A graphene dispersion and its preparation method and application in water-based cutting fluid
Through the preparation method of modified graphene dispersion, the problem of easy stacking of graphene in water-based cutting fluid is solved, and its uniform dispersion and lubrication performance in water-based cutting fluid is improved, which significantly improves the lubrication effect and wear resistance. Friction reduction performance.
Patent Information
- Application Number
- CN202411306256.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-19
AI Technical Summary
The existing water-based cutting fluid has shortcomings in lubricating properties, and graphene is easy to stack and agglomerate, resulting in reduced effective area and performance.
Using the preparation method of graphene dispersion, the graphene surface is modified by silane coupling agent, and titanium dioxide is absorbed and grown in situ in the graphene void, combining sodium polyacrylate, sodium dodecylbenzenesulfonate and cetyl group. Trimethyl ammonium bromide performs electrostatic adsorption and hydrophilic hydrophobic effects to stabilize the dispersion of graphene, and form a boundary lubricating film that is not easily destroyed by sodium lignin sulfonate. Nano-scale metal powder and boron nitride are added to improve thermal conductivity and reduce Moisture effect.
The uniform dispersion and stability of graphene in the water-based cutting fluid is achieved, the lubricating performance is significantly improved, the lubricating effect and anti-wear friction reduction performance are enhanced, and the finish of the workpiece and the stability of the cutting fluid are improved.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of water-based cutting fluid additives, and in particular, to a graphene dispersion liquid, a preparation method thereof, and an application thereof in water-based cutting fluids. Background Art
[0002] Water-based cutting fluid is an industrial liquid used in the process of metal cutting, grinding and milling to cool and lubricate cutting tools and workpieces. Cutting fluid is made of a variety of super-functional additives through scientific compounding, and has good cooling performance, lubrication performance, rust prevention performance, oil removal and cleaning function, anti-corrosion function, and easy dilution. It overcomes the problems of traditional soap-based emulsions that are easy to stink in summer, difficult to dilute in winter, and have poor anti-rust effect. It has no adverse effects on lathe paint and is suitable for cutting and grinding of ferrous metals. It is currently the most advanced grinding product. All indicators of cutting fluid are better than saponified oil. It has good cooling, cleaning, rust prevention and other characteristics. It is non-toxic, odorless, non-corrosive to the human body, non-corrosive to equipment, and non-polluting to the environment.
[0003] The current water-based cutting fluid focuses more on improving cooling, cleaning and rust prevention, but the lubrication performance is general and needs to be strengthened. In order to improve the above problems, researchers use graphene to improve the lubrication performance of water-based cutting fluid based on graphene's high thermal conductivity, high corrosion resistance and good friction reduction performance (Huang Peng, Luo Wei, Xiong Xuefeng. Application of two-dimensional nanomaterial modified water-based cutting fluid in niobium alloy material cutting processing [J]. Tool Technology, 2022(006):056.). Three-dimensional graphene has high chemical stability due to its special structural characteristics, such as high specific surface area and special two-dimensional honeycomb crystal structure. However, these characteristics also lead to strong van der Waals forces and π-π bond forces between graphene sheets, which makes graphene prone to irreversible stacking and agglomeration. This agglomeration phenomenon seriously reduces the effective area and performance of graphene, thus limiting the improvement effect. Summary of the invention
[0004] The purpose of the present application is to provide a graphene dispersion and a preparation method thereof. The graphene dispersion prepared by the raw materials and process has the advantages of uniform and stable graphene dispersion.
[0005] Another object of the present application is to provide an application of a graphene dispersion in a water-based cutting fluid, by which the lubricity of the water-based cutting fluid can be improved.
[0006] In order to solve the above technical problems, the technical solution adopted in this application is:
[0007] On the one hand, the present application provides a graphene dispersion, which includes the following raw materials per 100 parts of graphene dispersion, in parts by weight: 0.05-0.2 parts of graphene, 0.1-0.5 parts of sodium polyacrylate, 0.1-0.8 parts of sodium dodecylbenzene sulfonate, 0.1-0.8 parts of hexadecyltrimethylammonium bromide, 0.2-1 parts of titanium dioxide, 0.5-1.2 parts of metal powder, 0.1-1 parts of boron nitride, 0.03-0.15 parts of silane coupling agent, 1.5-2.8 parts of sodium lignin sulfonate, and the balance is water.
[0008] On the other hand, the present application provides a method for preparing a graphene dispersion, comprising the following steps:
[0009] S1, adding graphene to a silane coupling agent diluent, stirring evenly, then adding titanium dioxide sol after freeze drying, stirring, aging, and calcining to obtain graphene / titanium dioxide composite particles;
[0010] S2, stirring and mixing graphene / titanium dioxide composite particles, sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride, sodium lignin sulfonate and water to obtain a graphene mixed solution;
[0011] S3, magnetizing and ultrasonically dispersing the graphene mixed liquid in sequence to obtain the graphene dispersion liquid.
[0012] On the other hand, the present application also provides the use of the above-mentioned graphene dispersion as a lubricating additive in a water-based cutting fluid.
[0013] Compared with the prior art, the embodiments of the present application have at least the following advantages or beneficial effects:
[0014] 1. For the raw material formula of the present application, the present application uses graphene, sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, titanium dioxide, metal powder, boron nitride, silane coupling agent, sodium lignin sulfonate and water as raw materials to prepare graphene dispersion, wherein the silane coupling agent modifies the graphene surface, attracts titanium dioxide to adsorb and grow in situ in the graphene gap, and reduces the stacking and agglomeration problems of graphene due to the strong van der Waals force between the sheets; on this basis, sodium polyacrylate, sodium dodecylbenzene sulfonate and hexadecyltrimethylammonium bromide anionic surfactant are combined to stably and uniformly disperse graphene in water through electrostatic adsorption and hydrophilic-hydrophobic effects. The present application also adds sodium lignin sulfonate, utilizes its physical adsorption ability to wrap on the workpiece surface, combines the lubrication function of graphene to form a boundary lubrication film that is not easy to destroy on the workpiece contact surface, and improves the lubrication effect of graphene in water-based cutting fluid. Furthermore, the present application also adds nano-scale solid metal powder and boron nitride, which utilize their high thermal conductivity and ball bearing-like effect to easily enter the narrow workpiece contact surface during flushing, improve the finish of the workpiece, and further enhance the polishing and anti-wear and friction-reducing effects of the grease.
[0015] 2. With respect to the preparation method of the present application, the present application first modifies graphene by using a silane coupling agent and titanium dioxide sol, and then mixes the modified composite graphene / titanium dioxide composite particles with other raw materials and disperses them in water to obtain a graphene dispersion. Among them, freeze-drying the graphene can form a three-dimensional graphene porous aerogel, which increases the loading capacity of titanium dioxide and thus improves the dispersion modification effect. Finally, the preparation method of the present application uses a process of first magnetizing and then ultrasonicating. Under the action of magnetic force, various particles in the graphene mixture collide with each other, so that the hydrogen bonds between molecules are broken, and large molecular clusters become small molecular clusters, which are then evenly dispersed by ultrasound. During the cutting and flushing process, it is easier to penetrate into the contact gap between the metal and the tool, and then quickly form a boundary lubrication film on the metal surface. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0017] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0018] The embodiment of the present application provides a graphene dispersion liquid, which includes the following raw materials for every 100 parts of graphene dispersion liquid, in parts by weight: 0.05-0.2 parts of graphene, 0.1-0.5 parts of sodium polyacrylate, 0.1-0.8 parts of sodium dodecylbenzene sulfonate, 0.1-0.8 parts of hexadecyltrimethylammonium bromide, 0.2-1 parts of titanium dioxide, 0.5-1.2 parts of metal powder, 0.1-1 parts of boron nitride, 0.03-0.15 parts of silane coupling agent, 1.5-2.8 parts of sodium lignin sulfonate, and the balance is water.
[0019] In the present application, graphene is used as the main functional raw material. Its special structure makes it very easy to enter the contact surface between the friction pairs to form a physical adsorption film, thereby enhancing the lubrication effect and reducing friction.
[0020] Sodium polyacrylate is an anionic surfactant that can be used for electrostatic adsorption of surface activity. Graphene contains oxygen-containing functional groups (such as carboxyl and hydroxyl) that can be ionized into anions. Therefore, the surface of sodium polyacrylate can be used to modify graphene through the principle of electrostatic adsorption to make it more evenly dispersed in water.
[0021] Sodium dodecylbenzene sulfonate and hexadecyltrimethylammonium bromide are common surfactants in the field. One end of their molecular structure is hydrophilic and the other end is hydrophobic. The hydrophobic end can form strong hydrophobic adsorption with the hydrophobic surface of the graphene surface; accordingly, nanomaterials with hydrophilic ends can be better compatible with water and polymers. Through the connection and driving effect of sodium dodecylbenzene sulfonate and hexadecyltrimethylammonium bromide, graphene can be stably dispersed in water.
[0022] Titanium dioxide has good hydrophilicity and thermal stability and is commonly used in pigments, paints, coatings and cosmetics. In this application, a silane coupling agent modifies the surface of graphene, on which basis titanium dioxide is attracted to be adsorbed on the graphene surface and in the structural gaps, and grows in situ between graphene layers, increasing the distance and force between graphene molecules, thereby reducing the agglomeration and accumulation problem of graphene caused by van der Waals forces. This application uses titanium dioxide to modify graphene, which significantly reduces the stacking and agglomeration problems of graphene due to its own structure.
[0023] Sodium lignin sulfonate has the effect of reducing friction and wear. When the water-based cutting fluid contacts the workpiece, the polar molecules are adsorbed on the solid surface, making the physical adsorption capacity of the lignin sulfonate stronger, and a physical adsorption film can be formed on the workpiece surface, which is not easily destroyed. When sodium lignin sulfonate is combined with graphene, a boundary lubrication film can be formed on the workpiece surface, which not only plays a lubricating role, but also protects the workpiece surface from corrosion.
[0024] In some embodiments of the present application, every 100 parts of graphene dispersion includes the following raw materials: 0.1 parts of graphene, 0.3 parts of sodium polyacrylate, 0.5 parts of sodium dodecylbenzene sulfonate, 0.4 parts of hexadecyltrimethylammonium bromide, 0.5 parts of titanium dioxide, 0.8 parts of metal powder, 0.5 parts of boron nitride, 0.1 parts of silane coupling agent, 2.0 parts of sodium lignin sulfonate, and the balance of water.
[0025] In some embodiments of the present application, the metal powder includes at least one of copper powder, gold powder and zinc powder. The metal powder in the present application adopts nanoparticles, which have the effect of improving thermal conductivity. At the same time, the ball bearing-like nanometal powder can improve the smoothness of the contact surface when it acts on the surface of the tool and the workpiece, further improving the polishing and anti-wear and friction reduction effect of the cutting fluid.
[0026] In some embodiments of the present application, the metal powder and boron nitride are nano metal powder and nano boron nitride, and the titanium dioxide is titanium dioxide sol.
[0027] Boron nitride is specifically hexagonal boron nitride, which has a low friction coefficient, good high temperature stability, excellent thermal shock resistance, high strength, and high thermal conductivity, and can improve the stability of cutting fluid use.
[0028] In summary, the present application uses graphene, sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, titanium dioxide, metal powder, boron nitride, silane coupling agent, sodium lignin sulfonate and water as raw materials to prepare graphene dispersion, wherein the silane coupling agent modifies the graphene surface, attracts titanium dioxide to adsorb and grow in situ in the graphene gap, and reduces the stacking and agglomeration problems of graphene due to the strong van der Waals force between the sheets; on this basis, sodium polyacrylate, sodium dodecylbenzene sulfonate and hexadecyltrimethylammonium bromide anionic surfactants are combined to stably and uniformly disperse graphene in water through electrostatic adsorption and hydrophilic-hydrophobic effects. The present application also adds sodium lignin sulfonate, utilizes its physical adsorption ability to wrap around the workpiece surface, combines the lubrication function of graphene to form a boundary lubrication film that is not easily destroyed on the workpiece contact surface, and improves the lubrication effect of graphene in water-based cutting fluid.
[0029] Furthermore, the present application also adds nano-scale solid metal powder and boron nitride, which utilize their high thermal conductivity and ball bearing-like effect to easily enter the narrow workpiece contact surface during flushing, improve the finish of the workpiece, and further enhance the polishing and anti-wear and friction-reducing effects of the grease.
[0030] A method for preparing a graphene dispersion comprises the following steps:
[0031] S1, adding graphene to a silane coupling agent dilution solution, stirring evenly, then adding titanium dioxide sol after freeze drying, stirring, aging, and calcining to obtain graphene / titanium dioxide composite particles;
[0032] S2, stirring and mixing graphene / titanium dioxide composite particles, sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride, sodium lignin sulfonate and water to obtain a graphene mixed solution;
[0033] S3, subjecting the graphene mixed liquid to magnetization and ultrasonic dispersion in sequence to obtain the graphene dispersion liquid.
[0034] The present application first modifies graphene using a silane coupling agent and titanium dioxide sol, and then mixes the modified composite graphene / titanium dioxide composite particles with other raw materials and disperses them in water to obtain a graphene dispersion. The freeze-drying of graphene can form a three-dimensional graphene porous aerogel, which increases the loading capacity of titanium dioxide and thus improves the dispersion modification effect. Finally, the preparation method of the present application uses a process of first magnetization and then ultrasound. Under the action of magnetic force, various particles in the graphene mixture collide with each other, causing the hydrogen bonds between molecules to break, and large molecular clusters to become small molecular clusters, which are then evenly dispersed by ultrasound. During the cutting and flushing process, it is easier to penetrate into the contact gap between the metal and the tool, and then quickly form a boundary lubrication film on the metal surface.
[0035] In some embodiments of the present application, the mass concentration of the silane coupling agent dilution solution in the above-mentioned S1 step is 0.5-1%, the freeze-drying parameters are -60-80°C, the no-load vacuum degree is 12-15Pa, and the freeze-drying time is 6-12h; the aging time is 24-48h, the roasting temperature is 200-250°C, the roasting is 20-35min, and the calcination step is carried out under an inert gas atmosphere.
[0036] In some embodiments of the present application, the stirring rate of the mixing in the above step S2 is 500-800 r / min, and the mixing time is 5-10 min.
[0037] In some embodiments of the present application, the magnetic field intensity of the magnetization in the above step S3 is 3000-5000 GS, the magnetization time is 20-30 min, and the magnetization temperature is 32-35° C. The present application adopts a higher magnetization temperature than normal temperature to reduce the viscosity between molecules and improve the activity of molecules.
[0038] The invention discloses an application of a graphene dispersion as a lubricating additive in a water-based cutting fluid.
[0039] In some embodiments of the present application, the proportion of the above-mentioned graphene dispersion additive in the water-based cutting fluid is 0.1-5wt%.
[0040] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0041] Example 1
[0042] This embodiment discloses a graphene dispersion, and the raw materials used are as follows:
[0043] 1g graphene, 3g sodium polyacrylate, 5g sodium dodecylbenzene sulfonate, 4g hexadecyltrimethylammonium bromide, 5g titanium dioxide, 8g metal powder, 5g boron nitride, 1g silane coupling agent, 20g sodium lignin sulfonate, and water.
[0044] The graphene is natural graphite powder with a particle size of 70 to 80 μm, the metal powder is nano zinc, and the titanium dioxide is specifically titanium dioxide sol.
[0045] The preparation method of graphene dispersion is as follows:
[0046] S1. Prepare a diluent with a concentration of 1w% of a silane coupling agent, add graphene to the diluent, stir at a high speed of 1000 r / min for 5 min, and then freeze-dry for 12 h at -60°C and 14 Pa, and grind to obtain graphene powder; add titanium dioxide sol to the graphene powder, stir at a speed of 800 r / min for 10 min, and then age at room temperature for 24 h; under an argon atmosphere, first dry at 60°C for 12 h, and then calcine at 250°C for 35 min to obtain graphene / titanium dioxide composite particles;
[0047] S2, adding the above-mentioned graphene / titanium dioxide composite particles with sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride and sodium lignin sulfonate, and adding water to 1000g, stirring and mixing, stirring at a speed of 800r / min, stirring for 10min, to obtain a graphene mixed solution;
[0048] S3, heating the graphene mixed solution to 35° C., and then sending it into a magnetizer, adjusting the magnetization intensity to 5000 GS, and the magnetization time to 25 min; and ultrasonically dispersing the magnetized product for 5 min to obtain the graphene dispersion of this embodiment.
[0049] Example 2
[0050] This embodiment discloses a graphene dispersion, and the raw materials used are as follows:
[0051] 1.5g graphene, 4g sodium polyacrylate, 3g sodium dodecylbenzene sulfonate, 5g hexadecyltrimethylammonium bromide, 4.8g titanium dioxide, 6g metal powder, 8g boron nitride, 0.6g silane coupling agent, 15g sodium lignin sulfonate, and water.
[0052] The graphene is natural graphite powder with a particle size of 70 to 80 μm, the metal powder is nano copper, and the titanium dioxide is specifically titanium dioxide sol.
[0053] The preparation method of graphene dispersion is as follows:
[0054] S1. Prepare a diluent with a concentration of 0.8w% of a silane coupling agent, add graphene to the diluent, stir at a high speed of 1000 r / min for 5 min, and then freeze-dry for 12 h at -80°C and 14 Pa, and grind to obtain graphene powder; add titanium dioxide sol to the graphene powder, stir at a speed of 800 r / min for 15 min, and then age at room temperature for 24 h; dry at 60°C for 12 h, and then calcine at 230°C for 35 min under an argon atmosphere to obtain graphene / titanium dioxide composite particles;
[0055] S2, adding the above-mentioned graphene / titanium dioxide composite particles with sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride and sodium lignin sulfonate, and adding water to 1000g, stirring and mixing, stirring at a speed of 800r / min, stirring for 10min, to obtain a graphene mixed solution;
[0056] S3, heating the graphene mixed solution to 32° C., and then sending it into a magnetizer, adjusting the magnetization intensity to 3000 GS, and the magnetization time to 30 min; and ultrasonically dispersing the magnetized product for 5 min to obtain the graphene dispersion of this embodiment.
[0057] Example 3
[0058] This embodiment discloses a graphene dispersion, and the raw materials used are as follows:
[0059] 1.5g graphene, 4g sodium polyacrylate, 3g sodium dodecylbenzene sulfonate, 5g hexadecyltrimethylammonium bromide, 10g titanium dioxide, 8g metal powder, 8g boron nitride, 1.2g silane coupling agent, 22g sodium lignin sulfonate, and water.
[0060] The graphene is natural graphite powder with a particle size of 70 to 80 μm, the metal powder is nano copper, and the titanium dioxide is specifically titanium dioxide sol.
[0061] The preparation method of graphene dispersion is as follows:
[0062] S1. Prepare a diluent with a concentration of 0.5w% of a silane coupling agent, add graphene to the diluent, stir at a high speed of 1000 r / min for 5 min, and then freeze-dry at -80°C and 15 Pa for 8 h, and grind to obtain graphene powder; add titanium dioxide sol to the graphene powder, stir at a speed of 800 r / min for 15 min, and then age at room temperature for 24 h; under an argon atmosphere, first dry at 60°C for 15 h, and then calcine at 200°C for 35 min to obtain graphene / titanium dioxide composite particles;
[0063] S2, stirring and mixing the above-mentioned graphene / titanium dioxide composite particles with sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride, sodium lignin sulfonate and water at a stirring rate of 600 r / min for 10 min to obtain a graphene mixed solution;
[0064] S3, heating the graphene mixed solution to 35° C., and then sending it into a magnetizer, adjusting the magnetization intensity to 3000 GS, and the magnetization time to 30 min; and ultrasonically dispersing the magnetized product for 5 min to obtain the graphene dispersion of this embodiment.
[0065] Example 4
[0066] This embodiment discloses a graphene dispersion, and the raw materials used are as follows:
[0067] 1.5 g of graphene, 3.2 g of sodium polyacrylate, 6.5 g of sodium dodecylbenzene sulfonate, 2.5 g of hexadecyltrimethylammonium bromide, 6.8 g of titanium dioxide, 10 g of metal powder, 7 g of boron nitride, 0.6 g of silane coupling agent, 18 g of sodium lignin sulfonate, and water.
[0068] The graphene is natural graphite powder with a particle size of 70 to 80 μm, the metal powder is nano copper, and the titanium dioxide is specifically titanium dioxide sol.
[0069] The preparation method of graphene dispersion is as follows:
[0070] S1. Prepare a diluent with a concentration of 0.5w% of a silane coupling agent, add graphene to the diluent, stir at a high speed of 1000 r / min for 5 min, and then freeze-dry at -80°C and 12 Pa for 8 h, and grind to obtain graphene powder; add titanium dioxide sol to the graphene powder, stir at a speed of 800 r / min for 10 min, and then age at room temperature for 36 h; under an argon atmosphere, first dry at 60°C for 15 h, and then calcine at 200°C for 35 min to obtain graphene / titanium dioxide composite particles;
[0071] S2, mixing the graphene / titanium dioxide composite particles with sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride, sodium lignin sulfonate and water at a stirring rate of 800 r / min for 10 min to obtain a graphene mixed solution;
[0072] S3, heating the graphene mixed solution to 35° C., and then sending it into a magnetizer, adjusting the magnetization intensity to 4000 GS, and the magnetization time to 20 min; and ultrasonically dispersing the magnetized product for 10 min to obtain the graphene dispersion of this embodiment.
[0073] Example 5
[0074] This embodiment discloses a graphene dispersion, and the raw materials used are as follows:
[0075] 1.8g graphene, 2.5g sodium polyacrylate, 5g sodium dodecylbenzene sulfonate, 5.5g hexadecyltrimethylammonium bromide, 2.5g titanium dioxide, 8g metal powder, 6g boron nitride, 1.2 silane coupling agent, 18g sodium lignin sulfonate, water.
[0076] The graphene is natural graphite powder with a particle size of 70 to 80 μm, the metal powder is nano copper, and the titanium dioxide is specifically titanium dioxide sol.
[0077] The preparation method of graphene dispersion is as follows:
[0078] S1. Prepare a diluent with a concentration of 0.5w% of a silane coupling agent, add graphene to the diluent, stir at a high speed of 1000 r / min for 5 min, and then freeze-dry at -80°C and 12 Pa for 6 h, and grind to obtain graphene powder; add titanium dioxide sol to the graphene powder, stir at a speed of 800 r / min for 10 min, and then age at room temperature for 48 h; under an argon atmosphere, first dry at 50°C for 12 h, and then calcine at 200°C for 30 min to obtain graphene / titanium dioxide composite particles;
[0079] S2, mixing the graphene / titanium dioxide composite particles with sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride, sodium lignin sulfonate and water at a stirring rate of 800 r / min for 10 min to obtain a graphene mixed solution;
[0080] S3, heating the graphene mixed solution to 34° C., and then sending it into a magnetizer, adjusting the magnetization intensity to 4000 GS, and the magnetization time to 20 min; and ultrasonically dispersing the magnetized product for 10 min to obtain the graphene dispersion of this embodiment.
[0081] Example 6
[0082] This embodiment discloses a graphene dispersion, and the raw materials used are as follows:
[0083] 1g graphene, 3.5g sodium polyacrylate, 5g sodium dodecylbenzene sulfonate, 3.5g hexadecyltrimethylammonium bromide, 8.5g titanium dioxide, 8g metal powder, 8g boron nitride, 1.2 silane coupling agent, 26g sodium lignin sulfonate, water.
[0084] The graphene is natural graphite powder with a particle size of 70 to 80 μm, the metal powder is nano-gold, and the titanium dioxide is specifically titanium dioxide sol.
[0085] The preparation method of graphene dispersion is as follows:
[0086] S1. Prepare a diluent with a concentration of 0.5w% of a silane coupling agent, add graphene to the diluent, stir at a high speed of 800 r / min for 8 min, and then freeze-dry at -80°C and 12 Pa for 8 h, and grind to obtain graphene powder; add titanium dioxide sol to the graphene powder, stir at a speed of 800 r / min for 10 min, and then age at room temperature for 48 h; under an argon atmosphere, first dry at 50°C for 6 h, and then calcine at 200°C for 30 min to obtain graphene / titanium dioxide composite particles;
[0087] S2, mixing the graphene / titanium dioxide composite particles with sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride, sodium lignin sulfonate and water at a stirring rate of 800 r / min for 10 min to obtain a graphene mixed solution;
[0088] S3, heating the graphene mixed solution to 32° C., and then sending it into a magnetizer, adjusting the magnetization intensity to 4000 GS, and the magnetization time to 28 min; and ultrasonically dispersing the magnetized product for 8 min to obtain the graphene dispersion of this embodiment.
[0089] Comparative Example 1
[0090] The graphene dispersion of this comparative example is substantially the same as that of Example 1, except that the raw materials of this comparative example do not contain titanium dioxide and silane coupling agent.
[0091] The preparation method is:
[0092] Graphene was mixed with sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride and sodium lignin sulfonate, and water was added to make up to 1000 g, and the mixture was stirred at a stirring rate of 800 r / min for 10 min to obtain a graphene mixed solution;
[0093] The graphene mixed liquid was heated to 35° C., and then sent into a magnetizer, and the magnetization intensity was adjusted to 5000 GS, and the magnetization time was 25 min. The magnetized product was then ultrasonically dispersed for 5 min to obtain the graphene dispersion of this comparative example.
[0094] Comparative Example 2
[0095] The graphene dispersion of this comparative example is substantially the same as that of Example 1, except that there is no silane coupling agent in the raw materials of this comparative example, and the titanium dioxide is a nanopowder.
[0096] The preparation method is:
[0097] Graphene was mixed with titanium dioxide, sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride and sodium lignin sulfonate, and water was added to make up to 1000 g, and the mixture was stirred at a stirring rate of 800 r / min for 10 min to obtain a graphene mixed solution;
[0098] The graphene mixed liquid was heated to 35° C., and then sent into a magnetizer, and the magnetization intensity was adjusted to 5000 GS, and the magnetization time was 25 min. The magnetized product was then ultrasonically dispersed for 5 min to obtain the graphene dispersion of this comparative example.
[0099] Comparative Example 3
[0100] The graphene dispersion of this comparative example is substantially the same as that of Example 1, except that the raw materials of this comparative example do not contain metal powder and boron nitride.
[0101] Comparative Example 4
[0102] The graphene dispersion of this comparative example is substantially the same as that of Example 1, except that there is no sodium lignin sulfonate in the raw materials of this comparative example.
[0103] Comparative Example 5
[0104] The graphene dispersion of this comparative example is basically the same as that of Example 1, except that the preparation process of this comparative example does not have step S1, and the raw materials are directly mixed and dispersed in water, specifically:
[0105] Graphene, titanium dioxide, silane coupling agent, sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride and sodium lignin sulfonate were mixed, and water was added to make up to 1000 g, and the mixture was stirred at a stirring rate of 800 r / min for 10 min to obtain a graphene mixed solution;
[0106] The graphene mixed liquid was heated to 35° C., and then sent into a magnetizer, and the magnetization intensity was adjusted to 5000 GS, and the magnetization time was 25 min. The magnetized product was then ultrasonically dispersed for 5 min to obtain the graphene dispersion of this embodiment.
[0107] Comparative Example 6
[0108] The graphene dispersion in this comparative example is substantially the same as that in Example 1, except that step S3 of this comparative example does not include a magnetization process, and the graphene mixed solution is directly ultrasonically dispersed.
[0109] Experimental example
[0110] 1. This experimental example explores the dispersion stabilization effect of graphene in graphene dispersion.
[0111] The graphene dispersions prepared in Examples 1 to 6 and Comparative Examples 1 to 6 were allowed to stand after preparation, and then the transmittance of the graphene dispersions in each experimental group was accelerated by LUMiSizer centrifugal acceleration (30,000 r / min). The transmittance results within 30 minutes are shown in Table 1.
[0112] Table 1
[0113] Experimental Group 0min 5min 10min 15min 20min 25min 30min Example 1 0% 3.2% 10.5% 20.7% 35.4% 50.8% 56.4% Example 2 0% 2.7% 9.7% 18.6% 37.8% 52.7% 58.5% Example 3 0% 3.1% 10.2% 20.9% 36.4% 50.1% 55.3% Example 4 0% 4.0% 11.3% 22.1% 36.5% 52.0% 56.9% Example 5 0% 2.6% 10.0% 19.8% 34.1% 50.6% 56.1% Example 6 0% 2.9% 10.6% 21.0% 36.8% 51.4% 57.2% Comparative Example 1 0% 5.9% 20.8% 37.9% 50.7% 66.2% 75.4% Comparative Example 2 0% 4.8% 18.5% 25.4% 46.7% 64.1% 70.2% Comparative Example 3 0% 3.1% 12.2% 21.4% 35.2% 52.7% 57.2% Comparative Example 4 0% 3.2% 11.1% 20.5% 34.9% 51.0% 56.8% Comparative Example 5 0% 4.1% 12.9% 23.1% 38.5% 54.1% 62.8% Comparative Example 6 0% 10.8% 18.9% 25.4% 40.2% 52.7% 60.2%
[0114] As can be seen from Table 1, the graphene dispersions prepared in Examples 1 to 6 have good dispersion effects and dispersion stability. Comparative Example 1 does not contain titanium dioxide and silane coupling agent, and only uses conventional surfactants to disperse graphene, but the effect is limited. During the accelerated centrifugation process, the binding force of the surfactant on the graphene decreases, which accelerates the agglomeration of the graphene. Comparative Example 2 contains titanium dioxide but does not contain a silane coupling agent. From the results, it can be seen that when there is no silane coupling agent to modify the graphene, the adhesion and growth of titanium dioxide on the graphene surface are weakened, and its improvement of the van der Waals force between graphene layers is limited. The sedimentation effects of Comparative Examples 3 and 4 are less different from those of Example 1, indicating that sodium lignin sulfonate, metal powder and boron nitride have little effect on the dispersibility of graphene; Comparative Example 5 There is no S1 step in the comparative example 6, and all the raw materials are directly mixed and dispersed. The effect is significantly different from that in Example 1, indicating that the prior combination of other raw materials with graphene will affect the modification of graphene by the silane coupling agent, and further affect the combination of titanium dioxide and graphene; there is no magnetization step in the comparative example 6, and the deposition and agglomeration effect of the graphene appears faster, indicating that the magnetization step also has a significant effect on the stability of the graphene dispersion.
[0115] 2. This experimental example explores the effect of the graphene dispersion prepared in Examples 1 to 6 of the present application and Comparative Examples 1 to 6 on the lubrication performance of water-based cutting fluid.
[0116] The water-based cutting fluid formula (mass percentage) used in this embodiment is: 3.8% extreme pressure lubricant, 0.5% bactericide, 1.2% rust inhibitor, 0.8% corrosion inhibitor, 0.5% surfactant, 1% dispersant, 0.1% descaling agent, 0.1% defoamer, 3% graphene dispersion and 89% water. The above raw materials are ultrasonically dispersed for 10 minutes to obtain various experimental products.
[0117] This experiment set up a control group and a blank group at the same time. The control group used graphene powder instead of graphene dispersion; the blank group did not add graphene dispersion, and the proportion of water was increased accordingly.
[0118] The tribological properties of the products in each experimental group were tested using a four-ball friction and wear testing machine, and the results are shown in Table 2.
[0119] Table 2
[0120] Experimental Group Maximum no-seizure load PB Example 1 813 N Example 2 810 N Example 3 812 N Example 4 815 N Example 5 812 N Example 6 814 N Comparative Example 1 518 N Comparative Example 2 543 N Comparative Example 3 742 N Comparative Example 4 718 N Comparative Example 5 767 N Comparative Example 6 703 N Control group 471 N Blank group 457N
[0121] It can be seen from Table 2 that, compared with the blank group, adding graphene dispersion or graphene to the water-based cutting fluid can improve lubricity. Among them, the graphene dispersion prepared in Examples 1 to 6 has a significant and stable lubricity enhancement effect when added to the water-based cutting fluid. Comparative Example 1 lacks titanium dioxide modification of graphene. Although other surfactants promote dispersion, its lubrication ability is significantly reduced compared with Example 1, indicating that the agglomeration effect of graphene will affect the lubrication performance of water-based cutting fluid; Comparative Example 2 has the same problem, and it shows that titanium dioxide cannot completely modify graphene without the participation of silane coupling agent; Comparative Example 3 and Comparative Example 4 are compared with Example 1, which shows that sodium lignin sulfonate, metal powder and boron nitride also play a greater lubrication effect in water-based cutting fluid; Comparative Example 5 shows that the order of process steps will affect the preferred order of combination between raw materials, and the combination of graphene and surfactant will affect the modification of graphene by titanium dioxide; Comparative Example 6 shows that the magnetization step will not only affect the agglomeration of graphene, but may also affect the efficiency of the remaining raw materials entering the friction contact area of the workpiece, thereby affecting the lubricity of the water-based cutting fluid.
[0122] 3. The optimal addition ratio of graphene dispersion in water-based cutting fluid in this experimental example.
[0123] The water-based cutting fluid used in this experimental example is the same as that in Experimental Example 2, and the graphene dispersion prepared in Example 1 is used, and the addition ratio (mass percentage) is 0%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, and 7%. The friction coefficient is measured using a friction and wear tester, and the results are shown in Table 3.
[0124] Table 3
[0125] Add Scale 0% 0.1% 0.5% 1% 2% 3% 4% 5% 6% 7% Friction coefficient 0.157 0.151 0.146 0.132 0.101 0.075 0.064 0.065 0.063 0.059
[0126] It can be seen from Table 3 that when the addition amount of graphene dispersion in water-based cutting fluid is greater than 0.1%, it can play a significant friction reduction effect; before the addition amount of graphene dispersion is 5wt%, with the increase of graphene dispersion content, the friction coefficient of water-based cutting fluid gradually decreases. When the addition amount of graphene dispersion exceeds 5wt%, the friction coefficient increases slightly, indicating that the addition mass of graphene dispersion in water-based cutting fluid reaches saturation when 5wt%. Excessively high concentration of graphene dispersion will inevitably produce partial particle collisions during movement, causing agglomeration between particles, and the increase in particle size caused by agglomeration will affect its entry into the gap of the friction contact surface, thereby reducing the lubrication and friction reduction effect of the entire water-based cutting fluid.
[0127] In summary, the present application discloses a graphene dispersion and a preparation method thereof and application in a water-based cutting fluid.
[0128] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0129] In the description of the specification of the present application, the terms "include", "comprise", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plural" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0130] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A graphene dispersion, characterized in that: In parts by weight, every 100 parts of graphene dispersion liquid includes the following raw materials: 0.05-0.2 parts of graphene, 0.1-0.5 parts of sodium polyacrylate, 0.1-0.8 parts of sodium dodecylbenzene sulfonate, 0.1-0.8 parts of hexadecyltrimethylammonium bromide, 0.2-1 parts of titanium dioxide, 0.5-1.2 parts of metal powder, 0.1-1 parts of boron nitride, 0.03-0.15 parts of silane coupling agent, 1.5-2.8 parts of sodium lignin sulfonate, and the balance is water; The metal powder includes at least one of copper powder, gold powder and zinc powder; the metal powder and boron nitride are nano metal powder and nano boron nitride, and the titanium dioxide is titanium dioxide sol; The preparation method of the graphene dispersion comprises the following steps: S1, adding graphene to a silane coupling agent dilution solution, stirring evenly, then adding titanium dioxide sol after freeze drying, stirring, aging, and calcining to obtain graphene / titanium dioxide composite particles; S2, stirring and mixing graphene / titanium dioxide composite particles, sodium polyacrylate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, metal powder, boron nitride, sodium lignin sulfonate and water to obtain a graphene mixed solution; S3, magnetizing and ultrasonically dispersing the graphene mixed liquid in sequence to obtain the graphene dispersion liquid.
2. A graphene dispersion according to claim 1, characterized in that: Every 100 parts of graphene dispersion includes the following raw materials: 0.1 parts of graphene, 0.3 parts of sodium polyacrylate, 0.5 parts of sodium dodecylbenzene sulfonate, 0.4 parts of hexadecyltrimethylammonium bromide, 0.5 parts of titanium dioxide, 0.8 parts of metal powder, 0.5 parts of boron nitride, 0.1 parts of silane coupling agent, 2.0 parts of sodium lignin sulfonate, and the balance is water.
3. A graphene dispersion according to claim 1, characterized in that: The mass concentration of the silane coupling agent dilution in step S1 is 0.5-1%, the freeze-drying parameters are -60-80°C, the no-load vacuum degree is 12-15Pa, and the freeze-drying time is 6-12h; the aging time is 24-48h, the roasting temperature is 200-250°C, and the roasting time is 20-35min.
4. A graphene dispersion according to claim 1, characterized in that: The stirring rate of the mixing in the step S2 is 500-800 r / min, and the mixing time is 5-10 min.
5. A graphene dispersion according to claim 1, characterized in that: In the step S3, the magnetic field intensity of the magnetization is 3000-5000 GS, the magnetization time is 20-30 min, and the magnetization temperature is 32-35° C.
6. Use of the graphene dispersion according to any one of claims 1 to 5 as a lubricating additive in a water-based cutting fluid, characterized in that: The proportion of the graphene dispersion additive in the water-based cutting fluid is 0.1-5wt%.