depth of ion injection uniform. If the tilt angle is too large, the ions will be partially blocked, forming a large shadow area, causing a certain deviation between the actual injection area and the designed area. If the tilt angle is too small, the channeling effect cannot be solved well, and it is easy to cause a bimodal distribution. A common way to avoid the channeling effect is to set the injection angle to between 7 and 10° of the crystal plane normal, which helps to disrupt the path of the ions, reduce the probability of ions penetrating along the through channel, ensure the depth of ion injection and reduce the shadow effect of ion injection.

[0021] The acceleration voltage determines the depth and shape of the implanted ion distribution. As the injection acceleration voltage increases, the ion implantation depth increases, but the implantation trajectory dispersion trend decreases with the increase of the acceleration voltage. Considering the uniformity of ion implantation, the most appropriate selection of the magnesium alloy surface implantation depth is 1 to 3 μm, that is, the acceleration voltage is between 40 and 50 kV.

[0022] The entire ion implantation process must be carried out under high vacuum conditions to reduce the probability of collisions between charged ions and neutral gas molecules along the ion trajectory. Collisions will cause scattering and loss of ions, and unwanted ions will be produced during the charge exchange process between ions and neutral atoms, causing radiation pollution. In order to avoid radiation pollution, the vacuum degree should reach the order of 10-4pa. If the vacuum degree is too low, on the one hand, the beam current of the implanter will be relatively small, resulting in a decrease in the injection speed; on the other hand, it will lead to poor focusing of the ion flow, and the purity of the implantation will not meet the requirements, resulting in poor uniformity of the ion implantation depth. The higher the vacuum degree, the straighter the path of the electron beam, and the higher the energy reaching the sample surface, but the higher the energy, the deeper the injection depth, which means that the injection concentration will be smaller. Experimental exploration has found that the optimal pressure of the vacuum chamber is 2.0~6.0×10 -4 pa.

[0023] The injection beam current determines the scanning time. As the current increases, the scanning time shortens, the production capacity increases, and the number of impurity atoms injected per unit time also increases, resulting in poor injection uniformity. If the current is too small, the injection rate is too low, which affects the injection efficiency. Experimental results show that the appropriate injection rate range is 1.0~2.0mA.

[0024] The implantation dose is the total number of ions implanted per unit area of ​​the sample surface, measured in ions per square centimeter. The implantation dose formula is:

[0025]

[0026] where I is the beam current in amperes, t is the injection time in seconds, and q is the electron charge, which is equal to 1.6×10 -19 , n is the charge number of each ion, A is the implantation area in cm 2 .

[0027] The implantation dose determines the implantation depth. When the implantation exceeds a certain dose, point defects such as vacancies and interstitial atoms will be generated in the substrate, and the point defects will recombine to form defects such as dislocations. When high-energy ions are implanted into the alloy surface, the lattice distortion of the substrate surface is caused, which hinders the movement of dislocations, thereby strengthening the alloy. Experiments have found that when the ion implantation exceeds a certain value, the surface hardness of the magnesium alloy no longer continues to increase monotonically, but shows a trend of first decreasing and then increasing. In addition, excessive ion implantation will cause more surface defect problems. The sputtering effect caused by ion implantation will change the roughness of the magnesium alloy surface. Experimental results show that the roughness of the magnesium alloy surface will show a trend of first decreasing and then increasing with the increase of the implantation dose. Generally speaking, the smoother the surface of the alloy, the better its corrosion resistance and mechanical properties. In order to obtain magnesium alloys with the best corrosion resistance and mechanical properties, the most suitable Cu implantation dose is 0.8~3×10 17 ion / cm 2 .

[0028] Preferably, in the step 1, the surface oxide film is removed by pickling with a phosphoric acid solution having a volume fraction of 5-8%.

[0029] Preferably, the extrusion temperature in step 3 is 200-250°C, the extrusion speed is 9-11 mm / s, and the extrusion ratio is 54:1-64:1. This extrusion temperature can greatly prevent dynamic recrystallization during deformation to make the grains coarse, and a large extrusion ratio is conducive to plastic deformation strengthening.

[0030] Preferably, the magnesium alloy in step 1 is one or more of Mg, Mg-Zn, Mg-Mn and Mg-Zn-Mn alloy.

[0031] Preferably, the Mg content of the magnesium alloy is ≥ 98 wt.%.

[0032] Preferably, the step 2 is: using an induction furnace and a graphite crucible to melt the magnesium alloy cleaned in step 1 under the protection of CO2 and SF6 to obtain a molten alloy; pouring the molten alloy into a dry low-carbon steel mold with a BN coating on the inner wall, and cooling to obtain a cast magnesium alloy. Low-carbon steel is carbon steel with a carbon content of less than 0.25%.

[0033] In order to achieve the gradient structure of the surface of the magnesium alloy material and make it degraded in stages, preferably, the surface of the controllably degradable magnesium alloy material has a modified layer, and the modified layer is provided with a structural defect layer, a nano-fine crystal layer and a strained coarse crystal layer in sequence from the surface to the inside. The thickness of the modified layer is 1.5 to 2.1 μm; the outermost region of the modified layer is a structural defect layer with a depth of about 50 to 80 nm, the sub-surface region is a nano-fine crystal layer with a thickness of about 550 to 620 nm, and the innermost layer is a coarse crystal strain layer, the grain size of which is relatively large, and there are many fine precipitates and dislocations. The structural defects in the outermost region caused by ion implantation will accelerate degradation, and because the ion implantation makes the surface Cu element uniformly distributed, the galvanic corrosion is significantly inhibited, making the degradation mode uniform corrosion.

[0034] Preferably, the thickness of the structural defect layer is 50-80nm; the thickness of the nano-fine crystal layer is 550-620nm; the thickness of the strain coarse crystal layer is 870-1430nm. The structural defect layer in this thickness range is the best thickness choice. It not only ensures that in the initial stage of immersion, the most superficial area releases more Cu ions evenly, significantly inhibits bacterial infection in the early stage of surgery, avoids the occurrence of oral leakage during anastomosis surgery, but also avoids excessive degradation of the implant to provide sufficient mechanical support. The nano-fine crystal layer improves the corrosion resistance of the alloy due to its nanostructure and lower phase interface. At the same time, the corrosion-resistant substances such as CuO and MgO on the surface form a barrier to inhibit corrosion, ensuring that it slowly degrades in the middle stage of implantation to provide the mechanical support required for wound healing; the degradation cycle of the 550-620nm thick sub-surface area perfectly matches the mid-stage of healing after gastrointestinal anastomosis.

[0035] Preferably, the grain size of the structural defect layer is 500-580nm; the grain size of the nano-fine grain region is 250-300nm; and the grain size of the strained coarse grain region is 600-750nm. The grain size of the strained coarse grain layer is relatively large, and there are many fine precipitates and dislocations; the average strain accumulation is higher, but the strain difference between different grains is reduced, so the strained coarse grain layer area will degrade in a larger and more uniform degradation mode in the later stage of implantation, achieving rapid degradation at an appropriate rate in the later stage of implantation, avoiding side effects such as inflammation and wound scarring caused by implant residues.

[0036] Preferably, the annealing temperature in step 4 is 280-300°C.

[0037] Compared with the prior art, the advantages of the present invention are:

[0038] ① Adding copper can refine the microstructure of magnesium alloy, enhance mechanical properties and improve the degradation behavior of magnesium alloy; in addition, Cu is also an important factor in wound healing, promoting and inducing angiogenesis and stimulating endothelial cell proliferation; and Cu also has excellent antibacterial properties, so that the prepared magnesium alloy material can avoid the risk of anastomotic leakage in gastrointestinal anastomosis surgery caused by infection with common gastrointestinal bacteria such as Pseudomonas aeruginosa and Enterococcus faecalis.

[0039] ② Ion implantation can introduce beneficial copper elements into the surface of the sample to provide complete mechanical support for the implanted device during tissue healing. Ion implantation will cause structural defects in the outermost layer of the magnesium alloy. The Cu ions in the structural defect layer are released quickly and evenly in the early stage, while the nano-fine-grained layer forms copper oxide due to ion implantation, which inhibits corrosion and reduces the degradation rate. The degradation rate is lower than that of the outermost structural defect layer and the inner strain coarse-grained layer, which meets the requirements of controlled degradation of medical metal materials for in vivo implantation, that is, it is required to provide sufficient mechanical support and antibacterial properties before the healing of injured tissue, degrade slowly and evenly in the middle stage of healing, and degrade at a moderately fast rate in the late stage of healing to avoid inducing side effects such as inflammation. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic diagram of alloy melting of various embodiments of the present invention;

[0041] Figure 2 It is a schematic diagram of hot extrusion of various embodiments of the present invention;

[0042] Figure 3 Schematic diagram of ion implantation according to various embodiments of the present invention;

[0043] Figure 4 Schematic diagram of in vitro antibacterial experiment of various embodiments of the present invention. DETAILED DESCRIPTION

[0044] The present invention is further described in detail below with reference to the accompanying drawings.

[0045] Unless otherwise specified, the reagents and materials used in the examples can be obtained from commercial sources.

[0046] Example 1

[0047] A method for preparing a controllable degradable magnesium alloy material comprises the following steps:

[0048] 1) Cleaning: The pure Mg and Mg-50wt.% Zn master alloys were cleaned with 6% phosphoric acid solution to remove the surface oxide film, and then ultrasonically cleaned in anhydrous ethanol to remove the oxide layer on the surface of the material as well as the attached dust and oil.

[0049] 2) Alloy smelting: Use an induction furnace and a graphite crucible to melt the magnesium alloy cleaned in step 1 in sequence under the protection of CO2 and SF6 inert atmosphere, pour the prepared molten alloy into a dry low-carbon steel mold with a BN coating on the inner wall, and cool it to obtain a cast Mg-0.5wt.%Zn alloy. The alloy smelting process is shown in Figure 1 .

[0050] 3) Preparation of extruded alloy: First, the cast alloy obtained in step 2 was subjected to homogenization heat treatment, and then the surface of the cast alloy was polished with a grinding wheel to remove oil stains, burrs and oxide films on the sample surface. Finally, an extruded Mg-0.5wt.%Zn alloy was prepared at 220℃, a speed of 10mm / s and an extrusion ratio of 64:1. The alloy extrusion process is shown in Figure 2 .

[0051] 4) Wire preparation: The extruded alloy obtained in step 3) is subjected to annealing heat treatment at 290° C., and then subjected to multiple drawing passes at room temperature to obtain a wire a of Φ0.3-0.7 mm.

[0052] 5) Ion implantation: The wire a obtained in step 4) was cut and ground with SIC sandpaper of different particle sizes, ultrasonically cleaned with alcohol for 10 min, and then dried in air. Cu ion implantation was performed on a metal ion implanter equipped with a Cu cathode arc source to obtain a controllable degradation magnesium alloy material. The Cu ion implantation angle was 7°, the acceleration voltage was 40 kV, and the vacuum chamber pressure was 2.0×10 -4 pa, the injection beam current is 1.0 mA, and the Cu ion implantation dose is 0.8×10 17 ion / cm 2 The ion injection process is shown in Figure 3 The diffusion pump 2 removes the gas inside the ion implanter to achieve a high vacuum state; the wire a is placed on the rotating table 1, the ion source 4 generates the required copper ions, and the ion beam 3 is uniformly injected into the wire a.

[0053] Example 2

[0054] A method for preparing a controllable degradable magnesium alloy material comprises the following steps:

[0055] 1) Cleaning: The pure Mg and Mg-15wt.%Mn master alloys were cleaned with 6% phosphoric acid solution to remove the surface oxide film, and then ultrasonically cleaned in anhydrous ethanol to remove the oxide layer on the surface of the material as well as the attached dust and oil.

[0056] 2) Alloy smelting: Use an induction furnace and a graphite crucible to melt the samples in step 1) in sequence under the protection of CO2 and SF6 inert atmosphere. Then, pour the prepared molten alloy into a pre-dried low-carbon steel mold with a BN coating on the inner wall, and cool it to obtain a cast Mg-1wt.%Mn alloy.

[0057] 3) Preparation of extruded alloy: firstly, the cast alloy obtained in step 2) was subjected to homogenization heat treatment, and then the surface of the cast alloy was polished with a grinding wheel to remove the oil, burrs and oxide film on the surface of the sample. Finally, an extruded Mg-1wt.%Mn alloy was prepared at 220°C, a speed of 10mm / s, and an extrusion ratio of 64:1.

[0058] 4) Wire preparation: The extruded alloy obtained in step 3) is subjected to annealing heat treatment at 290° C., and then subjected to multiple drawing passes at room temperature to obtain Φ0.3-0.7 mm wire.

[0059] 5) Ion implantation: The wire obtained in step 4) was cut and ground with SIC sandpaper of different particle sizes, ultrasonically cleaned with alcohol for 10 min, and then dried in air. Cu ion implantation was performed on a metal ion implanter equipped with a Cu cathode arc source to obtain a controllable degradation magnesium alloy material. The ion implantation angle was 10°, the acceleration voltage was 50 kV, and the vacuum chamber pressure was 4.0×10 - 4 pa, the injection beam current is controlled at 2.0 mA. The Cu ion implantation dose is 1.5×10 17 ion / cm 2 .

[0060] Example 3

[0061] A method for preparing a controllable degradable magnesium alloy material comprises the following steps:

[0062] 1) Cleaning: The pure Mg, Mg-50wt.% Zn and Mg-15wt.% Mn master alloys were cleaned with 6% phosphoric acid solution to remove the surface oxide film, and then ultrasonically cleaned in anhydrous ethanol to remove the oxide layer on the surface of the material as well as the attached dust and oil.

[0063] 2) Alloy smelting: According to the designed composition, weigh the sample obtained in step 1). Use an induction furnace and a graphite crucible to melt the sample in step 1) in sequence under the protection of CO2 and SF6 inert atmosphere. Then, pour the prepared molten alloy into a pre-dried low-carbon steel mold with the inner wall coated with BN coating, and cool it to obtain a cast Mg-0.5wt.%Zn-1wt.%Mn alloy.

[0064] 3) Preparation of extruded alloy: firstly, the cast alloy obtained in step 2) was subjected to homogenization heat treatment, and then the surface of the cast alloy was polished with a grinding wheel to remove the oil, burrs and oxide film on the surface of the sample. Finally, an extruded Mg-0.5wt.%Zn-1wt.%Mn alloy was prepared at 220°C, a speed of 10mm / s, and an extrusion ratio of 64:1.

[0065] 4) Wire preparation: The extruded alloy obtained in step 3) is subjected to annealing heat treatment at 290° C., and then subjected to multiple drawing passes at room temperature to obtain Φ0.3-0.7 mm wire.

[0066] 5) Ion implantation: The wire obtained in step 4) was ground with SIC sandpaper of different particle sizes, cleaned with alcohol ultrasonically for 10 min, and then dried in air. Cu ion implantation was performed on a metal ion implanter equipped with a Cu cathode arc source to obtain a controllable degradation magnesium alloy material. The ion implantation angle was 10°, the acceleration voltage was 50 kV, and the vacuum chamber pressure was 6.0×10 - 4 pa, the injection beam current is controlled at 2.0 mA. The Cu ion implantation dose is 3×10 17 ion / cm 2 .

[0067] Comparative Example

[0068] 1) Cleaning: The pure Mg, Mg-50wt.% Zn and Mg-10wt.% Mn master alloys were cleaned with 6% phosphoric acid solution to remove the surface oxide film, and then ultrasonically cleaned in anhydrous ethanol to remove the oxide layer on the surface of the material as well as the attached dust and oil.

[0069] 2) Alloy smelting: According to the designed composition, weigh the sample obtained in step 1). Use an induction furnace and a graphite crucible to melt the sample in step 1) in sequence under the protection of CO2 and SF6 inert atmosphere. Then, pour the prepared molten alloy into a pre-dried low-carbon steel mold with the inner wall coated with BN coating, and cool it to obtain a cast Mg-0.5wt.%Zn-1wt.%Mn alloy.

[0070] 3) Preparation of extruded alloy: firstly, the cast alloy obtained in step 2) was subjected to homogenization heat treatment, and then the surface of the cast alloy was polished with a grinding wheel to remove the oil, burrs and oxide film on the surface of the sample. Finally, an extruded Mg-0.5wt.%Zn-1wt.%Mn alloy was prepared at 220°C, a speed of 10mm / s, and an extrusion ratio of 64:1.

[0071] 4) Wire preparation: The extruded alloy obtained in step 3) is subjected to annealing heat treatment at 290° C., and then subjected to multiple drawing passes at room temperature to obtain Φ0.3-0.7 mm wire.

[0072] The thickness of the surface modified layer was tested for the three examples obtained, and the degradation performance, antibacterial property and biocompatibility of the three examples and one comparative example were tested. The thickness of the surface modified layer was tested by using a hot mounting method to prepare the three examples into electron microscope observation samples, and then polished to 2000# with metallographic sandpaper step by step, and then polished to a mirror surface with a polishing paste of 2.5 μm particle size. After the electron microscope observation sample was cleaned with anhydrous ethanol, the thickness of the surface modified layer was obtained using a field emission scanning electron microscope equipped with an energy spectrometer.

[0073] The obtained examples were tested for the thickness of the surface modified layer, and the examples and comparative examples were tested for degradation performance, antibacterial properties and biocompatibility. The test results are shown in Table 1.

[0074] Test method for thickness of modified layer: The three embodiments were prepared into electron microscope observation samples by hot mounting method, and then polished to 2000# with metallographic sandpaper step by step, and then polished to a mirror surface with a polishing paste of 2.5μm particle size. After cleaning the electron microscope observation sample with anhydrous ethanol, the thickness of the surface modified layer was obtained by a field emission scanning electron microscope equipped with an energy spectrometer. In addition, the grain size of the structural defect layer of embodiments 1-3 was measured to be 500-580nm; the grain size of the nano-fine grain area was 250-300nm; the grain size of the strain coarse grain area was 600-750nm.

[0075] Degradation performance test: Corrosion immersion test was carried out according to ASTM G31-72 standard, and the immersion solution was simulated body fluid. The detailed composition of the simulated body fluid is shown in Table 2. The sample was ultrasonically cleaned with deionized water and anhydrous ethanol, blown dry and weighed. The sample was 0.05 cm 2 / mL immersion ratio was suspended in a centrifuge tube by a thin wire and placed in a 37℃ constant temperature box. The samples were taken out after different immersion times. First, the samples were ultrasonically cleaned with deionized water. The samples were placed in 200g·L -1 Ultrasonic cleaning was performed in CrO3, and after removing the corrosion products, the samples were washed with deionized water, dried, and weighed. Three parallel samples were set up for each immersion experiment. The corrosion products were removed from the three parallel samples and the average corrosion rate was calculated. The corrosion rate calculation formula obtained by the immersion weight loss method is as follows:

[0076]

[0077] Where CR is the corrosion rate (mm·year -1 ), coefficient K = 8.76 × 10 4 , Δm is the loss mass (g), ρ is the material density (g / cm 2 ), A is the initial surface area of ​​the immersed sample (cm 2 ), t is the soaking time (h).

[0078] Antibacterial test: Pseudomonas aeruginosa was selected as the experimental strain to study the antibacterial properties of the material, and LuriaBertani (LB) medium was selected. First, LB medium containing 15-20g agar was poured into a conical flask for high-temperature sterilization. Then, an alcohol lamp was lit on the clean bench, and the conical flask was poured into the culture dish. After the agar solidified, it was inverted and placed in a 37°C incubator for 24 hours. After the inoculated mycelial strain was cultured in a constant temperature shaker at 37°C and 120r / min for 24 hours, the bacterial suspension was collected, and then centrifuged at 7500rpm for 5 minutes in a centrifuge. After discarding the supernatant, the bacteria were collected and the bacterial concentration was controlled at 1×10 8 cfu / mL. The sample to be tested was ultrasonically cleaned with anhydrous ethanol for 5 minutes and then dried. It was sterilized under ultraviolet light for 24 hours before use. The prepared suspension of Pseudomonas aeruginosa was evenly spread on the culture medium plate, and the alloy was placed in the center of the culture medium plate and cultured in a 37°C constant temperature box for 24 hours. The growth morphology of Pseudomonas aeruginosa and the size of the antibacterial ring around the alloy were observed, and the antibacterial performance of the material was calculated by the formula:

[0079] B=(Dd) / 2

[0080] Among them, B: the size of the blank area of ​​the antibacterial ring; D: the diameter of the antibacterial ring; d: the sample diameter, in mm. When B ≥ 1 mm, it means that the material has good antibacterial performance; when B = 0 mm but there are no obvious colonies around, it means that the material has antibacterial performance; when B = 0 but there are obvious colonies growing around, it means that the material has poor antibacterial performance. The schematic diagram of the in vitro antibacterial experiment is as follows Figure 4 shown.

[0081] Biocompatibility test: MTT colorimetry was used to test the biocompatibility of the material. The sample to be tested was immersed in a cell culture medium to prepare an extract. The extract was used to culture rat small intestinal epithelial cells (IEC-6). The cytotoxicity of the material was evaluated by observing the growth of the cells. According to ISO 10993-5:2009 standard, the ratio of sample surface area to culture medium volume was 2 cm 2:3mL extraction ratio for the preparation of material extract, the extraction medium is 5% FBS high glucose DMEM medium (containing 0.01mg / mL insulin). The test material is first ultrasonically cleaned with deionized water and anhydrous ethanol, blown dry and placed in a centrifuge tube filled with anhydrous ethanol for 24 hours for disinfection, and then placed under the ultraviolet lamp of the clean bench for 2 hours. Then the sample is placed in a centrifuge tube with quantitative cell culture fluid and placed in a constant temperature incubator at 5% CO2 and 37°C for 24 hours to obtain an extract. IEC-6 cells are diluted with cell culture fluid to a cell suspension of 105 cells / mL. A 96-well culture plate containing 100μL of cell suspension in each well is placed in a constant temperature incubator at 37°C and 5% CO2 for 24 hours. Then the original cell culture fluid in the 96-well culture plate is removed, and 100μL of extract is added to each well. Each group of experiments has 6 parallel experimental groups, and the negative control group is a complete cell culture fluid. After 24 hours of culture, add 10 μL of MTT (5 mg / mL) to each well of the 96-well culture plate and place it in a constant temperature incubator for 4 hours. After 4 hours, remove the culture medium in the 96-well culture plate and add 100 μL of DMSO solution. Use an ELISA reader to measure the absorbance, and the selected ultraviolet wavelength is 550nm. Repeat the measurement three times and take the average value to calculate the relative cell proliferation rate (RGR, %).

[0082]

[0083] The biocompatibility of materials is evaluated according to the ISO 10993-5:2009 standard: RGR value ≥ 100%, cytotoxicity level 0, non-toxic; RGR value ≥ 80%, cytotoxicity level 1, slightly toxic; RGR value 50% to 80%, cytotoxicity level 2, slightly toxic; RGR value ≤ 49%, cytotoxicity level 3 to 4, unqualified.

[0084] Table 1 Performance of Examples and Comparative Examples

[0085]

[0086] Table 2 Simulated body fluid components for degradation performance test

[0087] Element Content (g) purity NaCl 8.035 99.5﹪ <![CDATA[NaHCO3]]> 0.355 99.5﹪ KCl 0.225 99.5﹪ <![CDATA[K2HPO4·3H2O]]> 0.231 99﹪ <![CDATA[MgCl2·6H2O]]> 0.311 98﹪ c(HCl)=1mol / L 39mL <![CDATA[CaCl2]]> 0.292 95﹪ <![CDATA[Na2SO4]]> 0.072 99﹪ TRIS 6.118 99﹪ c(HCl)=1mol / L 0-5mL

Claims

1. A method for preparing a controllable degradation magnesium alloy material, characterized in that: The following steps are involved: Step 1: Cleaning: remove the surface oxide film of magnesium alloy and then perform ultrasonic cleaning; Step 2, alloy smelting: melting the magnesium alloy cleaned in step 1 under inert atmosphere to obtain a molten alloy, and cooling to obtain a cast magnesium alloy; Step 3: Preparation of extruded alloy: firstly subject the cast alloy obtained in step 2 to homogenization heat treatment, and then extrude to obtain extruded magnesium alloy; Step 4: Wire preparation: annealing the extruded alloy obtained in step 3, and then performing multiple drawing to obtain magnesium alloy wire; Step 5, ion implantation: cutting the wire, grinding and cleaning the wire, and implanting copper ions in a metal ion implanter equipped with a copper cathode arc source to obtain a controllable degradation magnesium alloy material; The controllably degradable magnesium alloy material has a modified layer on its surface, and the modified layer is provided with a structural defect layer, a nano-fine crystal layer and a strain coarse crystal layer in sequence from the surface to the inside.

2. The method for preparing a controllable degradation magnesium alloy material according to claim 1, characterized in that: The magnesium alloy wire implanted with copper ions in step 5 is placed on a water-cooled target of a metal ion implanter, the ion implantation angle is 7-10°, the acceleration voltage is 40-50 kV, and the vacuum chamber pressure is 2.0-6.0×10 -4 pa, the injection beam current is 1.0-2.0 mA; the copper ion injection dose is 0.8-3×10 17 ion / cm 2 .

3. The method for preparing a controllable degradation magnesium alloy material according to claim 1, characterized in that: In the step 1, the surface oxide film is removed by pickling with a phosphoric acid solution having a volume fraction of 5-8%.

4. The method for preparing a controllable degradation magnesium alloy material according to claim 1, characterized in that: The extrusion temperature of step three is 200-250° C., the extrusion speed is 9-11 mm / s, and the extrusion ratio is 54:1-64:

1.

5. The method for preparing a controllable degradation magnesium alloy material according to claim 1, characterized in that: The magnesium alloy in step 1 is one or more of Mg, Mg-Zn, Mg-Mn and Mg-Zn-Mn alloy.

6. The method for preparing a controllably degradable magnesium alloy material according to claim 5, characterized in that: The content of Mg element in the magnesium alloy is ≥98wt.%.

7. The method for preparing a controllable degradation magnesium alloy material according to claim 1, characterized in that: The step 2 is: using an induction furnace and a graphite crucible to melt the magnesium alloy cleaned in step 1 under the protection of CO2 and SF6 to obtain a molten alloy; pouring the molten alloy into a dry low-carbon steel mold with a BN coating on the inner wall, and cooling to obtain a cast magnesium alloy.

8. The method for preparing a controllable degradation magnesium alloy material according to claim 1, characterized in that: The thickness of the structural defect layer is 50-80 nm; the thickness of the nano-fine crystal layer is 550-620 nm; and the thickness of the strained coarse crystal layer is 870-1430 nm.

9. The method for preparing a controllably degradable magnesium alloy material according to claim 1, characterized in that: The grain size of the structural defect layer is 500-580nm; the grain size of the nano-fine grain area is 250-300nm; and the grain size of the strained coarse grain area is 600-750nm.

10. The method for preparing a controllably degradable magnesium alloy material according to claim 1, characterized in that: The annealing temperature in step 4 is 280-300°C.

Citation Information

Patent Citations

  • Composite strengthening method for improving stress corrosion resistance of light alloy

    CN112609068A

  • Method for preparing antibacterial coating on surfaces of magnesium and magnesium alloy

    CN114369808A

  • Degradable pure magnesium or magnesium alloy surface modification method and pure magnesium or magnesium alloy material

    CN115522175A

  • High-temperature auxiliary ion implantation device and processing method

    CN115627450A

  • Properties and parameters of novel biodegradable metallic alloys

    US20200399742A1