A planar transfer stamp with a multi-layer composite structure and a preparation method thereof
By using the plane transfer seal of a multi-layer composite structure during the bonding process of Micro-LED chips, the deformation layer and adhesion layer of silicone oil and polymer materials is used to solve the problem that excessive viscosity will cause the chip to not be able to remain on the substrate. , realizes efficient LED chip transfer and fixation, reducing production costs and process complexity.
Patent Information
- Application Number
- CN202411334446.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-24
AI Technical Summary
The existing huge transfer technology During the bonding process of Micro-LED chips, excessive viscosity will cause the chip to be unable to remain on the target substrate, and the parallelism problem between the flat seal and the substrate will lead to poor bonding effect. It is difficult to promote the adsorption layer that relies on high-cost photothermal conversion layer and magnetic field control.
Planar transfer seals with multi-layer composite structures include substrate, adsorption layer, deformation layer and adhesion layer. The deformation layer is composed of silicone oil and polymer materials. It can deform when under stress, and change the viscosity through heating to avoid adhesion. Problems that are too big or too small.
It achieves the maintenance of sufficient deformation ability and adhesion during the bonding process, ensuring that the LED chip can be transferred and fixed on the target substrate smoothly, reducing production costs and process complexity.
Smart Images

Figure CN118841360B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a planar transfer stamp with a multi-layer composite structure and a preparation method thereof, belonging to the technical field of semiconductor device manufacturing. Background Art
[0002] As one of the prospects of the next generation of display technology, Micro-LED has become a hot research field. It is a light-emitting diode similar to traditional LED, but with smaller size, higher brightness and lower energy consumption. Compared with traditional liquid crystal display technology and organic light-emitting diode (OLED), Micro-LED has higher contrast, faster response speed and wider color gamut. However, the development of Micro-LED still faces many obstacles, mainly the limitations of growth technology, mass transfer technology and full-color technology, among which mass transfer technology is a key issue that needs to be overcome urgently.
[0003] Mass transfer technology is a key technology for Micro-LED to achieve mass production. This technology aims to transfer three-color Micro-LED chips from the epitaxial substrate to the target substrate in large quantities, at high speed and accurately through high-precision precision equipment, and to achieve reliable electrical and mechanical connections between the LED chip and the driving circuit. This technology requires the use of micro-operation processes and precision equipment, such as microscopic robotic arms, to ensure that each Micro-LED chip can be accurately positioned and fixed on the target substrate. This precise transfer process is an important step to ensure efficient mass production. Currently, the more mature mass transfer technologies in the industry include bonding technology, laser transfer technology, fluid self-assembly technology and roller transfer technology. The pick-and-place technology relies on adhesion to pick up the chip from the temporary substrate and place it on the target substrate.
[0004] The adhesive force of the elastomer stamp used in bonding technology can pick up the chip and bond it to the target substrate. However, in the actual bonding process, the adhesive force of the elastomer stamp is too large, so that the chip cannot stay on the target substrate; the parallelism problem between the flat stamp and the substrate will also make it impossible for the two to fit tightly, resulting in unsatisfactory bonding results.
[0005] The Chinese patent application with application number 202111282168.2 discloses an LED transfer device and an LED transfer method. The light-to-heat conversion layer of the device can be deformed under the irradiation of polarized light, and the adsorption layer can change viscosity under the action of a magnetic field.
[0006] The photothermal conversion layer of this method needs to be irradiated with polarized light to deform, while the adsorption layer needs to rely on the action of the magnetic field to change the viscosity. Both have relatively high requirements on production process, environment and cost during production, making them difficult to promote. Summary of the invention
[0007] In order to overcome the above problems, the present invention provides a planar transfer stamp with a multi-layer composite structure and a preparation method thereof, wherein the planar transfer stamp deforms when subjected to force to ensure that the stamp fits the target substrate. The adhesion between the stamp and the chip can be changed by heating to avoid the situation where the adhesion is too small to pick up the chip, and the adhesion is too large to leave the chip on the target substrate.
[0008] The technical solution of the present invention is as follows:
[0009] In a first aspect, a planar transfer stamp with a multi-layer composite structure includes a substrate and an adsorption layer disposed on the substrate, the adsorption layer can adsorb an LED chip, a deformation layer is disposed between the substrate and the adsorption layer, the deformation layer can deform when subjected to force; an adhesion layer is also disposed between the substrate and the deformation layer, the adhesion layer can adhere to the substrate and the deformation layer;
[0010] The deformation layer is composed of silicone oil and polymer material A, and the polymer material A is composed of one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin; the mass fraction of the silicone oil is 5% to 30%.
[0011] Furthermore, the viscoelasticity of the silicone oil is 5.0×10 2 ~6.0×10 5 mPa.s.
[0012] Furthermore, when the polymer material A is composed of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, the mass fraction of polyimide is 10%~40%, the mass fraction of polydimethylsiloxane is 10%~40%, the mass fraction of silicone rubber is 15%~40%, and the mass fraction of epoxy resin is 10%~40%.
[0013] Furthermore, the viscoelasticity of the adsorption layer may change when heated.
[0014] Furthermore, the adsorption layer is composed of a polymer material B, and the polymer material B is composed of one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin.
[0015] Furthermore, when the polymer material B is composed of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, the mass fraction of polyimide is 10%~40%, the mass fraction of polydimethylsiloxane is 10%~40%, the mass fraction of silicone rubber is 20%~40%, and the mass fraction of epoxy resin is 10%~40%, wherein the weight ratio of polydimethylsiloxane: silicone rubber is ≠1:1.
[0016] Furthermore, the adhesion layer is composed of a silane coupling agent and a polymer material C, the polymer material C is composed of one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, and the mass fraction of the silane coupling agent is 5% to 30%; the substrate is composed of one or more of glass, silicon wafer, and sapphire; before the adhesion layer is formed on the surface of the substrate, the surface of the substrate is treated with oxygen plasma or Piranha lotion.
[0017] Furthermore, when the polymer material C is composed of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, the mass fraction of polyimide is 10%~40%, the mass fraction of polydimethylsiloxane is 10%~40%, the mass fraction of silicone rubber is 15%~40%, and the mass fraction of epoxy resin is 10%~40%.
[0018] Furthermore, the material components of the adhesion layer, the deformation layer and the adsorption layer include at least one same polymer material.
[0019] In a second aspect, a method for preparing a planar transfer stamp having a multi-layer composite structure is provided, which is used to prepare the planar transfer stamp having a multi-layer composite structure as described in the first aspect, comprising the following steps:
[0020] The substrate surface is treated with oxygen plasma or Piranha solution;
[0021] A material composed of a silane coupling agent and a polymer material C is applied to the surface of the substrate to form a single-layer planar stamp; the polymer material C is one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin;
[0022] Performing a heating and curing treatment on the single-layer plane seal;
[0023] Applying a material composed of silicone oil and polymer material A to the coating side of the single-layer plane stamp to form a double-layer plane stamp; the polymer material A is one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin;
[0024] Performing a heating and curing process on the double-layer plane seal;
[0025] Applying polymer material B to the coating-containing side of the single-layer planar stamp to form a multi-layer planar stamp; the polymer material B is one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin;
[0026] The multi-layer planar stamp is subjected to a heating and curing treatment.
[0027] The present invention has the following beneficial effects:
[0028] The multi-layer flat stamp has an additional adhesive layer, in which a silane coupling agent is added, so that the adhesion of the adhesive surface to the substrate is improved and edge lifting is effectively prevented.
[0029] The deformation layer of the multi-layer flat seal is doped with silicone oil, which will not react with other polymer materials, has good thermal stability, still has rheological properties at high temperatures, can deform under the pressure of bonding, and is not affected by the high temperature of the bonding process.
[0030] The adsorption layer of the multi-layer planar stamp can be subjected to heat treatment to change the adhesive force, thereby preventing the chip from being unable to remain on the target substrate due to excessive adhesive force. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the planar transfer seal structure of the prior art.
[0032] Figure 2 Schematic diagram of bonding when the planar transfer stamp is not parallel to the target substrate.
[0033] Figure 3 Schematic diagram of bonding when the adhesion of the traditional seal glue surface is too large.
[0034] Figure 4 It is a schematic diagram of the process of preparing a planar transfer stamp of the present invention.
[0035] Figure 5 It is a schematic diagram of the bonding process of the planar transfer stamp of the present invention.
[0036] The reference numerals in the figure represent:
[0037] 1. Substrate; 2. Traditional stamp adhesive surface; 3. Chip; 4. Target substrate; 5. Adhesion layer; 6. Deformation layer; 7. Adsorption layer. DETAILED DESCRIPTION
[0038] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0039] refer to Figure 1 A commonly used planar transfer stamp includes a substrate 1 and a traditional stamp adhesive surface 2.
[0040] refer to Figure 2 During bonding, if the plane transfer stamp is not parallel to the target substrate 4 , the chips 3 on the plane transfer stamp cannot be completely transferred to the target substrate 4 .
[0041] refer to Figure 3 During bonding, if the adhesion between the planar transfer stamp and the chip 3 is too large, the chip 3 will not be able to remain on the target substrate 4.
[0042] First, refer to Figure 4A planar transfer stamp with a multi-layer composite structure comprises a substrate 1 and an adsorption layer 7 arranged on the substrate 1, wherein the adsorption layer 7 can adsorb an LED chip, a deformation layer 6 is arranged between the substrate 1 and the adsorption layer 7, and the deformation layer 6 can be deformed when subjected to force; an adhesion layer 5 is also arranged between the substrate 1 and the deformation layer 6, and the adhesion layer 5 can adhere to the substrate 1 and the deformation layer 6;
[0043] The deformation layer 6 is composed of silicone oil and polymer material A, wherein the polymer material A is composed of one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin; the mass fraction of the silicone oil is 5% to 30%.
[0044] When preparing the transfer stamp, a material composed of silicone oil and polymer material A is coated on the surface of the substrate 1. After heat treatment, the molecular material A can form a stable polymer network, and the silicone oil is dispersed in the polymer network in liquid form to ensure that the deformation layer 6 still has rheological properties after high-temperature treatment, providing sufficient deformation for the bonding process.
[0045] refer to Figure 5 When the plane transfer stamp is not parallel to the target substrate 4 , due to different forces at different positions of the plane transfer stamp during the bonding process, the deformation amounts of different positions of the deformation layer 6 are also different, so that the bottom adsorption layer 7 can better contact with the target substrate 4 .
[0046] In one embodiment of the present invention, the viscoelasticity of the silicone oil is 5.0×10 2 ~6.0×10 5 mPa.s.
[0047] In one embodiment of the present invention, when the polymer material A is composed of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, the mass fraction of polyimide is 10%~40%, the mass fraction of polydimethylsiloxane is 10%~40%, the mass fraction of silicone rubber is 15%~40%, and the mass fraction of epoxy resin is 10%~40%.
[0048] In one embodiment of the present invention, the viscoelasticity of the adsorption layer 7 may change when heated.
[0049] Compared with magnetic field control of viscoelasticity, temperature control is easier.
[0050] In one embodiment of the present invention, the adsorption layer 7 is composed of a polymer material B, and the polymer material B is composed of one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin.
[0051] During bonding, the planar transfer stamp is heat treated. After the heat treatment, the polymer material of the adsorption layer 7 is cross-linked and loses its adhesive force, thereby leaving the chip on the target substrate 4.
[0052] When the polymer material B is composed of one of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, the mass fraction of polyimide, polydimethylsiloxane, silicone rubber or epoxy resin is 100%.
[0053] In one embodiment of the present invention, when the polymer material B is composed of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, the mass fraction of polyimide is 10%~40%, the mass fraction of polydimethylsiloxane is 10%~40%, the mass fraction of silicone rubber is 20%~40%, and the mass fraction of epoxy resin is 10%~40%, wherein the weight ratio of polydimethylsiloxane: silicone rubber is ≠1:1.
[0054] In one embodiment of the present invention, the adhesion layer 5 is composed of a silane coupling agent and a polymer material C, the polymer material C is composed of one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, and the mass fraction of the silane coupling agent is 5% to 30%; the substrate 1 is composed of one or more of glass, silicon wafer, and sapphire; before the adhesion layer 5 is formed on the surface of the substrate 1, the surface of the substrate 1 is treated with oxygen plasma or Piranha lotion.
[0055] In order to prevent the deformation layer 6 from falling off from the substrate 1 , an adhesion layer 5 is arranged between the deformation layer 6 and the substrate 1 . The adhesion layer 5 can adhere the substrate 1 and the deformation layer 6 .
[0056] Preferably, the substrate 1 is made of quartz glass.
[0057] The surface of the substrate 1 is treated with oxygen plasma or Piranha solution to obtain a large number of hydroxyl groups on the surface of the substrate 1. The polymer material C forms a stable -Si-O-Si- bond with the hydroxyl-rich surface of the substrate 1 based on the silane coupling agent, thereby achieving stable adhesion.
[0058] In one embodiment of the present invention, when the polymer material C is composed of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, the mass fraction of polyimide is 10% to 40%, the mass fraction of polydimethylsiloxane is 10% to 40%, the mass fraction of silicone rubber is 15% to 40%, and the mass fraction of epoxy resin is 10% to 40%.
[0059] In one embodiment of the present invention, the material components of the adhesion layer 5 , the deformation layer 6 , and the adsorption layer 7 include at least one same polymer material.
[0060] In a second aspect, a method for preparing a planar transfer stamp having a multi-layer composite structure is provided, which is used to prepare the planar transfer stamp having a multi-layer composite structure as described in the first aspect, comprising the following steps:
[0061] The surface of the substrate 1 is treated with oxygen plasma or Piranha solution;
[0062] A material composed of a silane coupling agent and a polymer material C is coated on the surface of the substrate 1 to form a single-layer planar stamp; the polymer material C is one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin;
[0063] Performing a heating and curing treatment on the single-layer plane seal;
[0064] Applying a material composed of silicone oil and polymer material A to the coating side of the single-layer plane stamp to form a double-layer plane stamp; the polymer material A is one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin;
[0065] Performing a heating and curing process on the double-layer plane seal;
[0066] Applying polymer material B to the coating-containing side of the single-layer planar stamp to form a multi-layer planar stamp; the polymer material B is one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin;
[0067] The multi-layer planar stamp is subjected to a heating and curing treatment.
[0068] The following are some embodiments of the present invention.
[0069] Example 1
[0070] The substrate 1 is made of ordinary glass, and the surface of the substrate 1 is treated by oxygen plasma.
[0071] Three mixed solutions were prepared, the first of which was composed of 85% by mass of polydimethylsiloxane and 15% by mass of a silane coupling agent.
[0072] The second part is composed of 80% polydimethylsiloxane and silicone oil (viscosity 5.0×10 2 mPa.s) mass ratio is 20%.
[0073] The third part is composed of 100% polydimethylsiloxane by mass.
[0074] A single-layer planar transfer stamp was obtained by spin coating, and then the single-layer planar transfer stamp was heat-treated on a hot plate at a temperature of 100° C. for 5 min.
[0075] Subsequently, the second mixed solution was coated on the surface of the single-layer planar transfer stamp by spin coating to obtain a double-layer planar transfer stamp, and then the double-layer planar transfer stamp was heat-treated on a hot plate at a temperature of 100° C. for 5 minutes.
[0076] Subsequently, the third mixed solution was coated on the surface of the double-layer planar transfer stamp by spin coating to obtain a multi-layer planar transfer stamp, and then the multi-layer planar transfer stamp was heat-treated at 200° C. for 10 min using a hot plate.
[0077] The total thickness of the multi-layer planar transfer stamp is 46 μm, the deformation is 20 μm, and the adhesion is 0.001 MPa.
[0078] The planar transfer stamp with a multi-layer composite structure prepared in the above steps is applied to actual bonding. An LED chip array is adhered to the stamp, and there are indium bumps on the target substrate 4. The stamp and the target substrate 4 are aligned and hot-pressed and bonded, and the LED chip can be successfully bonded to the target substrate 4.
[0079] Example 2
[0080] The substrate 1 is made of sapphire, and the surface of the substrate 1 is treated by Piranha washing solution.
[0081] Three mixed solutions were prepared, the first of which consisted of 70% by mass of silicone rubber and 30% by mass of silane coupling agent.
[0082] The second part is composed of 70% silicone rubber and silicone oil (viscosity 6.0×10 5 mPa.s) mass ratio is 30%.
[0083] The third part is 100% silicone rubber by mass.
[0084] A single-layer planar transfer stamp was obtained by spin coating, and then the single-layer planar transfer stamp was heat-treated in an oven at a temperature of 250° C. for 3 min.
[0085] Subsequently, the second mixed solution was coated on the surface of the single-layer planar transfer stamp by spin coating to obtain a double-layer planar transfer stamp, and then the double-layer planar transfer stamp was heat-treated in an oven at a temperature of 250° C. for 1 min.
[0086] Subsequently, a multilayer planar transfer stamp was obtained by spin coating, and then the multilayer planar transfer stamp was heat treated on a hot plate at a temperature of 250° C. for 1 min.
[0087] The total thickness of the prepared multi-layer planar transfer stamp is 100 μm, the deformation is 30 μm, and the adhesion is 0.1 MPa.
[0088] The planar transfer stamp with a multi-layer composite structure prepared in the above steps is applied to actual bonding. An LED chip array is adhered to the stamp, and there are indium bumps on the target substrate 4. The stamp and the target substrate 4 are aligned and hot-pressed and bonded, and the LED chip can be successfully bonded to the target substrate 4.
[0089] Example 3
[0090] The substrate 1 is composed of a silicon wafer, and the surface of the substrate 1 is treated by oxygen plasma.
[0091] Three mixed solutions were prepared, the first of which was composed of 95% by mass of polyimide and 5% by mass of silane coupling agent.
[0092] The second part is composed of 70% polyimide by mass, silicone oil (viscosity 1.0×10 3 mPa.s) mass ratio is 30%.
[0093] The third part has a polyimide mass ratio of 100%.
[0094] A single-layer plane transfer stamp was obtained by scraping, and then the single-layer plane transfer stamp was heat-treated on a hot plate at a temperature of 150° C. for 3 min.
[0095] Subsequently, the second mixed solution was coated on the surface of the single-layer planar transfer stamp by blade coating to obtain a double-layer planar transfer stamp, and then the double-layer planar transfer stamp was heat-treated at 80° C. for 5 min on a hot plate.
[0096] Subsequently, the third mixed solution was coated on the surface of the double-layer planar transfer stamp by blade coating to obtain a multi-layer planar transfer stamp, and then the multi-layer planar transfer stamp was heat-treated at 150° C. for 5 minutes using a hot plate.
[0097] The total thickness of the multi-layer planar transfer stamp is 500 μm, the deformation is 230 μm, and the adhesion is 0.05 MPa.
[0098] The planar transfer stamp with a multi-layer composite structure prepared in the above steps is applied to actual bonding. An LED chip array is adhered to the stamp, and there are indium bumps on the target substrate 4. The stamp and the target substrate 4 are aligned and hot-pressed and bonded, and the LED chip can be successfully bonded to the target substrate 4.
[0099] Example 4
[0100] The substrate 1 is made of quartz glass, and the surface of the substrate 1 is treated by oxygen plasma.
[0101] Three mixed solutions were prepared, the first of which was composed of 95% by mass of epoxy resin and 5% by mass of silane coupling agent.
[0102] The second part is composed of 70% epoxy resin and 30% silicone oil (viscosity 3.0×103mPa.s).
[0103] The third part is made of 100% epoxy resin by mass.
[0104] The first mixed solution was applied to the surface of a glass substrate by spin coating to obtain a single-layer planar transfer stamp, and then the single-layer planar transfer stamp was heat-treated at 80° C. for 10 minutes on a hot plate.
[0105] Subsequently, the second mixed solution was coated on the surface of the single-layer planar transfer stamp by spin coating to obtain a double-layer planar transfer stamp, and then the double-layer planar transfer stamp was heat-treated at 80° C. for 10 min on a hot plate.
[0106] Subsequently, the third mixed solution was coated on the surface of the double-layer planar transfer stamp by spin coating, and a multi-layer planar transfer stamp was obtained by spin coating, scraping and spraying. The multi-layer planar transfer stamp was then heat treated at 100° C. for 20 min using a hot plate.
[0107] The total thickness of the multi-layer planar transfer stamp is 1000 μm, the deformation is 130 μm, and the adhesion is 0.03 MPa.
[0108] The planar transfer stamp with a multi-layer composite structure prepared in the above steps is applied to actual bonding. An LED chip array is adhered to the stamp, and there are indium bumps on the target substrate 4. The stamp and the target substrate 4 are aligned and hot-pressed and bonded, and the LED chip can be successfully bonded to the target substrate 4.
[0109] Example 5
[0110] The substrate 1 is made of ordinary glass, and the surface of the substrate 1 is treated with Piranha washing liquid.
[0111] Three mixed solutions were prepared. The first one was composed of a combination of various polymers with a weight ratio of 30% polyimide, 10% polydimethylsiloxane, 10% silicone rubber, 20% epoxy resin and 30% silane coupling agent.
[0112] The second part is a combination of various polymers with a mass ratio of 10% polyimide, 10% polydimethylsiloxane, 40% silicone rubber, 10% epoxy resin, silicone oil (viscosity 5.0×10 2 mPa.s) mass ratio is 30%.
[0113] The third part is composed of a combination of various polymers with a mass ratio of 30% polyimide, 20% polydimethylsiloxane, 30% silicone rubber, and 20% epoxy resin.
[0114] The first mixed solution was coated on the surface of a glass substrate by spraying to obtain a single-layer plane transfer stamp, and then the single-layer plane transfer stamp was heat-treated at a temperature of 100° C. and a treatment time of 10 minutes by a hot plate.
[0115] Subsequently, the second mixed solution was coated on the surface of the single-layer planar transfer stamp by spraying to obtain a double-layer planar transfer stamp, and then the double-layer planar transfer stamp was heat-treated at 100° C. for 5 minutes using a hot plate.
[0116] Subsequently, the third mixed solution was coated on the surface of the double-layer planar transfer stamp by spraying to obtain a multi-layer planar transfer stamp, and then the multi-layer planar transfer stamp was heat-treated with a hot plate at a temperature of 150° C. for 20 minutes.
[0117] The total thickness of the prepared multi-layer planar transfer stamp is 1000 μm, the deformation is 500 μm, and the adhesion is 0.001 MPa.
[0118] The planar transfer stamp with a multi-layer composite structure prepared in the above steps is applied to actual bonding. An LED chip array is adhered to the stamp, and there are indium bumps on the target substrate 4. The stamp and the target substrate 4 are aligned and hot-pressed and bonded, and the LED chip can be successfully bonded to the target substrate 4.
[0119] Example 6
[0120] The substrate 1 is made of sapphire, and the surface of the substrate 1 is treated by Piranha washing solution.
[0121] Three mixed solutions were prepared. The first one was composed of a combination of various polymers with a weight ratio of 40% polyimide, 10% polydimethylsiloxane, 15% silicone rubber, 30% epoxy resin and 5% silane coupling agent.
[0122] The second part is a combination of various polymers with a mass ratio of 10% polyimide, 40% polydimethylsiloxane, 20% silicone rubber, 10% epoxy resin, silicone oil (viscosity 9.0×10 3 mPa.s) mass ratio is 20%.
[0123] The third part is composed of a combination of various polymers with a mass ratio of 10% polyimide, 40% polydimethylsiloxane, 20% silicone rubber, and 30% epoxy resin.
[0124] The first mixed solution was applied to the surface of a glass substrate by spin coating to obtain a single-layer planar transfer stamp, and then the single-layer planar transfer stamp was heat-treated at 250° C. for 1 min on a hot plate.
[0125] Subsequently, the second mixed solution was coated on the surface of the single-layer planar transfer stamp by spin coating to obtain a double-layer planar transfer stamp, and then the double-layer planar transfer stamp was heat-treated at 80° C. for 1 min on a hot plate.
[0126] Then, the third mixed solution was applied to the surface of the double-layer planar transfer stamp by spin coating to obtain a multi-layer planar transfer stamp, and then the multi-layer planar transfer stamp was heat-treated at 80°C for 1 min using a hot plate. The total thickness of the multi-layer planar transfer stamp was 600 μm, the deformation was 350 μm, and the adhesion was 0.3 MPa.
[0127] The planar transfer stamp with a multi-layer composite structure prepared in the above steps is applied to actual bonding. An LED chip array is adhered to the stamp, and there are indium bumps on the target substrate 4. The stamp and the target substrate 4 are aligned and hot-pressed and bonded, and the LED chip can be successfully bonded to the target substrate 4.
[0128] The following are some comparative examples for comparing the embodiments of the present invention.
[0129] Comparative Example 1
[0130] The substrate 1 is made of quartz glass, and the surface of the substrate 1 is treated by oxygen plasma.
[0131] Three mixed solutions were prepared, the first of which was composed of 95% by mass of epoxy resin and 5% by mass of silane coupling agent.
[0132] The second part is composed of 100% epoxy resin and 0% silicone oil.
[0133] The third part is made of 100% epoxy resin by mass.
[0134] The first mixed solution was applied to the surface of a glass substrate by spin coating to obtain a single-layer planar transfer stamp, and then the single-layer planar transfer stamp was heat-treated at 80° C. for 10 minutes on a hot plate.
[0135] Subsequently, the second mixed solution was coated on the surface of the single-layer planar transfer stamp by spin coating to obtain a double-layer planar transfer stamp, and then the double-layer planar transfer stamp was heat-treated at 80° C. for 10 min on a hot plate.
[0136] Subsequently, the third mixed solution was coated on the surface of the double-layer planar transfer stamp by spin coating, and a multi-layer planar transfer stamp was obtained by spin coating, scraping and spraying. The multi-layer planar transfer stamp was then heat treated at 100° C. for 20 min using a hot plate.
[0137] The total thickness of the multi-layer planar transfer stamp was 1000 μm, the deformation was 0 μm, and the adhesive force was 0.001 MPa. The planar transfer stamp with a multi-layer composite structure prepared in the above steps was applied to actual bonding, but the stamp could not transfer and bond the LED chip array.
[0138] Comparative Example 2
[0139] The substrate 1 is made of ordinary glass, and the surface of the substrate 1 is treated by oxygen plasma.
[0140] Three mixed solutions were prepared, the first of which was composed of 100% polydimethylsiloxane by mass and 0% silane coupling agent by mass.
[0141] The second part is composed of 100% polydimethylsiloxane and 0% silicone oil by mass.
[0142] The third part is composed of 100% polydimethylsiloxane by mass.
[0143] A single-layer planar transfer stamp was obtained by spin coating, and then the single-layer planar transfer stamp was heat-treated on a hot plate at a temperature of 100° C. for 5 min.
[0144] Subsequently, the second mixed solution was coated on the surface of the single-layer planar transfer stamp by spin coating to obtain a double-layer planar transfer stamp, and then the double-layer planar transfer stamp was heat-treated on a hot plate at a temperature of 100° C. for 5 minutes.
[0145] Subsequently, the third mixed solution was coated on the surface of the double-layer planar transfer stamp by spin coating to obtain a multi-layer planar transfer stamp, and then the multi-layer planar transfer stamp was heat-treated at 200° C. for 10 min using a hot plate.
[0146] The total thickness of the multi-layer planar transfer stamp is 50 μm, the deformation is 5 μm, and the adhesion is 0.5 MPa.
[0147] The planar transfer stamp with a multi-layer composite structure prepared in the above steps can receive and transfer the LED chip array. However, during the transfer and bonding process of the LED chip array, the chip and the target substrate 4 are not parallel, resulting in the inability to transfer and bond all of the LED chip array to the target substrate 4. Figure 2 shown.
[0148] Comparative Example 3
[0149] The substrate 1 is made of ordinary glass, and the surface of the substrate 1 is treated with Piranha washing liquid.
[0150] Three mixed solutions were prepared, the first of which was a combination of various polymers with a polyimide mass ratio of 0%, a polydimethylsiloxane mass ratio of 40%, a silicone rubber mass ratio of 60%, an epoxy resin mass ratio of 0%, and a silane coupling agent mass ratio of 0%.
[0151] The second part is composed of a combination of various polymers with a polyimide mass ratio of 0%, a polydimethylsiloxane mass ratio of 40%, a silicone rubber mass ratio of 60%, an epoxy resin mass ratio of 0%, and a silicone oil mass ratio of 0%.
[0152] The third part is composed of a combination of various polymers with a polyimide mass ratio of 0%, a polydimethylsiloxane mass ratio of 50%, a silicone rubber mass ratio of 50%, and an epoxy resin mass ratio of 0%.
[0153] The first mixed solution was coated on the surface of a glass substrate by spraying to obtain a single-layer plane transfer stamp, and then the single-layer plane transfer stamp was heat-treated at a temperature of 100° C. and a treatment time of 10 minutes by a hot plate.
[0154] Subsequently, the second mixed solution was coated on the surface of the single-layer planar transfer stamp by spraying to obtain a double-layer planar transfer stamp, and then the double-layer planar transfer stamp was heat-treated at 100° C. for 5 minutes using a hot plate.
[0155] Subsequently, the third mixed solution was coated on the surface of the double-layer planar transfer stamp by spraying to obtain a multi-layer planar transfer stamp, and then the multi-layer planar transfer stamp was heat-treated with a hot plate at a temperature of 150° C. for 20 minutes.
[0156] The total thickness of the prepared multi-layer planar transfer stamp is 1000 μm, the deformation is 500 μm, and the adhesion is 3.0 MPa.
[0157] The planar transfer stamp with a multi-layer composite structure prepared in the above steps is applied to actual bonding. The stamp can be adhered with an LED chip array. There are indium bumps on the target substrate 4. The stamp and the target substrate 4 are aligned and hot-pressed. The LED chip cannot be bonded to the target substrate 4 due to excessive adhesion, and the edge area of the stamp is prone to edge formation during use. Figure 1 shown.
[0158] Table 1 shows the test results of some embodiments and comparative examples of the present invention.
[0159] Table 1 Test results of some embodiments of the present invention and comparative examples
[0160]
[0161] It can be seen from Table 1 that the embodiments of the present invention can achieve smooth bonding of LED chips.
[0162] In Comparative Examples 1 to 3, the deformation layer 6 is made of epoxy resin without adding silicone oil, resulting in that the planar transfer stamp has no deformation ability and cannot adapt to the problem that the planar transfer stamp is not parallel to the target substrate 4 .
[0163] In Comparative Examples 1 to 3, no silane coupling agent was added to the adhesive layer 5. The adhesive layer 5 could not be stably connected to the substrate 1 and was easily detached. In particular, in Comparative Example 3, the adhesive layer 5 had a serious edge phenomenon.
[0164] In Comparative Example 3, the materials of the adsorption layer 7 are composed of polydimethylsiloxane: silicone rubber at a weight ratio of 1:1, resulting in excessive adhesion, and the chip 3 cannot be successfully retained on the target substrate 4 .
[0165] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure made using the contents of the present invention's specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A planar transfer stamp with a multi-layer composite structure, comprising a substrate (1) and an adsorption layer (7) arranged on the substrate (1), wherein the adsorption layer (7) can adsorb an LED chip, and is characterized in that: A deformation layer (6) is provided between the substrate (1) and the adsorption layer (7), and the deformation layer (6) can deform when subjected to force; an adhesion layer (5) is also provided between the substrate (1) and the deformation layer (6), and the adhesion layer (5) can adhere to the substrate (1) and the deformation layer (6); The deformation layer (6) is composed of silicone oil and polymer material A, wherein the polymer material A is composed of one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin; the mass fraction of the silicone oil is 5% to 30%; The adsorption layer (7) is composed of a polymer material B, wherein the polymer material B is composed of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, wherein the mass fraction of polyimide is 10% to 40%, the mass fraction of polydimethylsiloxane is 10% to 40%, the mass fraction of silicone rubber is 20% to 40%, and the mass fraction of epoxy resin is 10% to 40%, wherein the weight ratio of polydimethylsiloxane to silicone rubber is ≠1:1; The adhesion layer (5) is composed of a silane coupling agent and a polymer material C, wherein the polymer material C is composed of one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, and the mass fraction of the silane coupling agent is 5% to 30%; the substrate (1) is composed of one or more of glass, silicon wafer and sapphire; before the adhesion layer (5) is formed on the surface of the substrate (1), the surface of the substrate (1) is treated with oxygen plasma or Piranha lotion.
2. The planar transfer stamp with a multi-layer composite structure according to claim 1, characterized in that: The viscoelasticity of the silicone oil is 5.0×10 2 ~6.0×10 5 mPa.s.
3. The planar transfer stamp with a multi-layer composite structure according to claim 1 or 2, characterized in that: When the polymer material A is composed of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, the mass fraction of polyimide is 10%-40%, the mass fraction of polydimethylsiloxane is 10%-40%, the mass fraction of silicone rubber is 15%-40%, and the mass fraction of epoxy resin is 10%-40%.
4. The planar transfer stamp with a multi-layer composite structure according to claim 1, characterized in that: The viscoelasticity of the adsorption layer (7) may change when heated.
5. The planar transfer stamp with a multi-layer composite structure according to claim 1, characterized in that: The material components of the adhesion layer (5), the deformation layer (6) and the adsorption layer (7) contain at least one identical polymer material.
6. The planar transfer stamp with a multi-layer composite structure according to claim 5, characterized in that: When the polymer material C is composed of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin, the mass fraction of polyimide is 10%-40%, the mass fraction of polydimethylsiloxane is 10%-40%, the mass fraction of silicone rubber is 15%-40%, and the mass fraction of epoxy resin is 10%-40%.
7. A method for preparing a planar transfer stamp with a multi-layer composite structure, used for preparing a planar transfer stamp with a multi-layer composite structure as claimed in claim 1, characterized in that: The following steps are involved: The surface of the substrate (1) is treated with oxygen plasma or Piranha solution; A material composed of a silane coupling agent and a polymer material C is coated on the surface of the substrate (1) to form a single-layer planar stamp; the polymer material C is one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin; Performing a heating and curing treatment on the single-layer plane seal; Applying a material composed of silicone oil and polymer material A to the coating side of the single-layer plane stamp to form a double-layer plane stamp; the polymer material A is one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin; Performing a heating and curing process on the double-layer plane seal; Applying polymer material B to the coating-containing side of the single-layer planar stamp to form a multi-layer planar stamp; the polymer material B is one or more of polyimide, polydimethylsiloxane, silicone rubber and epoxy resin; The multi-layer planar stamp is subjected to a heating and curing treatment.