Catalyst slurry, VOCs catalytic oxidation catalyst, and preparation methods and applications of catalyst slurry and VOCs catalytic oxidation catalyst
The catalyst slurry prepared through highly dispersed precipitation and grinding technology is loaded onto the carrier to form a highly efficient VOCs catalytic oxidation catalyst, which solves the problem of low catalyst resistance in water and sulfur atmospheres, improves catalytic performance and precious metal utilization efficiency, and is suitable for many applications. Preparation of fixed bed catalytic materials.
Patent Information
- Application Number
- CN202310484351.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing VOCs oxidation catalysts show low resistance in water and sulfur atmospheres, precious metal active centers are easily poisoned, and low-temperature catalytic oxidation activity efficiency is low. How to improve the water resistance and sulfur resistance of the catalyst and the utilization efficiency of precious metals are urgently needed. question.
By mixing and precipitating components such as precious metal precursors, alkaline earth metal precursors, matrix sources, and oxalic acid, a highly dispersed active material precursor is formed, and is mixed and ground with oxygen storage materials and binders to prepare a catalyst slurry, which is then loaded onto a carrier. After drying and roasting, a VOCs catalytic oxidation catalyst with high dispersion, high water resistance and sulfur resistance is formed.
It achieves high dispersion, stability and improvement of catalytic performance of the catalyst, significantly improves the degradation efficiency of VOCs, and extends the life of the catalyst. It is suitable for batch production and the application of various fixed bed catalytic materials.
Smart Images

Figure CN118847104A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalyst preparation, and in particular to a method for preparing a catalyst slurry, a catalyst slurry prepared by the method, a method for preparing a VOCs catalytic oxidation catalyst, a VOCs catalytic oxidation catalyst prepared by the method, and applications of the catalyst slurry and the VOCs catalytic oxidation catalyst in catalytic oxidation of VOCs. Background Art
[0002] Volatile Organic Compounds (VOCs) are the main pollutants in waste gas emitted during the production and processing of various industries such as petrochemicals, printing, and pharmaceuticals. They have a noticeable odor and can irritate or harm human organs. In severe cases, they can cause poisoning or cancer, endangering human health. In addition, VOCs participate in the formation of ozone and secondary aerosols in the atmospheric environment, and have an important impact on regional atmospheric ozone pollution and PM2.5 pollution.
[0003] VOCs pollution control can be divided into adsorption, incineration, catalytic oxidation, biological methods and membrane separation methods. Among them, catalytic oxidation technology is one of the most promising technologies for removing VOCs; and the development of high-performance catalytic oxidation catalysts is the key to achieving exhaust gas purification and green production. At present, catalytic oxidation catalysts are mostly based on honeycomb inert materials (such as cordierite, etc.) as carriers, loaded with active components with low-temperature oxidation properties to achieve VOCs catalytic oxidation.
[0004] VOCs oxidation catalysts used in industry usually use precious metals such as platinum and palladium as active components. This type of precious metal catalyst can activate hydrocarbons and oxygen at low temperatures and exhibit excellent low-temperature catalytic oxidation activity. However, precious metals are expensive. How to improve the utilization efficiency of precious metals by improving slurry preparation technology under the premise of low loading is an urgent problem to be solved in this field. In addition, the active center of the precious metal is easily poisoned when the reaction atmosphere contains water and sulfur. In order to improve the hydrothermal performance of the catalyst, CN109395742A discloses a catalyst for the purification of volatile organic compounds that is resistant to degradation. The coating contains Al 2 O 3 、MnO 2 Compared with the precious metal Pt, it still has excellent performance after hydrothermal aging, but the catalyst's sulfur resistance is not mentioned. In order to extend the life of precious metal catalysts, industrial catalytic oxidation integrated devices usually remove hydrogen sulfide from the gas through alkaline pre-desulfurization, but there is currently no good removal method for some alkaline sulfur-containing VOCs components. In this context, how to improve the catalyst's own water and sulfur resistance is the key to solving this type of problem. Summary of the invention
[0005] The purpose of the present invention is to provide a VOCs low-temperature catalytic oxidation catalyst with high dispersion of active components and high water and sulfur resistance. Specifically, a method for preparing a catalyst slurry, a catalyst slurry prepared by the method, a method for preparing a VOCs catalytic oxidation catalyst, a VOCs catalytic oxidation catalyst prepared by the method, and the use of the catalyst slurry and the VOCs catalytic oxidation catalyst in the catalytic oxidation of VOCs. The VOC catalytic oxidation catalyst has excellent water and sulfur resistance and also has a certain improvement in the degradation efficiency of VOCs.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a catalyst slurry, the method comprising:
[0007] (1) mixing a noble metal precursor, an alkaline earth metal precursor, a matrix source and a first solvent to obtain a mixed solution, adjusting the pH of the mixed solution to 2-5, adding oxalic acid to perform a first precipitation, and then sequentially adding a tin precursor and an alkali to perform a second precipitation to obtain a second precipitate, and sequentially dechlorinating, drying and calcining the second precipitate to obtain an active material precursor;
[0008] (2) mixing and grinding the active material precursor, the oxygen storage material, the binder and the second solvent to obtain a catalyst slurry;
[0009] Wherein, the noble metal precursor is a chlorate or chloride of a noble metal.
[0010] The second aspect of the present invention provides a catalyst slurry prepared by the method described above.
[0011] The third aspect of the present invention provides a method for preparing a VOCs catalytic oxidation catalyst, which comprises loading the catalyst slurry as described above onto a carrier, and then performing drying and calcining treatment to obtain a VOCs catalytic oxidation catalyst.
[0012] A fourth aspect of the present invention provides a VOCs catalytic oxidation catalyst prepared by the method described above.
[0013] A fifth aspect of the present invention provides use of the catalyst slurry as described above or the VOCs catalytic oxidation catalyst as described above in catalytic oxidation of VOCs.
[0014] The method described in the present invention can highly disperse and adsorb and anchor the noble metal chlorate anions by adjusting the surface hydroxyl charges of the matrix source, and in situ precipitate the noble metal precursor adsorbed on the surface of the matrix after adding oxalic acid to form a highly dispersed hydroxide precursor, thereby improving the dispersibility of the active metal. In combination with the use of other additives, the stability, water and sulfur resistance and catalytic performance of the catalyst are further improved.
[0015] The preparation method provided in the present invention is easy to operate, suitable for batch production, and is expected to be extended to the preparation of various fixed-bed catalytic materials, thus having broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The zeta potential values of different matrix sources are shown;
[0017] Figure 2 The adsorption performance of alumina for precious metal chlorates at different pH values. DETAILED DESCRIPTION
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0019] A first aspect of the present invention provides a method for preparing a catalyst slurry, the method comprising:
[0020] (1) mixing a noble metal precursor, an alkaline earth metal precursor, a matrix source and a first solvent to obtain a mixed solution, adjusting the pH of the mixed solution to 2-5, adding oxalic acid to perform a first precipitation, and then sequentially adding a tin precursor and an alkali to perform a second precipitation to obtain a second precipitate, and sequentially dechlorinating, drying and calcining the second precipitate to obtain an active material precursor;
[0021] (2) mixing and grinding the active material precursor, the oxygen storage material, the binder and the second solvent to obtain a catalyst slurry;
[0022] Wherein, the noble metal precursor is a chlorate or chloride of a noble metal.
[0023] Preferably, the noble metal is selected from at least one of platinum, palladium, rhodium and silver. The noble metal precursor may be chloroplatinic acid, chloropalladic acid, chlororhodic acid, and the like.
[0024] Preferably, the alkaline earth metal is selected from at least one of magnesium, calcium, strontium and barium.
[0025] Preferably, the alkaline earth metal precursor is a soluble salt of an alkaline earth metal, more preferably a nitrate, such as magnesium nitrate, calcium nitrate, and strontium nitrate.
[0026] Preferably, the matrix source is a substance that can be converted into a matrix under calcination conditions, and the matrix is selected from at least one of alumina, pseudo-boehmite, spinel, perovskite, silica-alumina, zeolite, kaolin, diatomaceous earth and perlite, preferably selected from at least one of alumina, pseudo-boehmite, spinel and perovskite, and more preferably alumina. Figure 1 The zeta potential values of different matrix sources (alumina and pseudo-boehmite) are shown. Figure 2 is the adsorption performance of aluminum oxide on precious metal chlorates at different pH values. Figure 1 , Figure 2 It can be seen that lowering the pH will increase the zeta potential of the matrix oxide surface, thereby increasing the adsorption capacity for negatively charged metal chlorate complex ions. This electrostatic adsorption effect helps the precious metal precursor salt to be fully dispersed on the matrix surface, and a highly dispersed precious metal active phase is obtained after precipitation and calcination.
[0027] Preferably, the first solvent is water.
[0028] A pH adjusting agent may be added to the mixed solution to adjust the pH of the mixed solution to 2-5, such as 2, 2.5, 3, 3.5, 4, 4.5, 5, and any range between any two values. Preferably, in step (1), the pH of the mixed solution is adjusted to 3-4.5. Preferably, the pH adjusting agent is a pH adjusting agent that cannot precipitate precious metals, such as nitric acid.
[0029] The concentration of the acid is not particularly limited, and may be, for example, 0.1-10 mol / L.
[0030] After the pH is adjusted to 2-5, oxalic acid is added to perform a first precipitation. The first precipitation can be performed under stirring conditions. Preferably, the first precipitation time is 0.5-2 hours.
[0031] After the first precipitation, a tin precursor and a base are sequentially added to perform a second precipitation. Preferably, the tin precursor salt is a soluble salt of tin, preferably a chloride of tin, such as tin tetrachloride.
[0032] Preferably, the alkali is selected from at least one of sodium hydroxide, sodium carbonate and aqueous ammonia.
[0033] Preferably, the amount of the base used makes the pH of the material during the second precipitation be 5-9, for example, it can be 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9 and any range between any two values, more preferably 5-8.
[0034] Preferably, the second precipitation time is 0.5-2h. The second precipitation can be carried out under stirring conditions.
[0035] Preferably, compared to 100 parts by weight of the mixed solution, the amount of the noble metal precursor is 0.01-0.5 parts by weight, for example, it can be 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5 parts by weight and any range between any two values, more preferably 0.1-0.4 parts by weight; the amount of the alkaline earth metal precursor is 0.1-1.2 parts by weight, for example The amount of the matrix source is 5-50 parts by weight, for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50 parts by weight, and any range between any two values, more preferably 10. -30 parts by weight; the amount of the first solvent is 50-95 parts by weight, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95 parts by weight and any range between any two values, more preferably 70-90 parts by weight; the amount of oxalic acid is 0.2-2 parts by weight, for example, 0.2, 0.4, 0.6, 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2 parts by weight and any range between any two values. any range between weight parts and any range between any two values, more preferably 0.4-1.5 weight parts; the amount of tin precursor is 0.1-2 weight parts, for example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2 weight parts and any range between any two values, more preferably 0.5-1.5 weight parts.
[0036] The amount of each precursor used is based on the weight of the compound.
[0037] The obtained second precipitate can be dechlorinated by conventional methods in the art. It should be understood that the second precipitate can be separated from the reaction material by solid-liquid separation in advance. Preferably, in step (1), the dechlorination method is washing until there is no precipitation of the silver nitrate detection reagent. The washing liquid used for washing can be water or ethanol.
[0038] Preferably, in step (1), the drying conditions include: a drying temperature of 80-140°C (for example, 80, 90, 100, 110, 120, 130, 140°C and any range between any two values), a drying time of 4-12h (for example, 4, 6, 8, 10, 12h and any range between any two values). The drying method may be vacuum drying, preferably, the vacuum degree is 0.05Mpa-0.1Mpa.
[0039] Preferably, in step (1), the calcination conditions include: a calcination temperature of 150-250°C (for example, 150, 160, 180, 200, 220, 240, 250°C and any range between any two values), a calcination time of 1-3h (for example, 1, 1.5, 2, 2.5, 3h and any range between any two values), and more preferably, the temperature is increased to 150-250°C at a rate of 2-6°C / min (for example, 2, 3, 4, 5, 6°C / min and any range between any two values).
[0040] Preferably, the calcination atmosphere is an ozone atmosphere.
[0041] In step (2), the active material precursor, the oxygen storage material, the binder and the second solvent are mixed and ground to obtain a catalyst slurry.
[0042] Preferably, the oxygen storage material is selected from at least one of bismuth oxide, cerium oxide, cerium-zirconium solid solution and niobium oxide, more preferably bismuth oxide.
[0043] Preferably, the binder is selected from at least one of silica sol, alumina sol and acidic alumina, wherein the amount of the binder is calculated based on the amount of its oxide.
[0044] Preferably, the second solvent is water.
[0045] Preferably, the amount of each component is such that in the catalyst slurry, the content of the active material precursor is 4-35 weight % (for example, it can be 4, 5, 10, 15, 20, 25, 30, 35 weight % and any range between any two values), more preferably 8-20 weight %, the content of the oxygen storage material is 0.5-4 weight % (for example, it can be 2, 3, 4, 5, 6°C / min and any range between any two values), more preferably 1-3 weight %, and the content of the binder is 1-3 weight % (for example, it can be 2, 3, 4, 5, 6°C / min and any range between any two values), more preferably 1.5-2.5 weight %.
[0046] Preferably, in step (2), the grinding method is ball milling. Preferably, the ball milling time is 1-5 hours, and the rotation speed is 500-1500 rpm. A vibrating ball mill (such as the GZM-6 vibrating ball mill of Tianjin Shengyuan Equipment Company) can be used for ball milling.
[0047] Preferably, in step (2), the grinding conditions are such that the average particle diameter of the catalyst slurry is less than 15 μm, more preferably 2-11 μm, for example, 2, 4, 6, 8, 10, 11 μm and any range between any two values.
[0048] The average diameter of the particles in the catalyst slurry is the equivalent volume diameter obtained by laser particle size method. Test instrument: Malvern Mastersizer 3000.
[0049] The second aspect of the present invention provides a catalyst slurry prepared by the method described above.
[0050] The third aspect of the present invention provides a method for preparing a VOCs catalytic oxidation catalyst, which comprises loading the catalyst slurry as described above onto a carrier, and then performing drying and calcining treatment to obtain a VOCs catalytic oxidation catalyst.
[0051] Preferably, the catalyst slurry loading is such that based on the volume of the carrier, the loading amount of the catalyst layer is 20-140 g / L, for example, it can be 20, 40, 60, 80, 100, 120, 140 g / L and any range between any two values, more preferably 30-100 g / L.
[0052] Preferably, the drying conditions include: a temperature of 80-140°C (e.g., 80, 90, 100, 110, 120, 130, 140°C and any range between any two values), a time of 0.5-4h (e.g., 0.5, 1, 2, 3, 4h and any range between any two values). The drying method may be vacuum drying, preferably, the vacuum degree is 0.05Mpa-0.1Mpa.
[0053] Preferably, the calcination conditions include: a calcination temperature of 150-300°C (e.g., 150, 250, 280, 300°C, and any range between any two values), and a calcination time of 1-3h (e.g., 1, 1.5, 2, 2.5, 3h, and any range between any two values). For example, the temperature may be raised to 250-550°C at a rate of 3-10°C / min (e.g., 3, 4, 6, 8, 10°C / min, and any range between any two values), and maintained for 1-3h.
[0054] Preferably, the calcination atmosphere is an ozone atmosphere.
[0055] The present invention has a wide range of choices for the carrier, and can be various carriers commonly used in the art, and the present invention has no particular limitation on this. For example, the carrier can be an inorganic oxide carrier. Preferably, the carrier is selected from at least one of cordierite, mullite, diamond, corundum, zirconium corundum, quartz, nepheline, feldspar, alumina and metal alloys.
[0056] Preferably, the carrier is a regular structure carrier, that is, the appearance of the carrier is a regular structure, which is easy to assemble, and the pore structure of the carrier can also be regular.
[0057] Preferably, the pore density of the cross section of the regular structure carrier is 50-400 pores / square inch, for example, it can be 50, 100, 150, 200, 250, 300, 350, 400 pores / square inch and any range between any two values.
[0058] Preferably, the cross-sectional area of each hole in the carrier is 0.4-10 square millimeters, preferably 0.4-4 square millimeters.
[0059] Preferably, the open porosity of the carrier surface is 20-80%, more preferably 50-80%.
[0060] The holes may be of regular or irregular shapes, and the shapes of the holes may be the same or different, and each hole may be independently in the shape of a square, a regular triangle, a regular hexagon, a circle, or a corrugated shape.
[0061] The carrier of the present invention can be used for the catalyst bed provided in the fixed bed reactor. The carrier can be a whole carrier block, with a hollow channel structure formed inside, a catalyst layer can be distributed on the inner wall and / or outer wall of the channel, and the channel space can be used as a flow space for the fluid. The carrier can be a regular carrier with honeycomb openings in the cross section (referred to as a honeycomb carrier).
[0062] In the present invention, the catalyst slurry can be evenly loaded on the surface of the carrier by spraying, coating or immersion, and then dried and calcined to obtain a carrier with catalyst layers loaded on the inner and outer surfaces. For example, the carrier can be immersed in the catalyst slurry for 5-30 seconds for loading.
[0063] It should be understood that in the present invention, the preferred conditions can be more conducive to improving the performance of the catalyst, reducing the catalytic temperature, and improving the catalytic effect.
[0064] A fourth aspect of the present invention provides a VOCs catalytic oxidation catalyst prepared by the method described above.
[0065] A fifth aspect of the present invention provides use of the catalyst slurry as described above or the VOCs catalytic oxidation catalyst as described above in catalytic oxidation of VOCs.
[0066] The present invention will be described in detail below by way of examples. The following examples will further illustrate the present invention, but are not intended to limit the present invention.
[0067] The average particle diameter in the catalyst slurry is the equivalent volume diameter obtained by laser particle size method. Test instrument: Malvern Mastersizer 3000.
[0068] The activity evaluation of the toluene catalytic oxidation reaction was completed on a micro-fixed bed reactor designed and manufactured by Tianjin Pengxiang Technology Co., Ltd., equipped with a Multigas 2030 infrared detector from MKS. The reaction was carried out under normal pressure, with an initial temperature of 150°C and a temperature increase rate of 3°C / min until the VOCs pollutants were completely converted. The inlet gas composition was 450ppm C 7 H 8 / 7%O 2 / N 2 , airspeed 12000h -1 .
[0069] The carrier is a VOC-specific cordierite honeycomb carrier purchased from Pingxiang Guanlin Environmental Protection Technology Co., Ltd. The carrier hole density is 300 holes / square inch, the cross-sectional area of each hole is 1.5 square millimeters, the open porosity is 70%, and the hole shape is circular.
[0070] Aluminum sol is produced by Shandong Guohua Chemical, with a solid content of 20% and a specific surface area of 0.256m 2 / g.
[0071] Example 1
[0072] (1) 2.5 g of chloroplatinic acid, 5 g of calcium nitrate, 250 g of aluminum oxide and 750 g of water were mixed, and then 1 mol / L nitric acid was used to adjust the pH to 3.5. 7.5 g of oxalic acid was added under stirring conditions. After 1 hour, 9 g of tin tetrachloride was added, and then sodium hydroxide was added to adjust the pH to 6. After stirring for 1 hour, the residual chloride ions were removed by repeated filtration and washing for 4 times until there was no precipitation of the silver nitrate detection reagent. The obtained precipitate was then dried at 120° C. for 6 hours, and heated to 200° C. at a rate of 5° C. / min in an ozone atmosphere, and maintained for 2 hours to obtain an active material precursor;
[0073] (2) 240 g of active material precursor, 40 g of bismuth oxide, 40 g of aluminum sol (calculated as alumina) and 2 L of water were mixed and stirred for 2 h. The mixture was fully ground using a vibrating ball mill (Tianjin Shengyuan Equipment Co., Ltd., GZM-6). The specific grinding conditions were: ball milling time 2.5 h, rotation speed 950 rpm, and the average particle diameter of the mixed solution after ball milling was 9.9 μm. The catalyst slurry was then evenly coated on the surface of a 300-mesh regular structure carrier so that the total coating amount on each liter of the ceramic carrier was 70 g.
[0074] (3) The carrier coated with the catalyst slurry was dried at 140° C. for 2 h, and then subjected to ozone calcination treatment, and the temperature was increased to 180° C. at a rate of 5° C. / min and maintained for 2 h to obtain a VOCs catalytic oxidation catalyst.
[0075] Example 2
[0076] (1) 2.0 g of chloroplatinic acid, 7 g of calcium nitrate, 200 g of aluminum oxide and 850 g of water were mixed, and then 1 mol / L nitric acid was used to adjust the pH to 3.5. 6.5 g of oxalic acid was added under stirring conditions. After 1 hour, 9 g of tin chloride was added in sequence, and then sodium hydroxide was added to adjust the pH to 6. After stirring for 1 hour, the residual chloride ions were removed by repeated filtration and washing for 4 times until there was no precipitation of the silver nitrate detection reagent. The obtained precipitate was then dried at 120° C. for 6 hours, and heated to 200° C. at a rate of 5° C. / min in an ozone atmosphere and maintained for 2 hours to obtain an active material precursor;
[0077] (2) 240 g of active material precursor, 30 g of bismuth oxide, 40 g of aluminum sol (calculated as alumina) and 2 L of water were mixed and stirred for 2 h. The mixture was fully ground using a vibrating ball mill (Tianjin Shengyuan Equipment Co., Ltd., GZM-6). The specific grinding conditions were: ball milling time 2.5 h, rotation speed 950 rpm, and the average particle diameter of the mixed solution after ball milling was 8.5 μm. The catalyst slurry was then evenly coated on the surface of a 300-mesh regular structure carrier so that the total coating amount on each liter of the ceramic carrier was 60 g.
[0078] (3) The carrier coated with the catalyst slurry was dried at 140° C. for 2 h, and then subjected to ozone calcination treatment, and the temperature was increased to 180° C. at a rate of 5° C. / min and maintained for 2 h to obtain a VOCs catalytic oxidation catalyst.
[0079] Example 3
[0080] In step (1), an equal mass of chloropalladic acid is used to replace chloroplatinic acid, and other conditions are the same as in Example 1.
[0081] Example 4
[0082] In step (1), 2.5 g of chloroplatinic acid, 5 g of calcium nitrate, 250 g of aluminum oxide and 750 g of water were mixed, and then the pH was adjusted to 4.5 using 1 mol / L nitric acid. Other conditions were the same as in Example 1.
[0083] Example 5
[0084] In step (1), 9 g of tin tetrachloride was added, and then sodium hydroxide was added to adjust the pH to 7. Other conditions were the same as in Example 1.
[0085] Example 6
[0086] In step (1), 9 g of tin tetrachloride was added, and then sodium hydroxide was added to adjust the pH to 8. Other conditions were the same as in Example 1.
[0087] Comparative Example 1
[0088] In step (1), no tin chloride and no precipitant are added, and other conditions are the same as those in Example 1.
[0089] Comparative Example 2
[0090] In step (2), no bismuth oxide is added, and other conditions are the same as those in Example 1.
[0091] Comparative Example 3
[0092] In step (1), tin chloride is mixed with a noble metal precursor, an alkaline earth metal salt, and a matrix source, and then 1 mol / L nitric acid is used to adjust the pH to 3.5, and 7.5 g of oxalic acid is added under stirring. After 1 hour, 6 g of sodium hydroxide is added, and after stirring for 1 hour, the mixture is filtered and washed four times to remove residual chloride ions until there is no precipitation of the silver nitrate detection reagent. The obtained precipitate is then dried at 120° C. for 6 hours, and heated to 200° C. at a rate of 5° C. / min in an ozone atmosphere, and maintained for 2 hours to obtain an active material precursor. Other conditions are the same as those in Example 1.
[0093] Comparative Example 4
[0094] No alkali was added after adding tin chloride in step (1), and other conditions were the same as in Example 1.
[0095] Comparative Example 5
[0096] In step (1), 2.5 g of chloroplatinic acid, 5 g of calcium nitrate, 250 g of aluminum oxide and 750 g of water were mixed without adjusting the pH (pH was 6), and then 7.5 g of oxalic acid was added under stirring. Other conditions were the same as in Example 1.
[0097] The performance of the VOCs catalytic oxidation catalysts obtained in the examples and comparative examples was evaluated using toluene as a model compound. The conversion temperature T 50 and T99 As shown in Table 1.
[0098] The catalysts prepared in the examples and comparative examples were treated with water and sulfur poisoning, respectively, and the conversion temperature T of the poisoned catalysts for toluene was 99 The results are shown in Table 1.
[0099] The catalyst poisoning conditions are: air atmosphere, containing 10% water vapor, 100 ppm methyl mercaptan, temperature 300° C., and 5 h.
[0100] Table 1 T of each catalyst sample for oxidation of toluene 50 , T 99
[0101]
[0102]
[0103] As can be seen from Table 1, the T 50 and T 99 The toluene oxidation performance and water and sulfur resistance are better than those of the comparative example. The VOCs catalytic material prepared by the present invention has higher pollutant degradation efficiency and is expected to be extended to the preparation of various fixed bed catalytic materials, and has broad application prospects.
[0104] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a catalyst slurry, characterized in that: The method includes: (1) mixing a noble metal precursor, an alkaline earth metal precursor, a matrix source and a first solvent to obtain a mixed solution, adjusting the pH of the mixed solution to 2-5, adding oxalic acid to perform a first precipitation, and then sequentially adding a tin precursor and an alkali to perform a second precipitation to obtain a second precipitate, and sequentially dechlorinating, drying and calcining the second precipitate to obtain an active material precursor; (2) mixing and grinding the active material precursor, the oxygen storage material, the binder and the second solvent to obtain a catalyst slurry; Wherein, the noble metal precursor is a chlorate or chloride of a noble metal.
2. The method according to claim 1, wherein: The noble metal is at least one selected from platinum, palladium and rhodium; and / or The alkaline earth metal is selected from at least one of magnesium, calcium, strontium and barium; preferably, the alkaline earth metal precursor is a soluble salt of the alkaline earth metal, more preferably a nitrate; and / or The matrix source is a substance that can be converted into a matrix under calcination conditions, and the matrix is selected from at least one of alumina, pseudo-boehmite, spinel, perovskite, silica-alumina, zeolite, kaolin, diatomaceous earth and perlite, preferably selected from at least one of alumina, pseudo-boehmite, spinel and perovskite, and more preferably alumina; and / or The tin precursor salt is a soluble salt of tin, preferably tin tetrachloride; and / or The alkali is selected from at least one of sodium hydroxide, sodium carbonate and ammonia water; and / or The first solvent is water; and / or Preferably, compared to 100 parts by weight of the mixed solution, the amount of the noble metal precursor is 0.01-0.5 parts by weight, more preferably 0.1-0.4 parts by weight; the amount of the alkaline earth metal precursor is 0.1-1.2 parts by weight, more preferably 0.3-0.9 parts by weight; the amount of the matrix source is 5-50 parts by weight, more preferably 10-30 parts by weight; the amount of the first solvent is 50-95 parts by weight, more preferably 70-90 parts by weight; the amount of oxalic acid is 0.2-2 parts by weight, more preferably 0.4-1.5 parts by weight; the amount of the tin precursor is 0.1-2 parts by weight, more preferably 0.5-1.5 parts by weight; Preferably, in step (1), the pH of the mixed solution is adjusted to 3-4.5; Preferably, the amount of the base used is such that the pH of the material during the second precipitation is 5-9.
3. The method according to claim 1, wherein: In step (1), the chlorine removal method is to wash until there is no precipitation of the silver nitrate detection reagent; and / or The drying conditions include: drying temperature of 80-140°C and time of 4-10h; The calcination conditions include: the calcination atmosphere is an ozone atmosphere, the calcination temperature is 150-250° C., and the calcination time is 1-3 hours.
4. The method according to claim 1, wherein: The oxygen storage material is selected from at least one of bismuth oxide, cerium oxide, cerium-zirconium solid solution and niobium oxide, preferably bismuth oxide; and / or The binder is selected from at least one of silica sol, alumina sol and acidic alumina; and / or The second solvent is water; Preferably, the amount of each component is such that in the catalyst slurry, the content of the active material precursor is 4-35% by weight, more preferably 8-20% by weight, the content of the oxygen storage material is 0.5-4% by weight, more preferably 1-3% by weight, and the content of the binder is 1-3% by weight, more preferably 1.5-2.5% by weight.
5. The method according to claim 1, wherein: In step (2), the grinding method is ball milling; Preferably, the grinding conditions are such that the average diameter of particles of the catalyst slurry is less than 15 μm, preferably 2-11 μm.
6. The catalyst slurry prepared by the method according to any one of claims 1 to 5.
7. A method for preparing a VOCs catalytic oxidation catalyst, characterized in that: The method comprises loading the catalyst slurry according to claim 6 onto a carrier, and then drying and calcining the carrier to obtain a VOCs catalytic oxidation catalyst; Preferably, the catalyst slurry loading is such that the loading of the catalyst layer is 20-140 g / L, more preferably 30-100 g / L, based on the volume of the carrier; Preferably, the drying conditions include: temperature of 80-140°C and time of 0.5-4h; Preferably, the calcination conditions include: the calcination atmosphere is an ozone atmosphere, the calcination temperature is 150-300° C., and the calcination time is 1-3 hours.
8. The method according to claim 7, wherein: The carrier is a regular structure carrier, Preferably, the cross-section of the carrier has a pore density of 50-400 pores / square inch and an open porosity of 20-80%; Preferably, the carrier is selected from at least one of cordierite, mullite, diamond, corundum, zirconium corundum, quartz, nepheline, feldspar, alumina and metal alloys.
9. The VOCs catalytic oxidation catalyst prepared according to the method of claim 7 or 8.
10. Use of the catalyst slurry according to claim 6 or the VOCs catalytic oxidation catalyst according to claim 9 in catalytic oxidation of VOCs.
Citation Information
Patent Citations
Precatalyst and its preparation method
CN100998941A
Preparation method of ruthenium and cerium co-doped tin-based catalyst for low-temperature catalytic combustion of chloroethylene and product and application of ruthenium and cerium co-doped tin-based catalyst
CN109395730A
Preparation method of catalyst slurry, catalyst slurry, catalyst element and catalytic module
CN112742438A
Carried noble metal complete-combustion catalyst and its prepn
CN1332035A
Exhaust-gas purification catalyst to be used close to the engine and process for its production
US20020039549A1