System and method for preparing high-activity SCM material from low-carbon raw material

Through the low-pressure suspended carbonization bed system and optimized carbonization process, the problems of a large proportion of calcium carbonate and insufficient activity of low-calcium low-carbon cement in cement production are solved, and the preparation of highly active SCM materials and flue gas CO2 capture are achieved, which is suitable for Industrial large-scale continuous production reduces carbon emissions.

CN118846969AActive Publication Date: 2024-10-29TIANJIN CEMENT IND DESIGN & RES INST CO LTD

Patent Information

Application Number
CN202410882294.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-29
Estimated Expiration
2044-07-03

AI Technical Summary

Technical Problem

Calcium carbonate accounts for a large proportion in the existing cement production process, resulting in a large amount of carbon emissions; low-calcium low-carbon cement has insufficient activity and limited application scope; the pressurized carbonization method is difficult to meet the needs of industrial-scale continuous production; the carbonization reaction residence time is short, and the reaction Insufficient, the material activity is low, and it is difficult to fully capture flue gas CO2.

Method used

A low-pressure suspended carbonization bed system is used, combined with a cement burning system and a clinker grinding system. The gas-solid fluidized mixing and water spray system in the suspended carbonization bed form a liquid film to increase the carbonization reaction rate, and through secondary temperature control The mixing chamber and powder selection and separation device optimize the carbonization process and achieve the preparation of highly active SCM materials.

Benefits of technology

It achieves the reduction of raw material carbonate consumption and flue gas CO2 capture, improves the activity and carbonization rate of SCM materials, is suitable for industrial-scale continuous production, and reduces carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118846969A_ABST
    Figure CN118846969A_ABST
Patent Text Reader

Abstract

The invention discloses a system and a method for preparing a high-activity SCM material from a low-carbon raw material. The system comprises a cement sintering system, a clinker grinding system, a low-pressure suspension carbonization bed system, a bag dust collector and an induced draft fan, a material outlet of the grate cooler is connected with a material inlet of the clinker grinding system, a flue gas outlet of the kiln tail preheating and predecomposition system is connected with a flue gas inlet of the clinker grinding system, a flue gas outlet of the kiln tail preheating and predecomposition system is connected with a flue gas inlet of the low-pressure suspension carbonization bed system through a dust remover, and a material inlet is formed in the low-pressure suspension carbonization bed system. The clean flue gas and the aqueous solution are sprayed into the suspension carbonization bed, a liquid film is formed on the surface of the material, CO2 in the clean flue gas is dissolved into the liquid film to be subjected to carbonization reaction with the material, powder collected by the bag dust collector can return to a low-pressure suspension carbonization bed system to be circularly carbonized, and a high-activity SCM material can also be directly obtained. According to the invention, the carbon emission is reduced, the carbonization rate is increased, and the activity of the prepared SCM material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon emission reduction, and in particular to a system and method for preparing high-activity SCM materials from low-carbon raw materials. Background Art

[0002] Cement production consumes a large amount of natural resources and emits a large amount of carbon dioxide. The cement industry is the third largest source of carbon dioxide emissions in my country, accounting for about 13% of the country's total industrial carbon emissions. In 2022, my country's cement production reached 2.118 billion tons, and carbon dioxide emissions were about 1.3 billion tons. Therefore, carbon emission reduction in the domestic cement industry is related to the realization of the strategic goals of carbon peak and carbon neutrality. To this end, academia and industry have proposed and adopted various energy-saving and emission reduction strategies, such as reducing the amount of cement in concrete, reducing the clinker coefficient in cement, reducing carbon emissions in the production process of cement clinker, using new biomass fuels, and carbon capture, utilization and storage.

[0003] The existing general-purpose cement is mainly ordinary Portland cement, whose main mineral composition is C3S, C2S, C3A, C4AF, etc., and is made into a cementitious material by adding water and stirring to produce a hydration reaction. The raw material of ordinary Portland cement is mainly limestone. The production of 1 ton of ordinary Portland cement clinker consumes about 1.2 tons of limestone and produces about 500kg CO2 emissions, accounting for about 60% of the total carbon emissions in the cement production process. In order to reduce carbon emissions from cement production, the development of new carbonizable low-calcium and low-carbon cement varieties is an important way. On the one hand, it reduces the raw material consumption of calcium carbonate, and on the other hand, it can capture some CO2 during the cement carbonization process. However, since carbonizable low-carbon cement is mainly used in the concrete products industry, this seriously restricts the promotion and application of this technology. Therefore, if the new carbonizable low-carbon clinker is prepared into a highly active auxiliary cementitious material and used in cement and concrete, so that the prepared cement and concrete become carbon-negative cement and concrete, then the application scope of the new carbonizable low-carbon cement is solved, which will also become one of the effective ways to reduce carbon emissions in the cement industry.

[0004] At present, most of the reports on carbonizable low-calcium and low-carbon cement are still in the laboratory research stage. In the Low-CO2 synthetic SCMs published by Solida Technology in the International Cement Review magazine, it is mentioned that low-carbon clinker mainly composed of carbonizable minerals is used to pass industrial tail gas containing carbon dioxide in a slurry or semi-wet state to prepare SCM materials. The low-carbon clinker used is mainly CS and C3S2. These two minerals basically do not react with water for hydration, but can react with carbon dioxide to form calcite and amorphous silica. Solida's literature mentioned that the SCM it prepared contains a large amount of calcite products. However, the GB175-2021 "General Portland Cement" standard has clear requirements for cement loss on ignition. If the SCM content is 30%, sufficient carbonization can form about 15% calcite. Since PⅡ type silicate cement requires limestone content ≤5%, silicate cement (PI and PⅡ) requires loss on ignition less than 3.0% and 3.5% respectively, and ordinary silicate cement requires PO loss on ignition ≤5.0%, and the GB / T1596-2017 "Fly ash in cement and concrete" standard requires loss on ignition as an admixture to be ≤8.0%, which seriously limits the dosage range of SCM materials prepared after full carbonization.

[0005] Low-carbon cement has broad application prospects in the field of carbon emission reduction. There are no reports on the industrial-grade carbonization method and carbonization system of low-carbon cement. At present, relatively more research is on the carbonization of steel slag. Chinese Patent Publication No. CN113072311A discloses a steel slag auxiliary cementitious material and its preparation method and application. It mentions the use of industrial tail gas to carbonize steel slag powder, and the introduction of industrial tail gas containing a carbon dioxide concentration of 20% during the grinding process. However, due to the limited volume of the grinding equipment, the residence time of the flue gas in the mill is short. It is difficult to fully carbonize the steel slag by only carbonization reaction inside the mill, and the carbonization process is uncontrollable. Chinese Patent Publication No. CN214571715U discloses a tailings soil test block carbonization steel slag heating and pressurization device, which significantly improves the carbonization rate by controlling the temperature and carbon dioxide gas pressure, greatly accelerates the reaction process, and improves the comprehensive utilization of steel slag and carbon dioxide. However, since the pressurization system is limited by the volume of the pressure vessel and the feeding method, this pressurized carbonization method is difficult to scale up and produce continuously in industry.

[0006] In summary, the problems existing in the prior art are:

[0007] (1) Calcium carbonate accounts for a large proportion of the commonly used cement raw materials, and the production process generates a large amount of carbon emissions.

[0008] (2) Low-calcium low-carbon cement can reduce the carbonate ratio and reduce carbon emissions, but if it is not carbonized to increase its activity, its application range will be relatively narrow.

[0009] (3) The existing pressurized carbonization method is difficult to meet the needs of large-scale production operations and continuous operation of the production process.

[0010] (4) The existing in-mill carbonization method has a short reaction residence time, incomplete carbonization reaction, uncontrollable carbonization process, low activity of the carbonized material, and cannot fully capture flue gas CO2.

[0011] Therefore, under the global carbon emission reduction situation, it is urgent to develop a new process method suitable for industrial-scale continuous production, with low raw material carbon emissions, high carbonization rate, and high activity of SCM materials after carbonization. Summary of the invention

[0012] In order to solve the problems existing in the prior art, the present invention provides a system and method for preparing high-activity SCM materials from low-carbon raw materials, which reduces the consumption of raw material carbonate and captures flue gas CO2, thereby reducing carbon emissions.

[0013] The present invention is achieved by a system for preparing high-activity SCM materials from low-carbon raw materials, comprising a cement burning system, a clinker grinding system, a low-pressure suspended carbonization bed system, a bag dust collector and an induced draft fan;

[0014] The cement burning system comprises a kiln tail preheating and precalcining system, a rotary kiln and a grate cooler which are connected in sequence; the material outlet of the grate cooler is connected to the material inlet of the clinker grinding system, the kiln tail flue gas outlet of the kiln tail preheating and precalcining system is connected to the flue gas inlet of the clinker grinding system, and the powdered material outlet of the clinker grinding system is connected to the material inlet of the low-pressure suspended carbonized bed system;

[0015] The low-pressure suspended carbonization bed system comprises an air duct, a suspended carbonization bed and a water spray system. The air duct is located below the suspended carbonization bed, and the bottom of the air duct is a flue gas inlet. The kiln tail flue gas outlet of the kiln tail preheating and predecomposition system is connected to the flue gas inlet of the air duct through a dust collector. The material inlet of the low-pressure suspended carbonization bed system is arranged on the air duct or the suspended carbonization bed, so that the powdered material moves upward under the drive of the flue gas. The top of the air duct is connected to the bottom of the suspended carbonization bed, and a spray pipe is arranged at the connection part, so that the clean flue gas after the kiln tail preheating and predecomposition system and dust removal is sprayed upward into the suspended carbonization bed; a plurality of spray guns are arranged at the lower part of the suspended carbonization bed and are located above the spray pipe, and the outlet of the water spray system is connected to the inlet of the spray gun, so that the aqueous solution is sprayed into the suspended carbonization bed in the form of droplets, and the water vapor in the flue gas in the suspended carbonization bed forms a critical saturation state of water vapor-water droplets, and a liquid film is formed on the surface of the material;

[0016] The outlet of the suspended carbonization bed is connected to the flue gas inlet of the bag dust collector; the material outlet of the bag dust collector is connected to the high-activity SCM material finished product, or is respectively connected to the high-activity SCM material finished product and the material inlet of the low-pressure suspended carbonization bed system, and the flue gas outlet of the bag dust collector is connected to the induced draft fan inlet.

[0017] In the above technical solution, preferably, the suspended carbonized bed comprises a sparging pipe, a carbonized bed cone and a carbonized bed column connected in sequence from bottom to top; the sparging pipe is a vertical pipe, and a guide device for evenly distributing the smoke is arranged inside the sparging pipe. The guide device is a guide plate, a grille or a guide ring.

[0018] In the above technical solution, it is further preferred that an ultrasonic generator is provided at the vertebral body of the carbonization bed.

[0019] In the above technical scheme, preferably, a secondary temperature-controlled mixing chamber is arranged between the suspended carbonization bed and the bag dust collector, and the secondary temperature-controlled mixing chamber is used to increase the temperature of the flue gas exiting the suspended carbonization bed and reduce the humidity of the flue gas; the secondary temperature-controlled mixing chamber has inlet one, inlet two and an outlet, the top outlet of the suspended carbonization bed is connected to inlet one of the secondary temperature-controlled mixing chamber, the kiln tail flue gas outlet of the kiln tail preheating and predecomposition system is connected to inlet two of the secondary temperature-controlled mixing chamber through a dust collector, and the outlet of the secondary temperature-controlled mixing chamber is connected to the flue gas inlet of the bag dust collector.

[0020] In the above technical solution, it is further preferred that a temperature measuring device is provided on the outlet pipe of the secondary temperature-controlled mixing chamber.

[0021] In the above technical scheme, it is further preferred that a powder selection and separation device is arranged between the secondary temperature-controlled mixing chamber and the bag dust collector, the outlet of the secondary temperature-controlled mixing chamber is connected to the flue gas inlet of the powder selection and separation device, the bottom material outlet of the powder selection and separation device is connected to the material inlet of the low-pressure suspended carbonization bed system, and the top flue gas outlet of the powder selection and separation device is connected to the flue gas inlet of the bag dust collector.

[0022] In the above technical solution, it is further preferred that the powder selection and separation device is a powder selector or a cyclone, which is used to separate coarse powder and fine powder in the material.

[0023] In the above technical solution, it is further preferred that an air lock valve and a material dividing valve are sequentially arranged on the material pipe of the bottom material outlet of the powder selection and separation device, and the bottom material outlet of the powder selection and separation device is also connected to the high-activity SCM material finished product through the material dividing valve, so that the coarse powder exiting the powder selection and separation device can enter the suspended carbonization bed and the high-activity SCM material finished product respectively.

[0024] In the above technical solution, preferably, a vertically placed filter bag is provided in the bag dust collector, and a compressed air blowing device for regularly cleaning powder cakes on the surface of the filter bag is also provided in the bag dust collector.

[0025] A method for preparing a high-activity SCM material from a low-carbon raw material comprises the following steps:

[0026] S1. Raw material batching and clinker burning

[0027] The silicon raw material, calcium raw material, gypsum and mineralizer are ground into raw materials in a certain proportion, and then the raw materials are preheated and decomposed by the preheating and predecomposition system at the kiln tail and sent to the rotary kiln for calcination. The calcination temperature in the rotary kiln is 1100-1300℃. The calcined clinker is sent to the grate cooler for cooling to obtain low-carbon cement clinker.

[0028] S2. Clinker grinding

[0029] The low-carbon cement clinker particles are transported to the clinker grinding system, and the tail gas from the kiln preheating and predecomposition system is introduced into the clinker grinding system. The tail gas from the kiln preheating and predecomposition system contains 25% to 35% CO2 in concentration, which is ground into low-carbon cement clinker powder. The average particle size of the low-carbon cement clinker powder is less than 200μm.

[0030] S3. Carbonization to prepare highly active SCM materials

[0031] Suspension Carbonization:

[0032] The clean flue gas after the preheating and pre-decomposition system at the kiln tail and the dust removal is introduced into the flue gas inlet of the air duct. The clean flue gas after the preheating and pre-decomposition system at the kiln tail and the dust removal has a temperature of 100-150°C and a CO2 concentration of 25%-35%; the clean flue gas moves upward and is sprayed into the suspended carbonization bed through the spray pipe; at the same time, the low-carbon cement clinker powder with a temperature of ≤60°C and an average particle size of less than 200μm is dispersed and fed into the air duct or the suspended carbonization bed, so that the material is suspended in the clean flue gas under the drag of the air flow; the pressure in the suspended carbonization bed is 0-3000Pa, and the average wind speed in the cross section of the suspended carbonization bed is 3-10m / s; at the same time, water or carbonization aid aqueous solution is sprayed into the suspended carbonization bed in the form of droplets through a spray gun, so that the water vapor in the flue gas forms a critical saturation state; the water vapor forms a liquid film on the surface of the material, and the CO2 in the flue gas dissolves in the liquid film to react with the material to carbonize;

[0033] Coarse powder circulation and finished product collection:

[0034] The flue gas from the suspended carbonization bed carries the material and enters the bag dust collector under the draft of the induced draft fan. After the material is collected, part of it returns to the low-pressure suspended carbonization bed system for cyclic carbonization, and part of it is led to the high-activity SCM material finished product; or, all of it is led to the high-activity SCM material finished product.

[0035] In the above technical scheme, preferably, the content of SiO2 in the siliceous raw material is ≥50%, the content of CaO in the calcareous raw material is ≥35%, the gypsum is one of desulfurized gypsum, phosphogypsum, and natural gypsum, and the mineralizer is one of fluorite, calcium fluoride, borax, and boric acid, or a combination of any two of them.

[0036] In the above technical scheme, preferably, the mineral composition of the low carbon cement clinker includes: α′-C2S, C4A3$, C5S2$, CS, β-C2S, wherein the sum of the contents of α′-C2S and β-C2S accounts for more than 40% of the total mass of the low carbon cement clinker, the sum of the contents of C4A3$ and C5S2$ accounts for more than 20% of the total mass of the low carbon cement clinker, the content of CS accounts for more than 20% of the total mass of the low carbon cement clinker, and the rest is glass phase.

[0037] In the above technical solution, preferably, during the suspended carbonization process, ultrasonic vibration is added to the bottom of the suspended carbonization bed.

[0038] In the above technical solution, preferably, in the carbonization aid aqueous solution, the carbonization aid is one or a combination of any two of lignin sulfonates, polycyclic aromatic salts, water-soluble resin sulfonates, and alcohol-ammonia organic substances.

[0039] In the above technical scheme, preferably, the flue gas carrying materials out of the suspended carbonization bed first enters the secondary temperature-controlled mixing chamber and is mixed with part of the clean flue gas out of the kiln tail preheating and predecomposition system and after dust removal, and then enters the powder selection and separation device; the flue gas temperature out of the secondary temperature-controlled mixing chamber is controlled at 70-100°C.

[0040] In the above technical scheme, it is further preferred that the flue gas carrying the material out of the secondary temperature-controlled mixing chamber first enters the powder selection and separation device, and the coarse powder in the material is collected and discharged from the bottom of the powder selection and separation device, part of which is returned to the low-pressure suspended carbonization bed system for cyclic carbonization, and part of which is led to the high-activity SCM material finished product; the fine powder is discharged from the top of the powder selection and separation device with the flue gas and enters the bag dust collector, and the flue gas passes through the filter bag with a filtration wind speed of 0.5 to 1.5 m / min, so that the fine powder forms a powder cake on the surface of the filter bag, and the CO2 in the flue gas continues to carbonize with the material during the process of passing through the powder cake, and the compressed air is regularly purged to clean the powder cake. The powder collected from the bag dust collector is a carbonized micropowder material, which is led to the high-activity SCM material finished product.

[0041] The advantages and positive effects of the present invention are:

[0042] (1) The present invention sets up a low-pressure suspended carbonization bed system, realizes gas-solid fluidized mixing in the suspended carbonization bed, and improves the carbonization reaction rate. The low-pressure working environment in the suspended carbonization bed creates conditions for continuous production. The carbonization aid aqueous solution is sprayed into the suspended carbonization bed and then dispersed and attached to the particle surface in the form of droplets to form a liquid film. The liquid film serves as a gas-solid mass transfer bridge for the carbonization reaction, which can accelerate the carbonization rate. At the same time, water or a carbonization aid aqueous solution with a crystal form control agent is sprayed into the suspended carbonization bed, which promotes the full coverage of the particle surface by water or the crystal form control agent, reduces the formation of calcite, increases amorphous calcium carbonate, and improves the activity of the SCM material.

[0043] (2) The present invention solves the problem of condensation in the flue gas exiting the suspended carbonization bed caused by water spraying or carbonization aid aqueous solution during the carbonization process, by introducing a preheating and predecomposition system at the kiln tail of the cement burning system and performing secondary temperature control on the flue gas at the kiln tail after dust removal, thereby increasing the amount of water sprayed in the suspended carbonization bed, which is beneficial to further carbonization; and the introduction of a preheating and predecomposition system at the kiln tail of the cement burning system and performing secondary temperature control on the flue gas at the kiln tail after dust removal increases the CO2 concentration, which is beneficial to carbonization along the subsequent pipeline and bag dust collector; and when the bag dust collector collects dust, the fine powder adheres to the surface of the filter bag, and the fine powder can continue to be carbonized during the process of CO2 gas penetrating the filter bag.

[0044] (3) A portion of the kiln tail flue gas discharged from the cement burning system of the present invention directly enters the clinker grinding system, and the other portion of the kiln tail flue gas is divided into two streams after dust removal, one of which is sprayed into the low-pressure suspended carbonization bed system, and the other enters the secondary temperature-controlled mixing chamber, so that the CO2 in the kiln tail flue gas can be fully captured, thereby reducing the carbon emission of the burning system.

[0045] (4) An ultrasonic generator is provided at the bottom of the suspended carbonization bed of the present invention to reduce particle agglomeration through high-frequency acoustic vibration, which is beneficial to a series of subsequent operations.

[0046] (5) The present invention returns the coarse powder to the low-pressure suspended carbonization bed system through the powder selection and separation process, thereby avoiding the problems of small specific surface area and low carbonization degree of the coarse powder, realizing cyclic carbonization, and cyclic carbonization improves the carbonization rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 Schematic diagram of a system for preparing highly active SCM materials from low-carbon raw materials provided in Example 1 of the present invention;

[0048] Figure 2 is a process flow chart for preparing high-activity SCM materials from low-carbon raw materials provided in Example 1 of the present invention;

[0049] Figure 3 It is a schematic diagram of the position relationship of the three phases of low carbon cement clinker, liquid film and flue gas in the suspended carbonization bed of the present invention;

[0050] Figure 4 Schematic diagram of a system for preparing highly active SCM materials from low-carbon raw materials provided in Example 2 of the present invention;

[0051] Figure 5 This is a process flow chart for preparing high-activity SCM materials from low-carbon raw materials provided in Example 2 of the present invention.

[0052] In the figure: Q1-clean flue gas from the air inlet; Q2-low CO2 flue gas; Q3-clean flue gas from the secondary temperature control mixing chamber; Q4-kiln tail flue gas from the clinker grinding system; M1-low carbon cement clinker powder; M2-first-stage finished product; M3-recycled material from the bag dust collector; M4-recycled material from the powder separation device; M5-second-stage finished product; M6-finished product after confluence; R1-raw material from the preheater; K-low carbon cement clinker particles; F-fuel; A-material particles; B-liquid film; C-flue gas;

[0053] 1- cement burning system; 101- preheater; 102- decomposition furnace; 103- rotary kiln; 104- grate cooler; 105- burner; 106- high temperature fan; 107- dust collector; 108- exhaust fan;

[0054] 2-Clinker grinding system;

[0055] 3- low-pressure suspended carbonization bed system; 301- spray pipe; 302- carbonization bed cone; 303- carbonization bed column; 304- ultrasonic generator; 305- water spray system; 306- spray gun; 307- air duct;

[0056] 4-bag dust collector; 401-filter bag;

[0057] 5- induced draft fan;

[0058] 6-secondary temperature control mixing chamber; 601-temperature measuring device;

[0059] 7-powder selection and separation device; 701-air lock valve; 702-material distribution valve;

[0060] The dashed line with arrow is the air flow direction; the solid line with arrow is the material flow direction. DETAILED DESCRIPTION

[0061] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0062] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "upper", "lower", "front", "back", "left", "right", "inside", "outside", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0063] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0064] Example 1

[0065] See also Figure 1 and Figure 2 An embodiment of the present invention provides a system for preparing high-activity SCM materials from low-carbon raw materials, including a cement burning system 1, a clinker grinding system 2, a low-pressure suspended carbonization bed system 3, a bag dust collector 4 and an induced draft fan 5.

[0066] The cement burning system 1 includes a kiln tail preheating and predecomposition system, a rotary kiln 103 and a grate cooler 104 connected in sequence, the kiln tail preheating and predecomposition system includes a preheater 101 and a decomposition furnace 102; the material outlet of the grate cooler 104 is connected to the material inlet of the clinker grinding system 2, the kiln tail flue gas outlet of the kiln tail preheating and predecomposition system is connected to the flue gas inlet of the clinker grinding system 2, and the powdered material outlet of the clinker grinding system 2 is connected to the material inlet of the low-pressure suspended carbonized bed system 3.

[0067] The low-pressure suspended carbonization bed system 3 includes an air duct 307, a suspended carbonization bed and a water spraying system 305. The air duct 307 is located below the suspended carbonization bed, and the bottom of the air duct 307 is a flue gas inlet. The kiln tail flue gas outlet of the kiln tail preheating and predecomposition system is connected to the flue gas inlet of the air duct 307 through a dust collector 107. The material inlet of the low-pressure suspended carbonization bed system 3 is arranged on the air duct 307 or the suspended carbonization bed. In this embodiment, a material inlet is arranged on the air duct 307, so that the low-carbon cement clinker powder M1 moves upward driven by the flue gas; the top of the air duct 307 is connected to the bottom of the suspended carbonization bed, and a spraying pipe 301 is arranged at the connection position, so that the clean flue gas exiting the kiln tail preheating and predecomposition system and after dust removal is sprayed upward into the suspended carbonization bed.

[0068] A plurality of spray guns 306 are arranged at the lower part of the suspended carbonized bed and are located above the spray pipe 301. The outlet of the water spray system 305 is connected to the inlet of the spray gun 306, so that the aqueous solution is sprayed into the suspended carbonized bed in the form of droplets. The water vapor in the flue gas in the suspended carbonized bed forms a critical saturation state of water vapor-water droplets, and a liquid film B is formed on the surface of the material particles A. Figure 3 shown.

[0069] The outlet of the suspended carbonization bed is connected to the flue gas inlet of the bag dust collector 4; the material outlet of the bag dust collector 4 is divided into two paths, one of which is connected to the finished product of the high-activity SCM material, and the other is connected to the air duct 307 or the material inlet of the suspended carbonization bed, and the collected materials are continuously returned to the air duct 307 or the suspended carbonization bed. In this embodiment, the material outlet of the bag dust collector 4 is connected to the material inlet of the air duct 307, and part of the materials collected by the bag dust collector are continuously returned to the air duct 307 for cyclic carbonization; the flue gas outlet of the bag dust collector 4 is connected to the inlet of the induced draft fan 5 to discharge the low CO2 flue gas.

[0070] As a preferred embodiment, the suspended carbonization bed includes a spray pipe 301, a carbonization bed cone 302 and a carbonization bed column 303 connected in sequence from bottom to top; the spray pipe 301 is a vertical pipe, and a guide device for evenly distributing the flue gas is arranged inside the spray pipe 301, and the guide device is a structure such as a guide plate, a grille or a guide ring.

[0071] The bag dust collector 4 is provided with a vertically placed filter bag 401 and a compressed air blowing device for regularly cleaning the powder cake on the surface of the filter bag. The flue gas passes through the filter bag 401, so that the fine powder forms a powder cake on the surface of the filter bag 401. The CO2 in the flue gas continues to carbonize with the material during the process of passing through the powder cake, and the compressed air is blown regularly to clean the powder cake.

[0072] The method for preparing high-activity SCM materials from low-carbon raw materials comprises the following steps:

[0073] S1. Raw material batching and clinker burning

[0074] The siliceous raw material, the calcareous raw material, the gypsum and the mineralizer are ground into raw materials in a certain proportion, wherein the content of SiO2 in the siliceous raw material is ≥50%, the content of CaO in the calcareous raw material is ≥35%, the gypsum is one of desulfurized gypsum, phosphogypsum and natural gypsum, and the mineralizer is one of fluorite, calcium fluoride, borax and boric acid or a combination of any two thereof.

[0075] The raw material is then preheated and decomposed in the preheater 101 and the calciner 102 at the end of the kiln and then sent to the rotary kiln 103 for calcination. The calcination temperature in the rotary kiln is 1100-1300°C and the calcination time is 30-60 minutes. The calcined clinker is in granular form and sent to the grate cooler 104 for cooling to obtain low-carbon cement clinker. The mineral composition of low-carbon cement clinker is: including α′-C2S, C4A3$, C5S2$, CS, and β-C2S, wherein the sum of the contents of α′-C2S and β-C2S accounts for more than 40% of the total mass of low-carbon cement clinker, the sum of the contents of C4A3$ and C5S2$ accounts for more than 20% of the total mass of low-carbon cement clinker, the content of CS accounts for more than 20% of the total mass of low-carbon cement clinker, and the rest is glass phase.

[0076] S2. Clinker grinding

[0077] The low-carbon cement clinker particles K are transported to the clinker grinding system 2, and the flue gas from the kiln tail preheating and pre-decomposition system is led to the clinker grinding system 2. The flue gas Q4 entering the clinker grinding system contains 25% to 35% CO2, which is ground into low-carbon cement clinker powder M1. The average particle size of the low-carbon cement clinker powder is less than 80μm, and the particle size distribution is 5 to 80μm. The proportion of particles is greater than 90%. During the grinding process, part of the low-carbon cement clinker reacts with the CO2 in the flue gas from the kiln tail preheating and pre-decomposition system to reduce the CO2 concentration in the flue gas.

[0078] S3. Carbonization to prepare highly active SCM materials

[0079] Suspension Carbonization:

[0080] The clean flue gas after preheating and pre-decomposition system at the kiln tail and dust removal is introduced into the flue gas inlet of the air duct. The temperature of the clean flue gas Q1 entering the air duct is 100-150°C and the CO2 concentration is 25%-35%. At the same time, the low-carbon cement clinker powder M1 with a temperature of ≤60°C and an average particle size of less than 80μm is dispersed and fed into the air duct 307 through a spreading device, so that the material is suspended in the clean flue gas under the drag of the air flow. The clean flue gas carries the low-carbon cement clinker powder M1 upward and is sprayed into the suspended carbonization bed through the spraying pipe 301. The suspended carbonization bed The pressure is 0~-3000Pa, and the average wind speed in the cross section of the suspended carbonization bed is 3~10m / s; at the same time, water or carbonization aid aqueous solution is sprayed into the suspended carbonization bed in the form of droplets through the spray gun 306, so that the water vapor in the flue gas forms a critical saturation state (relative humidity ≥90%); since the surface temperature of the material is lower than the dew point temperature of the water vapor, the water vapor condenses on the surface of the material to form a liquid film, and the liquid film provides a transmission medium in the gas-solid carbonization reaction, and the CO2 in the flue gas dissolves in the liquid film to react with the material to carbonize, thereby accelerating the carbonization process.

[0081] In the carbonization aid aqueous solution, the carbonization aid is one of lignin sulfonates, polycyclic aromatic salts, water-soluble resin sulfonates, and alcohol-ammonia organic substances, or a combination of any two of them.

[0082] Coarse powder circulation and finished product collection:

[0083] The flue gas out of the suspended carbonization bed carries the material and enters the bag dust collector 4 under the exhaust of the induced draft fan 5. After the material is collected, part of the material is returned to the air duct 307 of the low-pressure suspended carbonization bed system 3 as the circulating material M3 out of the bag dust collector for circulating carbonization, and part of the material is led to the high-activity SCM material finished product as the first-level finished product M2. The flue gas discharged from the bag dust collector 4 is low-CO2 flue gas Q2.

[0084] Example 2

[0085] See also Figure 3 and Figure 4 An embodiment of the present invention provides a system for preparing high-activity SCM materials from low-carbon raw materials, including a cement burning system 1, a clinker grinding system 2, a low-pressure suspended carbonization bed system 3, a secondary temperature-controlled mixing chamber 6, a powder selection and separation device 7, a bag dust collector 4 and an induced draft fan 5.

[0086] The structures of the cement burning system 1, the clinker grinding system 2 and the low-pressure suspended carbonization bed system 3 are the same as those of Example 1. Different from Example 1, an ultrasonic generator 304 is further provided at the carbonization bed cone 302, and the ultrasonic generator 304 is located below the inlet of the spray gun 306.

[0087] The secondary temperature control mixing chamber 6 is located between the suspended carbonization bed and the powder selection and separation device 7. The secondary temperature control mixing chamber 6 is used to increase the temperature of the flue gas from the suspended carbonization bed and reduce the humidity of the flue gas. The secondary temperature control mixing chamber 6 has an inlet 1, an inlet 2 and an outlet. The top outlet of the suspended carbonization bed is connected to the inlet 1 of the secondary temperature control mixing chamber 6. The flue gas outlet of the kiln tail preheating and predecomposition system is connected to the inlet 2 of the secondary temperature control mixing chamber 6 through a dust collector 107. The outlet of the secondary temperature control mixing chamber 6 is connected to the flue gas inlet of the powder selection and separation device 7. A temperature measuring device 601 is provided on the outlet pipe of the secondary temperature control mixing chamber 6. The temperature measuring device 601 is a thermocouple.

[0088] The powder selection and separation device 7 is a powder selection machine or a cyclone, which is used to separate the coarse powder and fine powder in the material. The material pipe at the bottom material outlet of the powder selection and separation device 7 is provided with an air lock valve 701 and a material distribution valve 702 in sequence. The bottom material outlet of the powder selection and separation device 7 is connected to the material inlet of the air duct 307 and the high-activity SCM material finished product through the material distribution valve 702, so that the coarse powder out of the powder selection and separation device 7 can enter the suspended carbonization bed and the high-activity SCM material finished product respectively. The top flue gas outlet of the powder selection and separation device 7 is connected to the flue gas inlet of the bag dust collector 4. The bag dust collector 4 is provided with a vertically placed filter bag 401 and a compressed air purge device for regularly cleaning the powder cake on the surface of the filter bag 401. The material outlet of the bag dust collector 4 is connected to the high-activity SCM material finished product, and the flue gas outlet of the bag dust collector 4 is connected to the inlet of the induced draft fan 5.

[0089] The method for preparing high-activity SCM materials from low-carbon raw materials comprises the following steps:

[0090] S1. Raw material batching and clinker burning

[0091] The siliceous raw material, the calcareous raw material, the gypsum and the mineralizer are ground into raw materials in a certain proportion, wherein the content of SiO2 in the siliceous raw material is ≥50%, the content of CaO in the calcareous raw material is ≥35%, the gypsum is one of desulfurized gypsum, phosphogypsum and natural gypsum, and the mineralizer is one of fluorite, calcium fluoride, borax and boric acid or a combination of any two thereof.

[0092] The raw material is then preheated and decomposed in the preheater 101 and the calciner 102 at the end of the kiln and then sent to the rotary kiln 103 for calcination. The calcination temperature in the rotary kiln is 1100-1300°C and the calcination time is 30-60 minutes. The calcined clinker is in granular form and sent to the grate cooler 104 for cooling to obtain low-carbon cement clinker. The mineral composition of low-carbon cement clinker is: including α′-C2S, C4A3$, C5S2$, CS, and β-C2S, wherein the sum of the contents of α′-C2S and β-C2S accounts for more than 40% of the total mass of low-carbon cement clinker, the sum of the contents of C4A3$ and C5S2$ accounts for more than 20% of the total mass of low-carbon cement clinker, the content of CS accounts for more than 20% of the total mass of low-carbon cement clinker, and the rest is glass phase.

[0093] S2. Clinker grinding

[0094] The low-carbon cement clinker particles K are transported to the clinker grinding system 2, and the flue gas from the kiln tail preheating and predecomposition system is introduced to the clinker grinding system 2. The flue gas Q4 entering the clinker grinding system contains 25% to 35% CO2, which is ground into low-carbon cement clinker powder M1. The average particle size of the low-carbon cement clinker powder is less than 200μm, and the particle size distribution of 5 to 200μm accounts for more than 90%. During the grinding process, part of the low-carbon cement clinker reacts with the CO2 in the flue gas from the kiln tail preheating and predecomposition system to reduce the CO2 concentration in the flue gas.

[0095] S3. Carbonization to prepare highly active SCM materials

[0096] Suspension Carbonization:

[0097] The clean flue gas after the preheating and pre-decomposition system at the kiln tail and dust removal is introduced into the flue gas inlet of the air duct 307. The temperature of the clean flue gas Q1 entering the air duct is 100-150°C and the CO2 concentration is 25%-35%. At the same time, the low-carbon cement clinker powder M1 with a temperature of ≤60°C and an average particle size of less than 200μm is dispersed and fed into the air duct 307 through a spreading device, so that the material is suspended in the flue gas under the drag of the air flow, and the clean flue gas carries the material upward and is sprayed into the suspended carbonization bed through the spraying pipe 301; the pressure in the suspended carbonization bed The pressure is 0~-3000Pa, and the average wind speed in the cross section of the suspended carbonization bed is 3~10m / s; at the same time, water or carbonization aid aqueous solution is sprayed into the suspended carbonization bed in the form of droplets through the spray gun 306, so that the water vapor in the flue gas forms a critical saturation state (relative humidity ≥90%); since the surface temperature of the material is lower than the dew point temperature of the water vapor, the water vapor condenses on the surface of the material to form a liquid film, and the liquid film provides a transmission medium in the gas-solid carbonization reaction, and the CO2 in the flue gas dissolves in the liquid film to react with the material to accelerate the carbonization reaction.

[0098] During the suspended carbonization process, ultrasonic vibration is added to the bottom of the suspended carbonization bed. High-frequency ultrasound can accelerate the disturbance of the material and flue gas flow at the bottom of the suspended carbonization bed, speed up the reaction speed, reduce particle agglomeration, promote the formation of liquid film on the material surface and fully cover the particle surface.

[0099] In the carbonization aid aqueous solution, the carbonization aid is one of lignin sulfonates, polycyclic aromatic salts, water-soluble resin sulfonates, and alcohol-ammonia organic substances, or a combination of any two of them.

[0100] Coarse powder cycle:

[0101] The water vapor in the flue gas leaving the suspended carbonization bed is close to the critical saturation state (relative humidity ≥ 90%). In order to avoid condensation in the subsequent powder selection and separation device 7 and the bag dust collector 4, a secondary temperature-controlled mixing chamber 6 is set before the powder selection and separation device 7. A part of the clean flue gas leaving the kiln tail preheating and predecomposition system and after dust removal is introduced into the secondary temperature-controlled mixing chamber 6 to increase the temperature of the flue gas leaving the suspended carbonization bed and reduce the humidity of the flue gas.

[0102] The flue gas with a temperature of 70-90°C out of the suspended carbonization bed carries the material into the secondary temperature control mixing chamber 6 and mixes with the clean flue gas (the clean flue gas Q3 entering the secondary temperature control mixing chamber) after the preheating and pre-decomposition system out of the kiln tail and dust removal. The flue gas temperature out of the secondary temperature control mixing chamber 6 is controlled at ≥90°C, and then enters the powder selection and separation device 7. The coarse powder in the material is collected and discharged from the bottom of the powder selection and separation device 7, and the fine powder is discharged from the top of the powder selection and separation device with the flue gas. The coarse powder out of the powder selection and separation device 7 is divided into two paths by the material dividing valve 702. One part is used as the circulating material M4 out of the powder selection and separation device and is transported back to the air duct 307 through the material pipe and then enters the suspended carbonization bed for circulating carbonization. The other part is used as the second-level finished product M5 and is led to the high-activity SCM material finished product. The circulation rate of the coarse powder in the suspended carbonization bed is controlled by the opening of the material dividing valve 702 to avoid the coarse powder that has been fully carbonized from circulating in the suspended carbonization bed indefinitely, thereby causing excessive circulation load and causing the suspended carbonization bed to press.

[0103] Finished product collection:

[0104] The flue gas and fine powder discharged from the top of the powder selection and separation device 7 enter the bag dust collector 4 under the exhaust of the induced draft fan 5, and the flue gas passes through the filter bag 401 with a filtration wind speed of 0.5-1.5 m / min, so that the fine powder forms a powder cake on the surface of the filter bag. The CO2 in the flue gas continues to carbonize with the material during the process of passing through the powder cake, and the compressed air is blown regularly to clean the powder cake. The powder collected from the bag dust collector is used as the first-stage finished product M2, and the first-stage finished product M2 and the second-stage finished product M5 are used as the combined finished product M6 and are led to the high-activity SCM material finished product. The flue gas discharged from the bag dust collector is low-CO2 flue gas Q2.

[0105] The following is a detailed description of the process of preparing high-activity SCM materials from low-carbon raw materials, as follows:

[0106] The siliceous raw material, the calcareous raw material, the gypsum and the mineralizer are ground into raw materials in a certain proportion, wherein the content of SiO2 in the siliceous raw material is ≥50%, the content of CaO in the calcareous raw material is ≥35%, the gypsum is phosphogypsum, and the mineralizer is fluorite and boron.

[0107] The raw material passes through the preheater 101 and the decomposition furnace 102 at the end of the kiln and is sent to the rotary kiln 103 for calcination. The calcination temperature is 1100-1300°C and the calcination time is 30-60 minutes. The calcined clinker is in granular form and is sent to the grate cooler 104 for cooling to obtain low-carbon cement clinker. The mineral composition of the low-carbon cement clinker includes: α′-C2S, C4A3$, C5S2$, CS, and β-C2S, wherein the sum of the contents of α′-C2S and β-C2S accounts for 45% of the total mass of the low-carbon cement clinker, the sum of the contents of C4A3$ and C5S2$ accounts for 25% of the total mass of the low-carbon cement clinker, the content of CS accounts for 23% of the total mass of the low-carbon cement clinker, and the rest is glass phase.

[0108] The flue gas at the kiln tail of the cement burning system comes from two parts: one part is the flue gas generated by the combustion of fuel. The fuel is fed into the rotary kiln and the decomposition furnace respectively, and the fuel and air are burned to produce flue gas; the other part is the CO2 generated by the decomposition of raw materials. The calcium carbonate in the raw materials is decomposed in the decomposition furnace to produce CO2. The CO2 generated by the decomposition of raw materials is mixed with the flue gas generated by the combustion of fuel as the flue gas at the kiln tail, and is discharged from the preheater 101 under the exhaust of the high-temperature fan 106. The flue gas at the kiln tail contains 25% to 35% CO2. The flue gas at the kiln tail of the high-temperature fan 106 is dedusted by the dust collector 107 and is used as clean flue gas. It enters the suspended carbonization bed and the secondary temperature control mixing chamber 6 respectively. The clean flue gas temperature is 100 to 150 ° C and the CO2 concentration is 25% to 35%.

[0109] The low-carbon cement clinker particles K are transported to the clinker grinding system 2, and the kiln tail flue gas Q4 entering the clinker grinding system is introduced to the clinker grinding system 2. The kiln tail flue gas contains 25% to 35% CO2. After grinding, low-carbon cement clinker powder M1 is produced, with an average particle size of less than 200um, and particles with a particle size distribution of 5 to 200um account for more than 90%. During the grinding process, part of the low-carbon cement clinker reacts with the CO2 in the flue gas to reduce the CO2 concentration in the flue gas.

[0110] The pressure in the suspended carbonization bed is 0 to -3000Pa. The clean flue gas Q1 from the air inlet pipe passes through the air duct 307 and the spray pipe 301 at the bottom of the suspended carbonization bed in turn and then sprays upward into the suspended carbonization bed layer. The average wind speed in the cross section of the suspended carbonization bed is 3 to 10m / s. The spray pipe 301 is a vertical pipe with a guide plate inside to promote the uniform distribution of flue gas. At the carbonization bed cone 302, the water or carbonization aid aqueous solution in the water spray system 305 is sprayed into the suspended carbonization bed in the form of droplets through a spray gun 306. By adjusting the amount of the sprayed aqueous solution, the water vapor content in the flue gas is close to the critical saturation concentration.

[0111] The ultrasonic generator 304 at the bottom of the suspended carbonization bed is turned on, and the room temperature low carbon cement clinker powder M1 (≤60°C) is dispersedly fed into the air duct 307 through the spreading device and sprayed into the suspended carbonization bed driven by the clean flue gas. The material is suspended in the flue gas under the drag of the airflow. Since the surface temperature of the material is lower than the dew point temperature of water vapor, water vapor condenses on the surface of the material particles A to form a liquid film B. The liquid film provides a transmission medium in the gas-solid carbonization reaction. The CO2 in the flue gas C dissolves into the liquid film to react with the material to carbonize, thereby accelerating the carbonization reaction.

[0112] The main carbonization reactions are as follows:

[0113]

[0114] In order to improve the activity, the carbonization degree is appropriate, and the carbonization rate of low carbon cement clinker powder is 10% to 20%.

[0115] The flue gas with a temperature of 70-90°C out of the suspended carbonization bed carries the material into the secondary temperature-controlled mixing chamber 6 and mixes with the clean flue gas Q2 entering the secondary temperature-controlled mixing chamber, so that the flue gas temperature out of the secondary temperature-controlled mixing chamber 6 is controlled at ≥90°C. The water vapor in the flue gas out of the suspended carbonization bed is close to the critical saturation state (relative humidity ≥90%). In order to avoid condensation in the subsequent powder selection and separation device 7 and the bag dust collector 4, a secondary temperature-controlled mixing chamber 6 is set before the powder selection and separation device 7, and a part of the clean flue gas is introduced into the secondary temperature-controlled mixing chamber 6, which can increase the temperature of the flue gas out of the suspended carbonization bed and reduce the humidity of the flue gas.

[0116] The flue gas from the secondary temperature-controlled mixing chamber 6 carries the material into the powder selection and separation device 7. The coarse powder in the material is collected and discharged from the bottom of the powder selection and separation device 7. The coarse powder from the powder selection and separation device 7 is divided into two paths through the dividing valve 702. One part is transported back to the air duct through the material pipe and then enters the suspended carbonization bed for cyclic carbonization. The other part is divided and led to the high-activity SCM material finished product. The circulation rate of the coarse powder in the suspended carbonization bed is controlled by the opening of the dividing valve to avoid the unlimited circulation of the fully carbonized coarse powder in the suspended carbonization bed, thereby causing excessive circulation load and causing the suspended carbonization bed to press. Fine powder is discharged from the air duct at the top of the powder selection and separation device with the flue gas.

[0117] The flue gas and fine powder discharged from the top of the powder selection and separation device 7 enter the bag dust collector 4 under the exhaust of the induced draft fan 5. A vertically placed filter bag 401 is arranged inside the bag dust collector 4. The flue gas passes through the filter bag with a filtration wind speed of 0.5-1.5 m / min, so that the fine powder forms a powder cake on the surface of the filter bag. The CO2 in the flue gas continues to carbonize with the material during the process of passing through the powder cake, and the compressed air is regularly purged to clean the powder cake regularly. The powder collected from the bag dust collector is a highly active SCM material after carbonization, and the flue gas discharged from the bag dust collector is a low CO2 flue gas Q3.

[0118] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents, and these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A system for preparing high-activity SCM materials from low-carbon raw materials, characterized by: Including cement burning system, clinker grinding system, low-pressure suspended carbonization bed system, bag dust collector and induced draft fan; The cement burning system comprises a kiln tail preheating and precalcining system, a rotary kiln and a grate cooler which are connected in sequence; the material outlet of the grate cooler is connected to the material inlet of the clinker grinding system, the kiln tail flue gas outlet of the kiln tail preheating and precalcining system is connected to the flue gas inlet of the clinker grinding system, and the powdered material outlet of the clinker grinding system is connected to the material inlet of the low-pressure suspended carbonized bed system; The low-pressure suspended carbonization bed system comprises an air duct, a suspended carbonization bed and a water spray system. The air duct is located below the suspended carbonization bed, and the bottom of the air duct is a flue gas inlet. The kiln tail flue gas outlet of the kiln tail preheating and predecomposition system is connected to the flue gas inlet of the air duct through a dust collector. The material inlet of the low-pressure suspended carbonization bed system is arranged on the air duct or the suspended carbonization bed, so that the powdered material moves upward under the drive of the flue gas. The top of the air duct is connected to the bottom of the suspended carbonization bed, and a spray pipe is arranged at the connection part, so that the clean flue gas after the kiln tail preheating and predecomposition system and dust removal is sprayed upward into the suspended carbonization bed; a plurality of spray guns are arranged at the lower part of the suspended carbonization bed and are located above the spray pipe, and the outlet of the water spray system is connected to the inlet of the spray gun, so that the aqueous solution is sprayed into the suspended carbonization bed in the form of droplets, and the water vapor in the flue gas in the suspended carbonization bed forms a critical saturation state of water vapor-water droplets, and a liquid film is formed on the surface of the material; The outlet of the suspended carbonization bed is connected to the flue gas inlet of the bag dust collector; the material outlet of the bag dust collector is connected to the high-activity SCM material finished product, or is respectively connected to the high-activity SCM material finished product and the material inlet of the low-pressure suspended carbonization bed system, and the flue gas outlet of the bag dust collector is connected to the induced draft fan inlet.

2. The system for preparing high-activity SCM materials from low-carbon raw materials according to claim 1, characterized in that: The suspended carbonization bed comprises a spray pipe, a carbonization bed cone and a carbonization bed column which are sequentially connected from bottom to top; the spray pipe is a vertical pipe, and a flow guide device for evenly distributing the smoke is arranged inside the spray pipe.

3. The system for preparing high-activity SCM materials from low-carbon raw materials according to claim 2, characterized in that: An ultrasonic generator is arranged at the vertebral body of the carbonization bed.

4. The system for preparing high-activity SCM materials from low-carbon raw materials according to claim 1, characterized in that: A secondary temperature-controlled mixing chamber is arranged between the suspended carbonization bed and the bag dust collector, and the secondary temperature-controlled mixing chamber is used to increase the temperature of the flue gas exiting the suspended carbonization bed and reduce the humidity of the flue gas; the secondary temperature-controlled mixing chamber has inlet one, inlet two and an outlet, the top outlet of the suspended carbonization bed is connected to inlet one of the secondary temperature-controlled mixing chamber, the kiln tail flue gas outlet of the kiln tail preheating and predecomposition system is connected to inlet two of the secondary temperature-controlled mixing chamber through a dust collector, and the outlet of the secondary temperature-controlled mixing chamber is connected to the flue gas inlet of the bag dust collector.

5. The system for preparing high-activity SCM materials from low-carbon raw materials according to claim 4, characterized in that: A temperature measuring device is provided on the outlet pipe of the secondary temperature-controlled mixing chamber.

6. The system for preparing highly active carbonized materials from low-carbon raw materials according to claim 4, characterized in that: A powder selection and separation device is arranged between the secondary temperature-controlled mixing chamber and the bag dust collector, the outlet of the secondary temperature-controlled mixing chamber is connected to the flue gas inlet of the powder selection and separation device, the bottom material outlet of the powder selection and separation device is connected to the material inlet of the low-pressure suspended carbonization bed system, and the top flue gas outlet of the powder selection and separation device is connected to the flue gas inlet of the bag dust collector.

7. The system for preparing high-activity SCM materials from low-carbon raw materials according to claim 6, characterized in that: The powder selection and separation device is a powder selection machine or a cyclone, which is used to separate coarse powder and fine powder in the material.

8. The system for preparing high-activity SCM materials from low-carbon raw materials according to claim 6, characterized in that: An air lock valve and a material distributor valve are sequentially arranged on the material pipe at the bottom material outlet of the powder selection and separation device. The bottom material outlet of the powder selection and separation device is also connected to the high-activity SCM material finished product through the material distributor valve, so that the coarse powder exiting the powder selection and separation device can enter the suspended carbonization bed and the high-activity SCM material finished product respectively.

9. The system for preparing high-activity SCM materials from low-carbon raw materials according to claim 1, characterized in that: The bag dust collector is provided with a vertically placed filter bag, and is also provided with a compressed air blowing device for regularly cleaning powder cakes on the surface of the filter bag.

10. A method for preparing a high-activity SCM material from a low-carbon raw material using the system according to any one of claims 1 to 9, comprising the following steps: S1. Raw material batching and clinker burning The silicon raw material, calcium raw material, gypsum and mineralizer are ground into raw materials according to a certain ratio, and then the raw materials are preheated and decomposed by the preheating and pre-decomposition system at the kiln tail, and then sent to the rotary kiln for calcination. The calcination temperature in the rotary kiln is 1100-1300℃. The calcined clinker is sent to the grate cooler for cooling to obtain low-carbon cement clinker; S2. Clinker grinding The low-carbon cement clinker particles are transported to the clinker grinding system, and the tail gas of the kiln preheating and pre-decomposition system is introduced to the clinker grinding system. The tail gas of the kiln preheating and pre-decomposition system contains 25% to 35% CO2, which is ground into low-carbon cement clinker powder. The average particle size of the low-carbon cement clinker powder is less than 200μm. S3. Carbonization to prepare highly active SCM materials Suspension Carbonization: The clean flue gas after the preheating and pre-decomposition system at the kiln tail and the dust removal is introduced into the flue gas inlet of the air duct. The clean flue gas after the preheating and pre-decomposition system at the kiln tail and the dust removal has a temperature of 100-150°C and a CO2 concentration of 25%-35%; the clean flue gas moves upward and is sprayed into the suspended carbonization bed through the spray pipe; at the same time, the low-carbon cement clinker powder with a temperature of ≤60°C and an average particle size of less than 200μm is dispersed and fed into the air duct or the suspended carbonization bed, so that the material is suspended in the clean flue gas under the drag of the air flow; the pressure in the suspended carbonization bed is 0-3000Pa, and the average wind speed in the cross section of the suspended carbonization bed is 3-10m / s; at the same time, water or carbonization aid aqueous solution is sprayed into the suspended carbonization bed in the form of droplets through a spray gun, so that the water vapor in the flue gas forms a critical saturation state; the water vapor forms a liquid film on the surface of the material, and the CO2 in the flue gas dissolves in the liquid film to react with the material to carbonize; Coarse powder circulation and finished product collection: The flue gas from the suspended carbonization bed carries the material and enters the bag dust collector under the draft of the induced draft fan. After the material is collected, part of it returns to the low-pressure suspended carbonization bed system for cyclic carbonization, and part of it is led to the high-activity SCM material finished product; or, all of it is led to the high-activity SCM material finished product.

11. The method for preparing high-activity SCM materials from low-carbon raw materials according to claim 10, characterized in that: The content of SiO2 in the siliceous raw material is ≥50%, the content of CaO in the calcareous raw material is ≥35%, the gypsum is one of desulfurized gypsum, phosphogypsum, and natural gypsum, and the mineralizer is one of fluorite, calcium fluoride, borax, and boric acid, or a combination of any two of them.

12. The method for preparing high-activity SCM materials from low-carbon raw materials according to claim 10, characterized in that: The mineral composition of the low carbon cement clinker includes: α′-C2S, C4A3$, C5S2$, CS, and β-C2S, wherein the sum of the contents of α′-C2S and β-C2S accounts for more than 40% of the total mass of the low carbon cement clinker, the sum of the contents of C4A3$ and C5S2$ accounts for more than 20% of the total mass of the low carbon cement clinker, the content of CS accounts for more than 20% of the total mass of the low carbon cement clinker, and the rest is glass phase.

13. The method for preparing high-activity SCM materials from low-carbon raw materials according to claim 10, characterized in that: During the suspension carbonization process, ultrasonic vibration is added to the bottom of the suspension carbonization bed.

14. The method for preparing high-activity SCM materials from low-carbon raw materials according to claim 10, characterized in that: In the carbonization aid aqueous solution, the carbonization aid is one of lignin sulfonates, polycyclic aromatic salts, water-soluble resin sulfonates, and alcohol-ammonia organic substances, or a combination of any two of them.

15. The method for preparing high-activity SCM materials from low-carbon raw materials according to claim 10, characterized in that: The flue gas carrying materials out of the suspended carbonization bed first enters the secondary temperature-controlled mixing chamber and mixes with part of the clean flue gas out of the kiln tail preheating and predecomposition system and after dust removal, and then enters the bag dust collector; the flue gas temperature out of the secondary temperature-controlled mixing chamber is controlled at ≥90℃.

16. The method for preparing high-activity SCM materials from low-carbon raw materials according to claim 15, characterized in that: The flue gas carrying the material out of the secondary temperature-controlled mixing chamber first enters the powder selection and separation device. The coarse powder in the material is collected and discharged from the bottom of the powder selection and separation device. Part of it returns to the low-pressure suspended carbonization bed system for cyclic carbonization, and part of it is led to the high-activity SCM material finished product; the fine powder is discharged from the top of the powder selection and separation device with the flue gas and enters the bag dust collector. The flue gas passes through the filter bag with a filtration wind speed of 0.5-1.5m / min, so that the fine powder forms a powder cake on the surface of the filter bag. The CO2 in the flue gas continues to carbonize with the material during the process of passing through the powder cake, and the compressed air is regularly blown to clean the powder cake. The powder collected from the bag dust collector is carbonized micro-powder material, which is led to the high-activity SCM material finished product.

Citation Information

Patent Citations

  • Carbonized micro-powder industrial production device based on gas-solid convection suspension carbonization principle

    CN115814715A

  • Method for preparing auxiliary cementing material and concrete product by using industrial kiln tail gas carbonized steel slag

    CN116903340A

  • Preparation method of novel low-carbon clinker and high-activity SCM material

    CN116947346A

  • Device for preparing low-carbon admixture by utilizing homogenization-carbonization synergy

    CN217757282U

  • Apparatus for the production of clinker from raw meal and relative process

    US20110311931A1

Cited By

  • Recycled concrete micro-powder preparation system with modified carbon sequestration function

    CN120920155A