A method for preparing a ceramic fiber skeleton rigid thermal insulation material

By using wet chemical self-assembly combined with cerium nitrate and yttrium nitrate and methyl block room temperature vulcanized silicone rubber and other technologies in the rigid thermal insulation materials of ceramic fiber frameworks, the modified alumina fiber and composite coating are formed, and the ceramic fiber is solved. The problem of uneven distribution of raw materials in the preparation of rigid thermal insulation materials of the frame improves the material's airflow erosion performance and stability, extends life and reduces maintenance costs.

CN118812273BActive Publication Date: 2024-11-22SHANDONG RES & DESIGN ACADEMY OF IND CERAMICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411288465.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-22
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

During the preparation process of the ceramic fiber skeleton rigid insulation material, there are uneven distribution of raw material fibers and auxiliary materials, resulting in poor high-speed airflow erosion resistance, low damage tolerance, high maintenance frequency, short service life in actual applications, and other problems. The overall stability Not good.

Method used

The wet chemical self-assembly method of combining cerium nitrate and yttrium nitrate forms a cerium phosphate/yttrium phosphate coating on alumina fibers, and is coated with methyl block room temperature vulcanized silicone rubber and fused silica glass fibers, and is coated by silane pairs. Coupling agent and titanate coupling agent are used to treat borosilicate glass powder, etc., to prepare composite coating agents, and spray-molding to improve the insulation performance and structural stability of the material.

Benefits of technology

It significantly improves the high-speed airflow erosion resistance, damage tolerance and overall stability of the rigid thermal insulation material of ceramic fiber skeleton, extends the service life, reduces maintenance frequency and maintenance costs, and enhances the mechanical properties and toughness of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention provides a method for preparing a ceramic fiber skeleton rigid thermal insulation material, which belongs to the field of thermal insulation materials. The method for preparing the ceramic fiber skeleton rigid thermal insulation material consists of the following steps: preparing modified alumina fiber, preparing a premixed slurry, forming a matrix, preparing a coating agent, and spraying forming. The method for preparing the ceramic fiber skeleton rigid thermal insulation material of the present invention can overcome the problem of uneven distribution of raw fiber and auxiliary materials in the preparation of the ceramic fiber skeleton rigid thermal insulation material, and at the same time improve the high-speed airflow erosion resistance of the ceramic fiber skeleton rigid thermal insulation material during actual application, improve damage tolerance, extend service life, reduce maintenance frequency and maintenance cost, and improve its overall stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermal insulation materials, and in particular to a method for preparing a ceramic fiber skeleton rigid thermal insulation material. Background Art

[0002] With the advancement of aerospace technology, the research on spacecraft has been heating up in recent years. From space shuttles to reusable carriers to hypersonic vehicles, when flying through the atmosphere, due to the friction between the surface of the vehicle and the surrounding air and the compression of the air in front, the spacecraft will be subjected to severe aerodynamic heating, high temperature and structural thermal stress, which has a significant impact on the safety of the spacecraft. Therefore, the thermal insulation material on the outer surface of the spacecraft plays an extremely important role in its safety and flight stability.

[0003] Ceramic fiber skeleton rigid insulation materials (i.e. insulation tiles) are generally micron-level porous structures with the advantages of light weight, excellent thermal insulation, mechanical properties, dielectric properties, and high operating temperature. Not only can they effectively reduce the weight of the spacecraft itself, but they also require very little material (such as fibers) to form a stable three-dimensional skeleton lap structure. In addition, ceramic fiber skeleton rigid insulation materials can also control the energy transferred from its surface to the interior, thereby effectively ensuring the stability of the spacecraft's external structure and the safety of its internal equipment when the spacecraft is flying for a long time.

[0004] The existing method for preparing ceramic fiber skeleton rigid thermal insulation materials mainly uses quartz fiber and alumina fiber as main raw materials, and after short cutting and pulping, they are processed through processes such as molding, drying, and sintering to obtain ceramic fiber skeleton rigid thermal insulation materials.

[0005] However, in the preparation of ceramic fiber skeleton rigid insulation materials, there is the problem of uneven distribution of raw material fibers and auxiliary materials; and the ceramic fiber skeleton rigid insulation materials are inherently brittle. In actual application, they are not resistant to high-speed airflow erosion, have low damage tolerance, high maintenance frequency and maintenance cost, and short service life, resulting in poor overall stability.

[0006] In this way, the problem of uneven distribution of raw materials and auxiliary materials in the preparation of ceramic fiber skeleton rigid thermal insulation materials is overcome, and at the same time, the high-speed airflow erosion resistance of ceramic fiber skeleton rigid thermal insulation materials in actual application is improved, the damage tolerance is improved, the service life is extended, the maintenance frequency and maintenance cost are reduced, and the overall stability is improved, which has important technical significance. Summary of the invention

[0007] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing a ceramic fiber skeleton rigid thermal insulation material, which can overcome the problem of uneven distribution of raw material fibers and auxiliary materials in the preparation of the ceramic fiber skeleton rigid thermal insulation material, and at the same time improve the high-speed airflow erosion resistance of the ceramic fiber skeleton rigid thermal insulation material in actual application, improve damage tolerance, extend service life, reduce maintenance frequency and maintenance cost, and improve its overall stability.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a ceramic fiber skeleton rigid thermal insulation material comprises the following steps: preparing modified alumina fiber, preparing premixed slurry, forming a matrix, preparing a coating agent, and spraying forming.

[0010] The method for preparing modified alumina fiber comprises the following steps: adding cerium nitrate and yttrium nitrate into an ethylene glycol aqueous solution with a volume concentration of 80-85%, stirring for 20-30 minutes, and obtaining a modified solution; adding alumina fiber into the modified solution with a weight of 100-110 times, controlling the immersion vacuum degree to be 0.04-0.06MPa, and after vacuum immersion for 50-60 minutes, stirring and adding disodium hydrogen phosphate, stirring at room temperature for 10-20 minutes, stirring and dripping a sodium hydroxide solution with a concentration of 0.06-0.08mol / min to adjust the pH to neutral, and continuing to stir for 20-30 minutes; then heating to 60-65°C at a heating rate of 0.7-0.8°C / min, keeping warm and stirring for 2-3 hours, separating and obtaining a solid, washing the solid with deionized water, and drying to obtain the modified alumina fiber.

[0011] In the preparation of the modified alumina fiber, the mass concentration of cerium nitrate in the modified solution is 3.7-4.0wt%, and the mass concentration of yttrium nitrate is 1.2-1.5wt%;

[0012] The diameter of alumina fibers is 7-13 μm, and the alumina content is 83-88 wt%;

[0013] The molar amount of disodium hydrogen phosphate is 1.1-1.2 times the sum of the molar amounts of cerium nitrate and yttrium nitrate in the modified solution.

[0014] The method for preparing the premixed slurry comprises: uniformly mixing methyl block room temperature vulcanized silicone rubber, tetraethyl orthosilicate and dimethyl silicone oil, stirring and heating to 40-45° C., and keeping the temperature and stirring for 60-90 minutes to obtain a premixed liquid; then chopping the modified alumina fiber and the fused quartz glass fiber to a length of 1-1.2 cm, adding the fibers to the premixed liquid, keeping the temperature and stirring at 40-45° C. for 3-4 hours, stirring and adding dibutyltin dilaurate and accelerator MZ, continuing to stir for 30-50 minutes, and then continuing to add boron nitride and stirring uniformly to obtain a premixed slurry.

[0015] In the preparation of the premixed slurry, the weight ratio of methyl block room temperature vulcanized silicone rubber, ethyl orthosilicate, and dimethyl silicone oil in the premixed liquid is 100:8-9:45-50;

[0016] The diameter of fused silica glass fiber is 7-10 μm and the silica content is 97-99 wt%;

[0017] Methyl block room temperature vulcanized silicone rubber is a copolymer of hydroxyl-capped polydimethylsiloxane (107 rubber) and methyltriethoxysilane oligomer (molecular weight 3-5);

[0018] The weight ratio of modified alumina fiber, fused silica glass fiber, premixed liquid, dibutyltin dilaurate, promoter MZ and boron nitride is 16-17:34-36:100:0.18-0.22:2.4-2.6:3-3.5.

[0019] The matrix forming method comprises the following steps: introducing the premixed slurry into a mold, standing for 3-5 minutes, filtering for 15-25 minutes to remove excess colloid, and obtaining a wet green body; then placing the mold containing the wet green body in a constant temperature drying oven, drying at 120-130° C. for 22-24 hours, demolding, and obtaining a preform; then placing the preform in a calcining furnace, controlling the heating rate to be 1.2-1.6° C. / min, heating to 1300-1400° C., and calcining at the temperature for 2-3 hours to obtain the matrix.

[0020] The method for preparing the coating agent comprises the following steps: adding borosilicate glass powder, β-eucryptite, quartz powder and isopropanol aqueous solution (volume concentration of 55-60%) into a ball mill, controlling the ball-to-material ratio to be 5-6:1, and the ball milling speed to be 90-120 rpm; after ball milling for 15-25 minutes, simultaneously spraying in a silane coupling agent A-1120 and a titanate coupling agent KR-38S, controlling the adding time of the silane coupling agent A-1120 and the titanate coupling agent KR-38S to be 15-20 minutes, continuing ball milling for 3-4 hours after the addition is completed, separating out solid matter, placing the solid matter in a constant temperature drying oven, and drying at 90-95° C. to a constant weight to obtain a ball milled matter; and then uniformly mixing the ball milled matter, silicon tetraboride, titanium dioxide, a dispersant AFCONA-4595 and deionized water to obtain the coating agent.

[0021] In the coating agent, the weight ratio of borosilicate glass powder, β-eucryptite, quartz powder, isopropanol aqueous solution, silane coupling agent A-1120, and titanate coupling agent KR-38S is 63-66:16-16.5:5-6:42-45:3.5-4:2.1-2.3;

[0022] The weight ratio of the ball milled material, silicon tetraboride, titanium dioxide, dispersant AFCONA-4595, and deionized water is 95-100:8-8.5:3.2-3.5:2-2.2:85-90.

[0023] The spraying molding method comprises the following steps: controlling the spraying gas source pressure to be 0.25-0.3MPa, the distance from the spray nozzle to the outer surface of the substrate to be 13-15cm, spraying the coating agent onto the outer surface of the substrate, transferring the substrate into a constant temperature drying oven, drying the substrate at 105-110°C for 4-5h, transferring the substrate into a sintering furnace, heating the substrate to 1150-1250°C at a heating rate of 3-3.5°C / min, sintering the substrate at the temperature for 2-3h, and cooling the substrate naturally to obtain a ceramic fiber skeleton rigid thermal insulation material.

[0024] In the spraying process, the spraying amount of the coating agent is adjusted according to the thickness of the coating formed by the final sintering of the coating agent, and the thickness of the coating formed by the sintering of the coating agent is controlled to be 90-100 μm.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The method for preparing a ceramic fiber skeleton rigid thermal insulation material of the present invention adopts cerium nitrate and yttrium nitrate to form a uniform cerium phosphate / yttrium phosphate coating on the outer surface of alumina fiber of specific specifications through wet chemical self-assembly to obtain modified alumina fiber; through the heat shielding effect of the cerium phosphate / yttrium phosphate coating on the alumina fiber, heat conduction is reduced and the overall thermal insulation performance of the thermal insulation material is improved; at the same time, the stability of the modified alumina fiber in a high temperature environment is improved, and the bonding performance of the modified alumina fiber with raw materials such as fused quartz glass fiber is improved, thereby further improving the structural stability of the thermal insulation material , improve the insulation material's resistance to high-speed airflow scouring and improve the insulation material's damage tolerance; then in the step of preparing the premixed slurry, the modified alumina fiber and the fused quartz glass fiber are chopped short, and then methyl block room temperature vulcanized silicone rubber, tetraethyl orthosilicate, and dimethyl silicone oil are used to coat the modified alumina fiber and the fused quartz glass fiber to further improve the insulation effect, and in the drying and calcining process of the matrix forming, silicon dioxide is generated by in-situ reaction, the bonding sites between the raw materials are increased, the bonding between the raw materials is reinforced, and the mechanical properties, toughness and structural stability of the insulation material are further improved. The intrinsic brittleness of the rigid thermal insulation material is overcome, and the damage tolerance of the thermal insulation material is further improved; then in the steps of preparing the coating agent and spraying the molding, the borosilicate glass powder, β-eucryptite, and quartz powder are first treated with the silane coupling agent A-1120 and the titanate coupling agent KR-38S to prepare the coating agent, which is then sprayed onto the outer surface of the substrate to obtain a ceramic fiber skeleton rigid thermal insulation material; the main raw materials are treated with the silane coupling agent A-1120 and the titanate coupling agent KR-38S to improve the bonding performance between the raw materials of the coating, and improve the compatibility and adhesion between the coating and the thermal insulation material substrate. A composite coating shell is constructed on the surface of the rigid thermal insulation material substrate, and the gaps on the surface of the rigid thermal insulation material substrate are filled with the composite coating to further improve the interface bonding strength between the coating and the substrate, and improve the overall stability of the thermal insulation material; the aforementioned technical means are combined with each other and work synergistically to overcome the problem of uneven distribution of raw fiber and auxiliary materials in the preparation of ceramic fiber skeleton rigid thermal insulation materials, and at the same time improve the high-speed airflow erosion resistance of ceramic fiber skeleton rigid thermal insulation materials in actual application, improve damage tolerance, extend service life, reduce maintenance frequency and maintenance cost, and improve its overall stability.

[0027] (2) The method for preparing a ceramic fiber skeleton rigid thermal insulation material of the present invention has a compressive strength of 3.3-3.4 MPa, a compressive strength of 2.9-3.2 MPa at 1200°C, a tensile strength in the thickness direction of 1.11-1.14 MPa, a tensile strength in the thickness direction of 1200°C of 1.02-1.09 MPa, and a fracture toughness of 0.86-0.91 MPa·m 1 / 2The thermal conductivity is 0.021-0.024W / m·k, and the interface bonding strength between the coating and the substrate is 3.0-3.2MPa.

[0028] (3) The method for preparing the ceramic fiber skeleton rigid thermal insulation material of the present invention has no deformation, shrinkage, cracking, or separation of the coating and the substrate after being kept at 1350°C for 10 hours; and after being kept at 1350°C for 720 hours, the weight loss rate of the ceramic fiber skeleton rigid thermal insulation material is 1.25-1.31wt%.

[0029] (4) The method for preparing the ceramic fiber skeleton rigid thermal insulation material of the present invention can effectively maintain the aerodynamic shape of the hypersonic aircraft while bearing the loads of aerodynamic heat, aerodynamic force and vibration coupling, thereby realizing the high reliability application of the thermal insulation material (i.e., thermal insulation tile). DETAILED DESCRIPTION

[0030] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0031] Example 1

[0032] A method for preparing a ceramic fiber skeleton rigid thermal insulation material, specifically comprising:

[0033] 1. Preparation of modified alumina fiber

[0034] Cerium nitrate and yttrium nitrate are added to an ethylene glycol aqueous solution with a volume concentration of 80%, and stirred for 20 minutes to obtain a modified solution; alumina fiber is added into 100 times the weight of the modified solution, and the immersion vacuum degree is controlled to be 0.04MPa. After vacuum immersion for 50 minutes, disodium hydrogen phosphate is added with stirring, and after stirring at room temperature for 10 minutes, a sodium hydroxide solution with a concentration of 0.06mol / min is added dropwise with stirring to adjust the pH to neutral, and stirring is continued for 20 minutes; then the temperature is increased to 60°C at a heating rate of 0.7°C / min, and after stirring for 2 hours, a solid is separated and washed with deionized water and dried to obtain modified alumina fiber.

[0035] The mass concentration of cerium nitrate in the modified solution is 3.7wt%, and the mass concentration of yttrium nitrate is 1.2wt%.

[0036] The diameter of the alumina fiber is 9 μm and the alumina content is 86 wt%.

[0037] The molar amount of disodium hydrogen phosphate is 1.1 times the sum of the molar amounts of cerium nitrate and yttrium nitrate in the modified solution.

[0038] 2. Preparation of premixed slurry

[0039] Methyl block room temperature vulcanized silicone rubber, tetraethyl orthosilicate and dimethyl silicone oil were mixed evenly, heated to 40°C with stirring, and kept stirring for 60 minutes to obtain a premixed liquid; then the modified alumina fiber and the fused quartz glass fiber were chopped to a length of 1 cm and added to the premixed liquid. After stirring at 40°C for 3 hours, dibutyltin dilaurate and accelerator MZ were added with stirring, and stirring was continued for 30 minutes, and then boron nitride was added and stirred evenly to obtain a premixed slurry.

[0040] Wherein, the weight ratio of methyl block room temperature vulcanized silicone rubber, ethyl orthosilicate and dimethyl silicone oil in the premix is ​​100:8:45.

[0041] The diameter of the fused silica glass fiber is 8 μm and the silica content is 99 wt%.

[0042] Methyl block room temperature vulcanized silicone rubber is a copolymer of hydroxyl-capped polydimethylsiloxane (107 rubber) and methyltriethoxysilane oligomer (molecular weight 3-5).

[0043] The weight ratio of modified alumina fiber, fused silica glass fiber, premix, dibutyltin dilaurate, promoter MZ, and boron nitride is 16:34:100:0.18:2.4:3.

[0044] 3. Matrix molding

[0045] The premixed slurry was introduced into the mold, allowed to stand for 3 minutes, and then filtered for 15 minutes to remove excess colloid to obtain a wet green body; the mold containing the wet green body was then placed in a constant temperature drying oven, dried at 120°C for 22 hours, and demolded to obtain a preform; the preform was then placed in a calcining furnace, the heating rate was controlled to be 1.2°C / min, the temperature was raised to 1300°C, and the temperature was kept and calcined for 2 hours to obtain a matrix.

[0046] 4. Preparation of coating agent

[0047] Borosilicate glass powder, β-eucryptite, quartz powder, isopropanol aqueous solution (volume concentration of 55%) were put into a ball mill, the ball-to-material ratio was controlled to be 5:1, the ball milling speed was 90 rpm, and after ball milling for 15 minutes, silane coupling agent A-1120 and titanate coupling agent KR-38S were sprayed in at the same time, and the addition time of silane coupling agent A-1120 and titanate coupling agent KR-38S was controlled to be 15 minutes. After the addition was completed, the ball milling was continued for 3 hours, and the solid matter was separated. The solid matter was placed in a constant temperature drying oven and dried at 90°C to constant weight to obtain a ball-milled product; then the ball-milled product, silicon tetraboride, titanium dioxide, dispersant AFCONA-4595, and deionized water were evenly mixed to prepare a coating agent.

[0048] Among them, the weight ratio of borosilicate glass powder, β-eucryptite, quartz powder, isopropyl alcohol aqueous solution, silane coupling agent A-1120, and titanate coupling agent KR-38S is 63:16:5:42:3.5:2.1.

[0049] The weight ratio of the ball-milled material, silicon tetraboride, titanium dioxide, dispersant AFCONA-4595, and deionized water is 95:8:3.2:2:85.

[0050] 5. Spraying molding

[0051] The spraying gas source pressure was controlled to be 0.25MPa, and the distance from the spray nozzle to the outer surface of the substrate was 13cm. After the coating agent was sprayed onto the outer surface of the substrate, it was transferred to a constant temperature drying oven, dried at 105°C for 4h, and then transferred to a sintering furnace, heated to 1150°C at a heating rate of 3°C / min, sintered for 2h, and naturally cooled to obtain a ceramic fiber skeleton rigid insulation material.

[0052] The spraying amount of the coating agent is adjusted according to the thickness of the coating formed by the final sintering of the coating agent, and the thickness of the coating formed by the sintering of the coating agent is controlled to be 90 μm.

[0053] Example 2

[0054] A method for preparing a ceramic fiber skeleton rigid thermal insulation material, specifically comprising:

[0055] 1. Preparation of modified alumina fiber

[0056] Cerium nitrate and yttrium nitrate are added to an ethylene glycol aqueous solution with a volume concentration of 82%, and stirred for 25 minutes to obtain a modified solution; alumina fiber is added into 105 times the weight of the modified solution, and the immersion vacuum degree is controlled to be 0.05MPa. After vacuum immersion for 55 minutes, disodium hydrogen phosphate is added with stirring, and after stirring at room temperature for 15 minutes, a sodium hydroxide solution with a concentration of 0.07mol / min is added dropwise with stirring to adjust the pH to neutral, and stirring is continued for 25 minutes; then the temperature is increased to 62°C at a heating rate of 0.75°C / min, and after stirring for 2.5 hours, a solid is separated and washed with deionized water and dried to obtain modified alumina fiber.

[0057] The mass concentration of cerium nitrate in the modified solution is 3.9wt%, and the mass concentration of yttrium nitrate is 1.3wt%.

[0058] The diameter of the alumina fiber is 9 μm and the alumina content is 86 wt%.

[0059] The molar amount of disodium hydrogen phosphate is 1.12 times the sum of the molar amounts of cerium nitrate and yttrium nitrate in the modified solution.

[0060] 2. Preparation of premixed slurry

[0061] Methyl block room temperature vulcanized silicone rubber, tetraethyl orthosilicate and dimethyl silicone oil were mixed evenly, heated to 42°C with stirring, and kept stirring for 80 minutes to obtain a premixed liquid; then the modified alumina fiber and the fused quartz glass fiber were chopped to a length of 1.1 cm and added to the premixed liquid. After stirring at 42°C for 3.5 hours, dibutyltin dilaurate and accelerator MZ were added with stirring, and stirring was continued for 40 minutes. Then, boron nitride was added and stirred evenly to obtain a premixed slurry.

[0062] Among them, the weight ratio of methyl block room temperature vulcanized silicone rubber, tetraethyl orthosilicate and dimethyl silicone oil in the premix is ​​100:8.5:47.

[0063] The diameter of the fused silica glass fiber is 8 μm and the silica content is 99 wt%.

[0064] Methyl block room temperature vulcanized silicone rubber is a copolymer of hydroxyl-capped polydimethylsiloxane (107 rubber) and methyltriethoxysilane oligomer (molecular weight 3-5).

[0065] The weight ratio of modified alumina fiber, fused silica glass fiber, premix, dibutyltin dilaurate, promoter MZ, and boron nitride is 16.5:35:100:0.2:2.5:3.2.

[0066] 3. Matrix molding

[0067] The premixed slurry was introduced into the mold, allowed to stand for 4 minutes, and then filtered for 20 minutes to remove excess colloid to obtain a wet green body; the mold containing the wet green body was then placed in a constant temperature drying oven, dried at 125°C for 23 hours, and demolded to obtain a preform; the preform was then placed in a calcining furnace, the heating rate was controlled to be 1.4°C / min, the temperature was raised to 1350°C, and the temperature was kept and calcined for 2.5 hours to obtain a matrix.

[0068] 4. Preparation of coating agent

[0069] Borosilicate glass powder, β-eucryptite, quartz powder, isopropanol aqueous solution (volume concentration 58%) were put into a ball mill, the ball-to-material ratio was controlled to be 5.3:1, the ball milling speed was 110 rpm, and after ball milling for 20 minutes, silane coupling agent A-1120 and titanate coupling agent KR-38S were sprayed in at the same time, and the addition time of silane coupling agent A-1120 and titanate coupling agent KR-38S was controlled to be 18 minutes. After the addition was completed, the ball milling was continued for 3.5 hours, and the solid matter was separated. The solid matter was placed in a constant temperature drying oven and dried at 92°C to constant weight to obtain a ball-milled product; then the ball-milled product, silicon tetraboride, titanium dioxide, dispersant AFCONA-4595, and deionized water were evenly mixed to prepare a coating agent.

[0070] Among them, the weight ratio of borosilicate glass powder, β-eucryptite, quartz powder, isopropyl alcohol aqueous solution, silane coupling agent A-1120, and titanate coupling agent KR-38S is 65:16.3:5.5:44:3.8:2.2.

[0071] The weight ratio of the ball-milled material, silicon tetraboride, titanium dioxide, dispersant AFCONA-4595, and deionized water is 97:8.3:3.4:2.1:88.

[0072] 5. Spraying molding

[0073] The spraying gas source pressure was controlled to be 0.28MPa, and the distance from the spray nozzle to the outer surface of the substrate was 14cm. After the coating agent was sprayed onto the outer surface of the substrate, it was transferred into a constant temperature drying oven. After drying at 108°C for 4.5h, it was transferred into a sintering furnace and heated to 1200°C at a heating rate of 3.2°C / min. It was sintered at this temperature for 2.5h and cooled naturally to obtain a ceramic fiber skeleton rigid insulation material.

[0074] The spraying amount of the coating agent is adjusted according to the thickness of the coating formed by the final sintering of the coating agent, and the thickness of the coating formed by the sintering of the coating agent is controlled to be 95 μm.

[0075] Example 3

[0076] A method for preparing a ceramic fiber skeleton rigid thermal insulation material, specifically comprising:

[0077] 1. Preparation of modified alumina fiber

[0078] Cerium nitrate and yttrium nitrate are added to an ethylene glycol aqueous solution with a volume concentration of 85%, and stirred for 30 minutes to obtain a modified solution; alumina fiber is added into 110 times the weight of the modified solution, and the immersion vacuum degree is controlled to be 0.06MPa. After vacuum immersion for 60 minutes, disodium hydrogen phosphate is added with stirring, and after stirring at room temperature for 20 minutes, a sodium hydroxide solution with a concentration of 0.08mol / min is added dropwise with stirring to adjust the pH to neutral, and stirring is continued for 30 minutes; then the temperature is increased to 65°C at a heating rate of 0.8°C / min, and after stirring for 3 hours, a solid is separated and washed with deionized water and dried to obtain modified alumina fiber.

[0079] The mass concentration of cerium nitrate in the modified solution is 4.0wt%, and the mass concentration of yttrium nitrate is 1.5wt%.

[0080] The diameter of the alumina fiber is 9 μm and the alumina content is 86 wt%.

[0081] The molar amount of disodium hydrogen phosphate is 1.2 times the sum of the molar amounts of cerium nitrate and yttrium nitrate in the modified solution.

[0082] 2. Preparation of premixed slurry

[0083] Methyl block room temperature vulcanized silicone rubber, tetraethyl orthosilicate and dimethyl silicone oil were mixed evenly, heated to 45°C with stirring, and kept stirring for 90 minutes to obtain a premixed liquid; then the modified alumina fiber and the fused quartz glass fiber were chopped to a length of 1.2 cm and added to the premixed liquid. After stirring at 45°C for 4 hours, dibutyltin dilaurate and accelerator MZ were added with stirring, and stirring was continued for 50 minutes. Then, boron nitride was added and stirred evenly to obtain a premixed slurry.

[0084] Wherein, the weight ratio of methyl block room temperature vulcanized silicone rubber, ethyl orthosilicate and dimethyl silicone oil in the premix is ​​100:9:50.

[0085] The diameter of the fused silica glass fiber is 8 μm and the silica content is 99 wt%.

[0086] Methyl block room temperature vulcanized silicone rubber is a copolymer of hydroxyl-capped polydimethylsiloxane (107 rubber) and methyltriethoxysilane oligomer (molecular weight 3-5).

[0087] The weight ratio of modified alumina fiber, fused silica glass fiber, premix, dibutyltin dilaurate, promoter MZ, and boron nitride is 17:36:100:0.22:2.6:3.5.

[0088] 3. Matrix molding

[0089] The premixed slurry was introduced into the mold, allowed to stand for 5 minutes, and then filtered for 25 minutes to remove excess colloid to obtain a wet green body; the mold containing the wet green body was then placed in a constant temperature drying oven, dried at 130°C for 24 hours, and demolded to obtain a preform; the preform was then placed in a calcining furnace, the heating rate was controlled to be 1.6°C / min, the temperature was raised to 1400°C, and the temperature was kept and calcined for 3 hours to obtain a matrix.

[0090] 4. Preparation of coating agent

[0091] Borosilicate glass powder, β-eucryptite, quartz powder, isopropanol aqueous solution (volume concentration 60%) were put into a ball mill, the ball-to-material ratio was controlled to be 6:1, the ball milling speed was 120rpm, and after ball milling for 25 minutes, silane coupling agent A-1120 and titanate coupling agent KR-38S were sprayed in at the same time, and the addition time of silane coupling agent A-1120 and titanate coupling agent KR-38S was controlled to be 20 minutes. After the addition was completed, the ball milling was continued for 4 hours, and the solid matter was separated and placed in a constant temperature drying oven, and dried at 95°C to constant weight to obtain a ball-milled product; then the ball-milled product, silicon tetraboride, titanium dioxide, dispersant AFCONA-4595, and deionized water were evenly mixed to prepare a coating agent.

[0092] Among them, the weight ratio of borosilicate glass powder, β-eucryptite, quartz powder, isopropyl alcohol aqueous solution, silane coupling agent A-1120, and titanate coupling agent KR-38S is 66:16.5:6:45:4:2.3.

[0093] The weight ratio of the ball-milled material, silicon tetraboride, titanium dioxide, dispersant AFCONA-4595, and deionized water is 100:8.5:3.5:2.2:90.

[0094] 5. Spraying molding

[0095] The spraying gas source pressure was controlled to be 0.3MPa, and the distance from the spray nozzle to the outer surface of the substrate was 15cm. After the coating agent was sprayed onto the outer surface of the substrate, it was transferred to a constant temperature drying oven, dried at 110°C for 5h, and then transferred to a sintering furnace, heated to 1250°C at a heating rate of 3.5°C / min, sintered for 3h, and cooled naturally to obtain a ceramic fiber skeleton rigid insulation material.

[0096] The spraying amount of the coating agent is adjusted according to the thickness of the coating formed by the final sintering of the coating agent, and the thickness of the coating formed by the sintering of the coating agent is controlled to be 100 μm.

[0097] Comparative Example 1

[0098] The technical solution of Example 2 is adopted, but the differences are: 1) the step of preparing modified alumina fiber is omitted, and unmodified alumina fiber is used in subsequent steps; 2) in the step of preparing premix, the addition of tetraethyl orthosilicate, dimethyl silicone oil and boron nitride is omitted.

[0099] Comparative Example 2

[0100] The technical solution of Example 2 is adopted, except that in the step of preparing the coating agent, the addition of the silane coupling agent A-1120 and the titanate coupling agent KR-38S is omitted, and the remaining materials are ball-milled and mixed uniformly to obtain the coating agent.

[0101] The preparation methods of the ceramic fiber skeleton rigid thermal insulation materials of Examples 1-3 and Comparative Examples 1-2 were respectively used to test the compressive strength, 1200°C compressive strength, thickness direction tensile strength, 1200°C thickness direction tensile strength, fracture toughness, thermal conductivity, and interface bonding strength between the coating and the substrate of the prepared ceramic fiber skeleton rigid thermal insulation materials.

[0102] Among them, the 1200℃ compressive strength is the compressive strength of the ceramic fiber skeleton rigid insulation material at a temperature of 1200℃; the 1200℃ thickness direction tensile strength is the thickness direction tensile strength of the ceramic fiber skeleton rigid insulation material at a temperature of 1200℃; the fracture toughness is tested by the single-edge notched beam method (SENB method).

[0103] The specific results are shown in the following table:

[0104]

[0105] Furthermore, the ceramic fiber skeleton rigid thermal insulation materials of Examples 1-3 and Comparative Examples 1-2 were placed in a calcining furnace, and heated to 1350°C at a heating rate of 30°C / min in an air atmosphere. After keeping warm for 10 hours, observe whether each ceramic fiber skeleton rigid thermal insulation material has deformation, shrinkage, or cracking problems; and observe whether each ceramic fiber skeleton rigid thermal insulation material has separation problems between the coating and the substrate. Furthermore, after each ceramic fiber skeleton rigid thermal insulation material was kept warm at 1350°C in an air atmosphere for 720 hours, the weight loss rate of each ceramic fiber skeleton rigid thermal insulation material was detected. The specific results are shown in the following table:

[0106]

[0107] It can be seen that the preparation method of the ceramic fiber skeleton rigid thermal insulation material of the present invention adopts cerium nitrate and yttrium nitrate to form a uniform cerium phosphate / yttrium phosphate coating on the outer surface of alumina fiber of specific specifications through wet chemical self-assembly to obtain modified alumina fiber; through the heat shielding effect of the cerium phosphate / yttrium phosphate coating on the alumina fiber, heat conduction is reduced and the overall thermal insulation performance of the thermal insulation material is improved; at the same time, the stability of the modified alumina fiber in a high temperature environment is improved, the bonding performance of the modified alumina fiber with raw materials such as fused quartz glass fiber is improved, and the structural stability of the thermal insulation material is further improved. Qualitative, improve the insulation material's resistance to high-speed airflow scouring, and improve the insulation material's damage tolerance; then in the step of preparing the premixed slurry, the modified alumina fiber and the fused quartz glass fiber are chopped short, and then methyl block room temperature vulcanized silicone rubber, tetraethyl orthosilicate, and dimethyl silicone oil are used to coat the modified alumina fiber and the fused quartz glass fiber to further improve the insulation effect, and in the drying and calcining process of the matrix forming, silicon dioxide is generated by in-situ reaction, the bonding sites between the raw materials are increased, the bonding between the raw materials is reinforced, and the mechanical properties, toughness and structural stability of the insulation material are further improved. The intrinsic brittleness of the rigid thermal insulation material is overcome, and the damage tolerance of the thermal insulation material is further improved; then in the steps of preparing the coating agent and spraying the molding, the silane coupling agent A-1120 and the titanate coupling agent KR-38S are first used to treat the borosilicate glass powder, β-eucryptite, and quartz powder to make a coating agent, which is then sprayed onto the outer surface of the substrate to obtain a ceramic fiber skeleton rigid thermal insulation material; the main raw materials are treated with the silane coupling agent A-1120 and the titanate coupling agent KR-38S to improve the bonding performance between the raw materials of the coating, and improve the compatibility and adhesion between the coating and the thermal insulation material substrate, and the coating is coated with the coating agent. A composite coating shell is constructed on the surface of the rigid thermal insulation material substrate, and the gaps on the surface of the rigid thermal insulation material substrate are filled with the composite coating to further improve the interface bonding strength between the coating and the substrate, and improve the overall stability of the thermal insulation material; the aforementioned technical means are combined with each other and work synergistically to overcome the problem of uneven distribution of raw fiber and auxiliary materials in the preparation of ceramic fiber skeleton rigid thermal insulation materials, and at the same time improve the high-speed airflow erosion resistance of ceramic fiber skeleton rigid thermal insulation materials in actual application, improve damage tolerance, extend service life, reduce maintenance frequency and maintenance cost, and improve its overall stability.

[0108] Unless otherwise specified, all percentages used in the present invention are by mass.

[0109] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a ceramic fiber skeleton rigid thermal insulation material, characterized in that: The method comprises the following steps: preparing modified alumina fiber, preparing premixed slurry, forming a matrix, preparing a coating agent, and spraying and forming; The method for preparing modified alumina fiber comprises: adding cerium nitrate and yttrium nitrate into an ethylene glycol aqueous solution, dispersing them uniformly, and obtaining a modified solution; adding alumina fiber into the modified solution, vacuum impregnating, stirring and adding disodium hydrogen phosphate, stirring at room temperature, stirring and dripping sodium hydroxide solution to adjust the pH to neutral, and continuing stirring; heating to 60-65° C., keeping the temperature and stirring for 2-3 hours, separating and obtaining a solid, washing the solid with deionized water, and drying to obtain the modified alumina fiber; The method for preparing the premixed slurry comprises: mixing methyl block room temperature vulcanized silicone rubber, ethyl orthosilicate, and dimethyl silicone oil uniformly, stirring and heating to 40-45° C., and stirring while keeping warm to obtain a premixed liquid; then chopping the modified alumina fiber and the fused quartz glass fiber, adding them to the premixed liquid, stirring while keeping warm at 40-45° C. for 3-4 hours, stirring and adding dibutyltin dilaurate and accelerator MZ, stirring, and then continuing to add boron nitride, stirring uniformly to obtain a premixed slurry; The methyl block room temperature vulcanized silicone rubber is a copolymer of hydroxyl-capped polydimethylsiloxane and a methyltriethoxysilane oligomer with a molecular weight of 3-5; The matrix forming method comprises the following steps: introducing the premixed slurry into a mold, allowing the premixed slurry to stand, filtering out excess colloid, and obtaining a wet green body; drying and demolding the wet green body, and then calcining the wet green body to obtain the matrix; The method for preparing the coating agent comprises: putting borosilicate glass powder, β-eucryptite, quartz powder and isopropanol aqueous solution into a ball mill, ball milling them uniformly, then spraying silane coupling agent A-1120 and titanate coupling agent KR-38S into the ball mill at the same time, continuing ball milling for 3-4 hours, separating solid matter, drying the solid matter and obtaining a ball milled product; then mixing the ball milled product, silicon tetraboride, titanium dioxide, dispersant AFCONA-4595 and deionized water uniformly to obtain the coating agent; The spray molding method comprises the following steps: spraying the coating agent onto the outer surface of the substrate, drying the substrate, transferring the substrate into a sintering furnace, heating the substrate to 1150-1250° C., sintering the substrate at a constant temperature, and cooling the substrate to obtain a ceramic fiber skeleton rigid thermal insulation material.

2. The method for preparing a ceramic fiber skeleton rigid thermal insulation material according to claim 1, characterized in that: In the preparation of the modified alumina fiber, the volume concentration of the ethylene glycol aqueous solution is 80-85%; The weight ratio of alumina fiber to modifying liquid is 1:100-110; The mass concentration of cerium nitrate in the modified solution is 3.7-4.0wt%, and the mass concentration of yttrium nitrate is 1.2-1.5wt%; The diameter of alumina fibers is 7-13 μm, and the alumina content is 83-88 wt%; The molar amount of disodium hydrogen phosphate is 1.1-1.2 times the sum of the molar amounts of cerium nitrate and yttrium nitrate in the modified solution.

3. The method for preparing a ceramic fiber skeleton rigid thermal insulation material according to claim 1, characterized in that: In the preparation of the modified alumina fiber, the vacuum degree of vacuum impregnation is 0.04-0.06MPa, and the vacuum impregnation time is 50-60min; After adjusting to neutrality with sodium hydroxide solution, continue stirring for 20-30 minutes; The heating rate to 60-65°C is 0.7-0.8°C / min.

4. The method for preparing a ceramic fiber skeleton rigid thermal insulation material according to claim 1, characterized in that: In the preparation of the premixed slurry, the weight ratio of methyl block room temperature vulcanized silicone rubber, ethyl orthosilicate, and dimethyl silicone oil in the premixed liquid is 100:8-9:45-50; The diameter of fused silica glass fiber is 7-10 μm and the silica content is 97-99 wt%; The weight ratio of modified alumina fiber, fused silica glass fiber, premixed liquid, dibutyltin dilaurate, promoter MZ and boron nitride is 16-17:34-36:100:0.18-0.22:2.4-2.6:3-3.

5.

5. The method for preparing a ceramic fiber skeleton rigid thermal insulation material according to claim 1, characterized in that: During the matrix forming, the drying temperature of the wet body is 120-130°C and the drying time is 22-24h; The calcination heating rate is 1.2-1.6°C / min, and the calcination temperature is 1300-1400°C; The calcination time at 1300-1400℃ is 2-3h.

6. The method for preparing a ceramic fiber skeleton rigid thermal insulation material according to claim 1, characterized in that: In the preparation of the coating agent, the volume concentration of the isopropanol aqueous solution is 55-60%; The ball-to-material ratio of ball milling is 5-6:1, and the ball milling speed is 90-120rpm; The addition time of silane coupling agent A-1120 and titanate coupling agent KR-38S is controlled to be 15-20 minutes.

7. The method for preparing a ceramic fiber skeleton rigid thermal insulation material according to claim 1, characterized in that: In the coating agent, the weight ratio of borosilicate glass powder, β-eucryptite, quartz powder, isopropanol aqueous solution, silane coupling agent A-1120, and titanate coupling agent KR-38S is 63-66:16-16.5:5-6:42-45:3.5-4:2.1-2.3; The weight ratio of the ball milled material, silicon tetraboride, titanium dioxide, dispersant AFCONA-4595, and deionized water is 95-100:8-8.5:3.2-3.5:2-2.2:85-90.

8. The method for preparing a ceramic fiber skeleton rigid thermal insulation material according to claim 1, characterized in that: During the spraying process, the spraying gas source pressure is controlled to be 0.25-0.3 MPa, and the distance from the spraying nozzle to the outer surface of the substrate is 13-15 cm; The heating rate to 1150-1250°C is 3-3.5°C / min; The sintering time at 1150-1250℃ is 2-3h; The coating thickness formed by the coating agent on the outer surface of the substrate is 90-100 μm.