A method for inhibiting metal grain recrystallization, aluminum alloy and preparation method thereof
By applying the synergistic effect of pressure and temperature field in the annealing treatment of aluminum alloy, the problem of grain recrystallization of aluminum alloy during thermal processing is solved, and the preparation of high-thermal stability micro-crystalline aluminum alloy is realized, which significantly improves the material Mechanical properties.
Patent Information
- Application Number
- CN202411308204.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-19
AI Technical Summary
The prior art is difficult to effectively inhibit the recrystallization and growth of aluminum alloys during thermal processing or heat treatment, resulting in a decline in the mechanical properties of the materials.
By applying pressure to the aluminum alloy at the annealing temperature, the initial pressure is maintained at 100% but less than 130% of the yield strength, combined with a constant temperature field for annealing to ensure that the strain remains unchanged, the pressure is gradually reduced, and the extension is extended by 3~11 hours to promote Dislocation movement eliminates deformation and energy storage.
It effectively inhibits the recrystallization and growth of aluminum alloy grains, significantly reduces the grain size, improves the thermal stability and strain ability of the material, and significantly reduces the formation of coarse grains.
Smart Images

Figure CN118814097B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal processing, and in particular relates to a method for inhibiting metal grain recrystallization, an aluminum alloy and a preparation method thereof. Background Art
[0002] Metal grains refer to a number of crystals formed by metal atoms that are arranged continuously according to certain rules with the crystal nucleus as the core during the cooling and solidification process of liquid metal.
[0003] Aluminum alloy is the most common metal. It is lightweight, abundant in resources and has good comprehensive performance. It is widely used in important fields such as transportation, aerospace and military industry. The continuous innovation in the aerospace field has put forward higher requirements for the various properties of aluminum alloys. For aluminum alloys, poor processing performance or insufficient service performance of finished structural parts often occurs. This is mainly caused by coarse and uneven grains and strong texture. Fine grain structure can improve the strength and toughness of aluminum alloys, while weakening the texture structure, so that the alloy has high strength, high plasticity, and low anisotropy, so as to better meet the needs of aerospace structural parts.
[0004] Large plastic deformation is currently the most commonly used and convenient process for preparing fine-grained metal materials. Multi-directional forging is a type of large plastic deformation. The process is characterized by forming a subgrain structure with high dislocation density and defect density through severe plastic deformation in different directions, so that the metal grain size is refined to the micron level or even nanometer level. However, high-density dislocations and ultrafine grains correspond to extremely high recrystallization driving forces. This makes the recrystallization behavior of metal materials after multi-directional forging during hot working or heat treatment cause the deformed grains to grow preferentially, thereby weakening the gain of fine-grained structure on the mechanical properties of the material.
[0005] Pre-recovery treatment is a method that can effectively control the recrystallization behavior of metals. Its essence is to make the high-density dislocations remaining after deformation fully move and rearrange through long-term recovery treatment, thereby eliminating the energy storage of some deformed metals and adding new recrystallization nucleation points, so that the metal can obtain the fine-grained structure inherited from deformation.
[0006] At present, the most commonly used pre-recovery treatment method is to anneal the deformed material for a long time in an environment below the recrystallization temperature. However, from the research results so far, the effect of pre-recovery treatment on suppressing the grain growth of deformed alloys is limited, and the deformed structure will still undergo obvious grain growth after high-temperature processing. The reason is that the current technical methods only apply a temperature field to the metal, which cannot fully move the dislocations of the deformed metal. This results in the inability to completely eliminate the deformation storage energy of the deformed metal. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a method for inhibiting metal grain recrystallization, an aluminum alloy and a preparation method thereof, which can effectively inhibit the recrystallization and growth of metal grains, reduce the grain size and improve the strain capacity of the metal.
[0008] An embodiment of the present invention provides a method for inhibiting the recrystallization of metal grains, wherein the metal is placed under pressure and maintained at an annealing temperature, wherein the initial pressure of the metal per unit area is greater than 100% of the yield strength of the metal and less than 130% of the yield strength of the metal, and the yield strength of the metal is the yield strength of the metal at the annealing temperature; the metal is an aluminum alloy with fine grains, and the holding time is 3 to 11 hours.
[0009] Keeping the metal under pressure is called "holding pressure". The initial pressure F of the "holding pressure" treatment is calculated by the following formula: Wherein, K2 is the pressure coefficient, K2 is greater than 0.6, preferably greater than 0.7, more preferably greater than 1.0 and less than 1.3 (more preferably greater than 1.0 and less than 1.1); S is the cross-sectional area of the metal; The yield strength of the metal at the "pressure holding" treatment temperature. Pressure exceeding the above range does not significantly improve the effect of inhibiting recrystallization. The pressure holding time is 3 to 11 hours, preferably 5 to 7 hours.
[0010] The present invention limits the initial pressure. According to the concept of "stress relaxation" in materials science, in a material that maintains a constant deformation, the stress will decrease with the increase of time. Therefore, during the "pressure-maintaining annealing" process, the strain is kept constant and the pressure will gradually decrease.
[0011] In one embodiment, the annealing temperature is greater than 35% of the melting point of the metal and less than 55% of the melting point of the metal.
[0012] Preferably, the temperature is greater than 40% of the melting point of the metal.
[0013] The metal is also kept at a certain temperature, i.e. "annealed", and the temperature T of the annealing treatment is calculated by the following formula: , where K 1 is the temperature coefficient, ranging from 0.35 to 0.55; T m The melting point of the metal. The time for heat preservation annealing is generally the same as that for pressure preservation treatment.
[0014] In one embodiment, when the metal is placed under pressure, the strain rate of the metal is no more than 1s -1 Preferably, the strain rate of the metal is not greater than 0.1s -1 .
[0015] In one embodiment, the preparation method of the aluminum alloy with fine grains is to subject the aluminum alloy to large plastic deformation, such as equal-diameter angular extrusion, high-temperature multi-directional forging or high-pressure torsion. Large plastic deformation is preferably high-temperature multi-directional forging; preferably, the steps of high-temperature multi-directional forging are three-upsetting and three-drawing, and the X, Y and Z directions of the blank are upset and drawn once respectively, the single deformation amount is 50-70%, the forging temperature is 300℃-400℃, and the final forging temperature is ≥200℃.
[0016] The embodiment of the present invention provides a method for preparing an aluminum alloy, wherein an aluminum alloy with fine grains is treated according to the method for inhibiting metal grain recrystallization, cooled, and solution treated to obtain the aluminum alloy.
[0017] An embodiment of the present invention provides an aluminum alloy obtained by using the aluminum alloy preparation method.
[0018] The beneficial effect of the present invention is that, in order to suppress the recrystallization and abnormal grain growth problems of the forging billet during high-temperature processing, the present invention proposes a method for preparing a micron-fine-grained aluminum alloy forging billet with high thermal stability, by applying a stress field to the aluminum alloy forging billet during the pre-recovery treatment, under the synergistic effect of the temperature field and the stress field, the dislocation movement is more intense, thereby eliminating the recrystallization driving force as thoroughly as possible and suppressing the formation of coarse grains.
[0019] The present invention applies a stress field in a conventional pre-recovery treatment process so that the fine-grained forging blank obtained by multi-directional forging is subjected to the synergistic effect of force and temperature during the pre-recovery process, thereby fully eliminating the distortion energy of the forging blank, effectively improving the thermal stability of the grain structure of the forging blank, inhibiting its recrystallization and the formation of coarse grains during high-temperature processing or annealing, and providing excellent conditions for improving the strength and plasticity of the material and reducing anisotropy.
[0020] After the aluminum alloy is subjected to a "pressure-holding annealing" pre-recovery treatment by the annealing method provided by the present invention, the average grain size of the pressure-holding annealing aluminum alloy after solution treatment is only 7.44 μm, while the average grain size of the untreated alloy is as high as 167.12 μm, and the average grain size of the alloy subjected to conventional pre-recovery treatment is also 90.44 μm. It can be seen that the process method of the present invention can greatly inhibit recrystallization and the formation of coarse grains. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a grain structure diagram of the forging blank after multi-directional forging of the present invention after air cooling to room temperature.
[0022] Figure 2 This is the grain structure diagram of the pressure-maintained annealing forging billet after solution treatment in Example 1 of the present invention.
[0023] Figure 3This is the grain structure diagram of the press-annealed forging billet after solution treatment in Example 2 of the present invention.
[0024] Figure 4 This is the grain structure diagram of the press-annealed forging billet after solution treatment in Example 3 of the present invention.
[0025] Figure 5 This is the grain structure diagram of the press-annealed forging billet after solution treatment in Example 4 of the present invention.
[0026] Figure 6 This is the grain structure diagram of the pressure-maintained annealing forging billet after solution treatment in Comparative Example 1 of the present invention.
[0027] Figure 7 This is the grain structure diagram of the pressure-maintained annealing forging billet after solution treatment in Comparative Example 2 of the present invention.
[0028] Figure 8 This is the grain structure diagram of the pressure-maintained annealing forging billet after solution treatment in Comparative Example 3 of the present invention.
[0029] Fig. 9 This is the grain structure diagram of the forging blank after solution treatment in Comparative Example 4 of the present invention.
[0030] Fig.10 This is the grain structure diagram of the forging billet after solution treatment in Comparative Example 5 of the present invention.
[0031] Fig.11 It is a statistical diagram of the average grain size of Examples 1 to 4 of the present invention and Comparative Examples 1 to 5.
[0032] Fig.12 The engineering stress-strain curves of Example 2, Comparative Example 4 and Comparative Example 5 of the present invention after aging treatment are shown in FIG.
[0033] Fig.13 This is the grain structure diagram of the pressure-maintained annealing forging billet after solution treatment in Example 5 of the present invention.
[0034] Fig.14 This is the grain structure diagram of the press-annealed forging billet after solution treatment in Example 6 of the present invention. DETAILED DESCRIPTION
[0035] The present invention provides a method for preparing a high thermal stability micron fine-grained aluminum alloy forging billet, comprising: performing multi-directional forging on the aluminum alloy to obtain a fine-grained casting billet; and then performing a "pressure-holding annealing" pre-recovery treatment to obtain a "pressure-holding annealing" fine-grained casting billet.
[0036] In the present invention, the "pressure-holding annealing" pre-recovery treatment is an annealing treatment method; the "pressure-holding annealing" pre-recovery treatment refers to an annealing method in which a constant temperature field is applied while compressing the forging blank to a certain initial force and keeping the strain unchanged.
[0037] The present invention will be further described in detail below with reference to specific embodiments. Example 1
[0038] In the heat treatment method for inhibiting the recrystallization and grain growth of aluminum alloy described in this embodiment, the alloy grade used is 2195 alloy, and the alloy composition mass percentage is: Si: 0.03, Fe: 0.04, Cu: 4.1, Mn: 0.04, Mg: 0.28, Zr: 0.13, Ag: 0.26, Li: 0.9, and the rest is Al. The melting point of the alloy described in this embodiment is 660°C.
[0039] The alloy was processed into billets with dimensions of 100 × 130 × 167 mm (length 100 mm, width 130 mm, height 167 mm).
[0040] High temperature multi-directional forging: The billet is heated to 400℃ and multi-directional forging is performed by three upsetting and three drawing. The single deformation is 60%. The final forging temperature is 290℃. Finally, the billet is shaped into a rectangular shape of 120×120×151mm (length 120mm, width 120mm, height 151mm). The forging billet after multi-directional forging is air-cooled to room temperature. The grain structure diagram is as follows Figure 1 shown.
[0041] The yield strength of the alloy at 360°C was measured to be 56 MPa.
[0042] The "pressure-maintaining annealing" treatment process is adopted, and the specific steps are as follows:
[0043] Heat the forging blank to 360℃ (K1 is approximately 0.55). Compress the forging blank until the force reaches 800KN (K2 is approximately 1.0), and keep the mold still. After pressure annealing for 5h, air cool to room temperature. The treated alloy is solution treated. The solution treatment temperature is 510℃ and the holding time is 1h. EBSD detects the grain structure after solution treatment. Example 2
[0044] The difference between Example 2 and Example 1 is that the “pressure holding annealing” time is 7 hours, and the rest is the same as Example 1. Example 3
[0045] The only difference between Example 3 and Example 2 is that the "pressure holding annealing" temperature is 260° C. (K1 is approximately 0.4), and the rest is the same as Example 2. Example 4
[0046] The only difference between Example 4 and Example 2 is that the pressure of "pressure-holding annealing" is 650 KN (K2 is approximately 0.8), and the rest is the same as Example 2. Comparative Example 1
[0047] The only difference between Comparative Example 1 and Example 2 is that the “pressure holding annealing” temperature is 200° C. (K1 is approximately 0.3), and the rest is the same as Example 2. Comparative Example 2
[0048] The difference between Comparative Example 2 and Example 2 is that the “pressure holding annealing” temperature is 400° C. (K1 is 0.6), and the rest is the same as Example 2. Comparative Example 3
[0049] The difference between Comparative Example 3 and Example 2 is that the pressure of "pressure holding annealing" is 400KN (K2 is 0.5), and the rest is the same as Example 2. Comparative Example 4
[0050] The materials used in Comparative Example 4 are the same as those in Example 1. In Comparative Example 4, the multi-directional forging blank is directly subjected to solid solution treatment. The solid solution treatment system is the same as that in Example 1. EBSD is used to detect the grain structure after solid solution treatment. Comparative Example 5
[0051] The difference between Comparative Example 5 and Comparative Example 4 is that the forging blank is kept at 360° C. for 7 hours before the solution treatment and then air-cooled to room temperature. The rest is the same as Comparative Example 4.
[0052] The grain structure and size diagram of each embodiment and comparative example are shown in FIG. Figure 1-11 As shown, the engineering stress-strain curves of Example 2, Comparative Example 4 and Comparative Example 5 after aging treatment are as shown in Fig.12 As shown, it can be seen that the present invention greatly suppresses recrystallization and the formation of coarse grains. Example 5
[0053] The only difference between Example 5 and Example 2 is that the pressure of "pressure holding annealing" is 880KN (K2 is approximately 1.1), and the rest is the same as Example 2. Example 6
[0054] The only difference between Example 6 and Example 2 is that the pressure of "pressure-holding annealing" is 1040 KN (K2 is approximately 1.3), and the rest is the same as Example 2.
[0055] The experimental results are as follows Figure 13-14 shown.
[0056] A person skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of protection of the present application is limited to these examples. In line with the concept of the present application, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of different aspects of one or more embodiments of the present application as described above, which are not provided in detail for the sake of simplicity.
[0057] One or more embodiments of the present application are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the present application. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of one or more embodiments of the present application should be included in the protection scope of the present application.
Claims
1. A method for inhibiting recrystallization of metal grains, Its characteristics are: The metal is placed under pressure and maintained at an annealing temperature, wherein the initial pressure of the metal per unit area is greater than 100% of the yield strength of the metal and less than 130% of the yield strength of the metal, wherein the yield strength of the metal is the yield strength of the metal at the annealing temperature; the metal is an aluminum alloy with fine grains, and the holding time is 3 to 11 hours; The annealing temperature is greater than 35% of the melting point of the metal and less than 55% of the melting point of the metal.
2. The method according to claim 1, Its characteristics are: The holding time is 5-7h.
3. The method according to claim 2, Its characteristics are: The initial pressure is greater than 100% of the yield strength of the metal and less than 110% of the yield strength of the metal.
4. The method according to claim 1, Its characteristics are: The annealing temperature is greater than 40% of the melting point of the metal and less than 55% of the melting point of the metal.
5. The method according to any one of claims 1 to 3, Its characteristics are: When a metal is placed under pressure, the strain rate of the metal is no more than 1s -1 .
6. The method according to claim 1, Its characteristics are: The method for preparing the aluminum alloy with fine grains is to subject the aluminum alloy to large plastic deformation.
7. A method for preparing an aluminum alloy, Its characteristics are: An aluminum alloy with fine grains is treated according to the method as described in any one of claims 1 to 6, cooled, and solution treated to obtain an aluminum alloy with fine grains.
8. An aluminum alloy, Its characteristics are: The preparation method as claimed in claim 7 is used to obtain the
Citation Information
Patent Citations
Manufacturing method of aluminum alloy thin plate with stable performance
CN102876940A
Preparation method of aluminum alloy strip with high yield strength after baking
CN115679166A