CuZnAl-LDO / CeO2 catalyst as well as preparation method and application thereof

By doping the Ce element on the CuZnAl-LDH support and using the supercritical hydrothermal method to prepare the CuZnAl-LDO/CeO2 catalyst, the problem of insufficient active sites of CeO2 nanoparticles in the field of photothermal catalysis was solved, and the catalytic efficiency and selectivity were improved. , achieving efficient photothermal catalysis effect.

CN118847129AActive Publication Date: 2024-10-29SHAANXI UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410872587.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-29
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

The development of existing CeO2 nanoparticles in the field of photothermal catalysis is limited by a single electron transmission path and insufficient active sites, resulting in low catalytic efficiency. In addition, the particle size distribution prepared by the hydrothermal method is wide, resulting in a reduction in the binding contact surface of active components. .

Method used

By doping the Ce element on the CuZnAl-LDH carrier, the CeO2 nanoparticles are evenly dispersed on the CuZnAl-LDO nanophotothermal catalyst using the supercritical hydrothermal method to form a CuZnAl-LDO/CeO2 catalyst, which increases active sites and promotes electron transfer. .

Benefits of technology

It improves the catalytic activity of the catalyst for photothermal hydrogenation reduction of CO2, enhances visible light absorption and carrier separation, achieves a selectivity of 99% for CO, reduces thermal conductivity, and improves solar energy utilization efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847129A_ABST
    Figure CN118847129A_ABST
Patent Text Reader

Abstract

The invention provides a CuZnAl-LDO / CeO2 catalyst as well as a preparation method and application thereof, and belongs to the technical field of nano material preparation. A preparation method of a CuZnAl-LDO / CeO2 catalyst comprises the following steps: dispersing a zinc source, a copper source and an aluminum source into water, uniformly mixing to obtain a mixed solution, mixing the mixed solution with ammonia water, carrying out a co-precipitation reaction, and cleaning after the reaction is finished to obtain a ternary LDH precursor solution; a ternary LDH precursor solution and an alkaline solution containing Ce ions are subjected to a supercritical hydrothermal reaction, in the reaction process, an LDO sheet layer is obtained through the oxidation effect of LDH, and a CeO2 nano-particle structure is attached to the LDO sheet layer to obtain the CuZnAl-LDO / CeO2 catalyst. The Ce element is loaded on the LDO carrier, the number of active sites is increased, and the catalytic performance is improved through the synergistic effect of CeO2 and LDO.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nano material preparation, and more specifically to a CuZnAl-LDO / CeO2 catalyst and a preparation method and application thereof. Background Art

[0002] Precious metal-based photothermal catalytic materials have a high efficiency in catalytic reduction of CO2, but the catalytic cost is high, which is not conducive to long-term industrial use. Therefore, it is urgent to design efficient non-precious metal-based photothermal catalytic materials. Layered double hydroxides (LDHs), commonly known as hydrotalcites, are simple to prepare and require abundant resources. LDHs layers have rich physical and chemical properties (such as acid-base catalysis, redox properties, photoelectric functions, etc.) due to their diversity of composition, exchangeability of interlayer anions, and compatibility with other materials, especially organic and biological materials. Using LDHs materials as a single precursor, catalytic materials with highly dispersed active sites and adjustable composition can be prepared through layer peeling, lattice confinement, intercalation assembly and arraying.

[0003] Cerium dioxide (CeO2) is a rare earth metal oxide with rich oxygen migration ability. 3+ and Ce 4+ The flexible transition of Ce valence states between CeO2 and CeO2 makes it very popular. Studies have shown that rare earth CeO2 defects rich in oxygen vacancies greatly promote the charge transfer process in photothermal catalytic reactions. And metal nanoparticles can shorten the free path of free electrons, reduce the plasma operating frequency, and then improve the catalytic efficiency by scattering light absorption. However, the single electron transport pathway of CeO2 and insufficient active sites limit the development of CeO2 in the field of photothermal catalysis. Since CeO2 has few active sites and a large bandgap, the strategy of combining CeO2 with active components is often used to improve the activity of CeO2-based photothermal catalysts.

[0004] However, the CeO2 nanoparticles prepared by the general hydrothermal method often have a wide particle size distribution and secondary agglomeration, which greatly reduces the contact surface with the active components. Summary of the invention

[0005] In view of the above problems, the present invention provides a CuZnAl-LDO / CeO2 catalyst, a preparation method and an application thereof. The Ce element is loaded on a carrier of LDO to increase the number of active sites. The synergistic effect of CeO2 and LDO improves the catalytic performance.

[0006] The first object of the present invention is to provide a method for preparing a CuZnAl-LDO / CeO2 catalyst, comprising the following steps:

[0007] The zinc source, the copper source and the aluminum source are dispersed in water and mixed evenly to obtain a mixed solution, the mixed solution is mixed with ammonia water for coprecipitation reaction, and after the reaction is completed, the solution is washed to obtain a ternary LDH precursor solution;

[0008] The ternary LDH precursor solution and the alkaline solution containing Ce ions undergo a supercritical hydrothermal reaction. During the reaction, LDH itself is oxidized to obtain LDO sheets, and the structure of CeO2 nanoparticles attached above the LDO sheets obtains the CuZnAl-LDO / CeO2 catalyst.

[0009] In a preferred embodiment of the present invention, the amount of Ce ions added is 5%-20% of the molar amount of the zinc source. For example, the amount of Ce ions added is 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20% of the molar amount of the zinc source. However, it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, which will not be repeated here.

[0010] In a preferred embodiment of the present invention, the added amount of Ce ions is 10% of the molar amount of the zinc source.

[0011] In a preferred embodiment of the present invention, the preheating process of the supercritical hydrothermal reaction is preheating at 180°C-190°C for 10min-20min. For example, the preheating temperature is 180°C, 181°C, 182°C, 183°C, 184°C, 185°C, 186°C, 187°C, 188°C, 189°C or 190°C. The preheating time is 11min, 12min, 13min, 14min, 15min, 16min, 17min, 18min, 19min or 20min, etc. However, it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, so they will not be repeated here.

[0012] In a preferred embodiment of the present invention, the reaction is carried out at 300°C-400°C for 20min-25min after preheating. For example, the reaction temperature after preheating is 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C or 400°C. The reaction time after preheating is 20min, 21min, 22min, 23min, 24min or 25min, etc. However, it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, so they will not be repeated here.

[0013] In a preferred embodiment of the present invention, in the mixed solution, the molar ratio of the zinc source, the copper source and the aluminum source is 4-5:3-4:2-4. For example, the molar ratio of the zinc source, the copper source and the aluminum source is 4:4:2, 4:4:3, 4:4:4, 4.5:4:2, 4.5:4:3, 4.5:4:4, 5:4:2, 5:4:3, 5:4:4, 4:3:2, 4:3:3 or 4:3:4, etc., but is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, which will not be repeated here.

[0014] In a preferred embodiment of the present invention, the reaction temperature of the coprecipitation reaction is 60°C-70°C, and the reaction time is 16-20h. For example, the reaction temperature of the coprecipitation reaction is 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C or 70°C, etc. The reaction time is 16h, 17h, 18h, 19h or 20h, etc. However, it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, so they will not be repeated here.

[0015] The second object of the present invention is to provide a CuZnAl-LDO / CeO2 catalyst prepared by the above preparation method.

[0016] The third object of the present invention is to provide the use of the above-mentioned CuZnAl-LDO / CeO2 catalyst in photothermal catalytic reduction of CO2.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The present invention uses a supercritical hydrothermal method to react CuZnAl-LDH with Ce(OH)3, oxidizes LDH into bimetallic oxide (LDO) nanoparticles, and evenly disperses CeO2 nanoparticles on the CuZnAl-LDO nanophotothermal catalyst, thereby avoiding the problem of CeO2 nanoparticle agglomeration. LDO is combined with the active component CeO2, and the obtained photothermal catalyst CuZnAl-LDO / CeO2 effectively improves the transfer of electrons, enhances visible light absorption, reduces thermal conductivity, improves the utilization of solar energy, promotes the separation and transfer of photogenerated carriers, and then improves the catalytic activity of the photothermal hydrogenation reduction of CO2 of the catalyst, and the selectivity for CO is 99%. The one-step supercritical hydrothermal method used in the present invention is simple and has good repeatability. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A flow chart of preparing CuZnAl-LDO / CeO2 catalyst according to the present invention;

[0020] Figure 2XRD pattern (a) and TEM pattern (b) of CuZnAl-LDH prepared in the present invention;

[0021] Figure 3 XRD patterns (a) and TEM patterns (b) of the catalysts prepared in Examples 1 to 3 of the present invention and Comparative Example 1;

[0022] Figure 4 This is the photothermal catalytic performance diagram of CuZnAl-LDO / CeO2 catalyst. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] As described in the background art, the single electron transport pathway and insufficient active sites of CeO2 in the prior art limit the development of CeO2 in the field of photothermal catalysis.

[0025] Since CeO2 has few active sites and a large bandgap, the strategy of combining CeO2 with active components is often used to improve the activity of CeO2-based photothermal catalysts.

[0026] However, the prepared CeO2 nanoparticles often have a wide particle size distribution, secondary agglomeration, and the degree of agglomeration cannot be well controlled.

[0027] Therefore, the present invention composites CeO2 and CuZnAl hydrotalcite through supercritical hydrothermal treatment, so that CeO2 can be evenly dispersed on CuZnAl nanoparticles, and the composite of CeO2 and CuZnAl can improve the catalytic performance.

[0028] The present invention provides a method for preparing a CuZnAl-LDO / CeO2 catalyst, such as Figure 1 As shown, the following steps are included:

[0029] The zinc source, the copper source and the aluminum source are dispersed in water and mixed evenly to obtain a mixed solution, the mixed solution is mixed with ammonia water for coprecipitation reaction, and after the reaction is completed, the solution is washed to obtain a ternary LDH precursor solution;

[0030] The ternary LDH precursor solution and the alkaline solution containing Ce ions underwent supercritical hydrothermal reaction to obtain the CuZnAl-LDO / CeO2 catalyst.

[0031] Supercritical fluid has the characteristics of both liquid and gas phases. It has more voids than ordinary fluids and is highly compressible. This makes supercritical fluids have low viscosity, high density, low surface tension, and good flow, diffusion, penetration, mass transfer, heat transfer and other characteristics. The density of the fluid can be changed by adjusting the pressure, temperature or both at the same time, and then the solvation ability of the fluid can be converted and adjusted from gas-like to liquid-like. The inventor used supercritical water to thin and peel the LDH layer and the oxidation of LDH itself at high temperature to obtain LDO layer. The structure of CeO2 nanoparticles attached to the top of the LDO layer greatly increases the number of active sites; CeO2 doping can provide oxygen vacancies and synergistic effects with LDO to generate electrons, change its electronic structure, accelerate electron transfer, accelerate the adsorption of intermediates and the desorption of products. The present invention has low cost and short synthesis time, and fully utilizes the advantages of the hydrothermal system.

[0032] The present invention has no particular restrictions on the types of compounds of the zinc source, copper source, and aluminum source, as long as the compounds of the zinc source, copper source, and aluminum source can be provided. Those skilled in the art can select well-known zinc source, copper source, and aluminum source related compounds according to actual application conditions. The zinc source used in the present invention is zinc nitrate, the copper source is copper nitrate, and the aluminum source is aluminum nitrate. It is understood that the zinc source, copper source, and aluminum source can also use corresponding hydrochlorides, chlorides, sulfates, hydrochlorides, acetates, etc.

[0033] In order to form a stable LDH and obtain a ternary LDH precursor solution, the trivalent element needs to account for 0.2 to 0.33 of the sum of the divalent element and the trivalent element. Therefore, the molar ratio of the zinc source, the copper source and the aluminum source in the mixed solution A is further limited to 4-5:3-4:2-4.

[0034] The purpose of adding ammonia water is to fully precipitate CuZnAl, so the amount of ammonia water added is sufficient to completely precipitate the zinc source, copper source and aluminum source. The ammonia water used in the present invention is ammonia water with a concentration of 28%.

[0035] The reaction temperature of the coprecipitation reaction is 60°C-70°C, and the reaction time is 16h-20h.

[0036] The amount of Ce ions added is 5%-20% of the molar amount of the zinc source. The active sites of LDH are mainly edges and defects. The tightly stacked structure prevents it from exposing more active sites. By introducing Ce elements, lattice distortion is generated, which can increase defects and oxygen vacancies. The electronic structure of LDO is adjusted, the electron transfer ability is enhanced, and thus the catalytic activity is enhanced.

[0037] The supercritical hydrothermal reaction is preheated at 180° C.-190° C. for 10 min-20 min, and then reacted at 300° C.-400° C. for 20 min-25 min. The present invention uses temperature to control the start time and speed of LDH structure formation.

[0038] The CuZnAl-LDO / CeO2 catalyst prepared by the present invention can be used for photothermal hydrogenation reduction of CO2. The CuZnAl-LDO / CeO2 catalyst effectively improves the transfer of electrons, enhances visible light absorption, reduces thermal conductivity, improves the utilization of solar energy, promotes the separation and transfer of photogenerated carriers, and thus improves the catalytic activity of the catalyst.

[0039] Example 1

[0040] Step 1: Ce(NO3)3·6H2O particles are fully dissolved in deionized water and stirred to obtain a 25ml Ce(NO3)3·6H2O solution with a concentration of 0.1mol / L. 75ml of NaOH solution with a concentration of 0.3mol / L is added dropwise to the Ce(NO3)3·6H2O solution. A magnetic stirrer is used to stir the solution during the titration process. After the titration, the solution is stirred for precipitation reaction and stirred for 18h to fully react. After the reaction is completed, the solution is repeatedly centrifuged and washed with water until the pH value of the supernatant in the centrifuge tube is approximately equal to 7, the attached materials on the centrifuge tube are dissolved, and the volume is fixed to 100mL to obtain an alkaline aqueous solution of Ce(OH)3.

[0041] Step 2. Weigh zinc nitrate, copper nitrate and aluminum nitrate in a molar ratio of 4:4:2, place them in a beaker and add 20 mL of deionized water with a pipette to obtain a liquid A with a total molar weight of 0.05 mol. Then measure 96 mL of deionized water in a round-bottom flask, add 4 mL of ammonia water to the flask with a pipette to obtain liquid B. Then set the magnetic stirrer parameters to 65°C and start heating. Use a dropper to drip liquid A into liquid B drop by drop at a rate of 5s / drop under rotor stirring conditions. Start timing from the time the first drop of liquid A is added to liquid B, and heat and stir to react for 18 hours. After the reaction is completed, wash it three times with deionized water and anhydrous ethanol in the order of water, ethanol, and water, transfer it to a volumetric flask and make up the volume to 100 mL to obtain an LDH precursor.

[0042] Step 3, take 10mL of the prepared LDH precursor in a stainless steel reactor. Add 0.2mL of Ce(OH)3 solution with Ce ions accounting for 5% of the molar amount of Zn element in the LDH precursor, and finally add deionized water to ensure that the liquid volume in the reactor is 20mL unchanged. The temperature of the homogeneous reactor is set to 180°C, and the temperature of the well-type swing furnace is set to 400°C. Install the reactor containing the precursor and Ce(OH)3, put it in the homogeneous reactor for preheating for 20min, and reduce the time required for the reaction system to heat up during the supercritical reaction. After the preheating is completed, the reactor is immediately transferred to the well-type swing furnace for supercritical reaction for 20min. After the reaction is completed, the reactor is placed in water for rapid cooling to obtain CuZnAl-LDO / CeO2 nanocomposite material. The product is centrifuged and washed 3 times with deionized water and anhydrous ethanol in the order of water, ethanol, and water. After cleaning, add an appropriate amount of anhydrous ethanol into the centrifuge tube, shake and disperse, and then dry in an oven to obtain a sample, which is recorded as 400°C-5Ce.

[0043] Example 2

[0044] Step 1: Ce(NO3)3·6H2O particles are fully dissolved in deionized water and stirred to obtain a 25ml Ce(NO3)3·6H2O solution with a concentration of 0.1mol / L. A NaOH solution with a concentration of 0.3mol / L is added dropwise to the Ce(NO3)3·6H2O solution. The titration process is stirred with a magnetic stirrer. After the titration, the stirring is continued to cause a precipitation reaction and stirred for 18h to fully react. After the reaction is completed, centrifuge and wash repeatedly until the pH value of the supernatant in the centrifuge tube is approximately equal to 7, so that the attachments on the centrifuge tube are dissolved, and the volume is fixed to 100mL to obtain an alkaline aqueous solution of Ce(OH)3.

[0045] Step 2. Weigh zinc nitrate, copper nitrate and aluminum nitrate in a molar ratio of 4:4:2, place them in a beaker and add 20 mL of deionized water with a pipette to obtain a solution A with a total molar weight of 0.05 mol. Then measure 96 mL of deionized water in a round-bottom flask, add 4 mL of ammonia water to the flask with a pipette to obtain a solution B. Then set the magnetic stirrer parameters to 65 ° C and start heating. Use a dropper to drip solution A into solution B drop by drop at a rate of 5 s / drop under rotor stirring conditions. Start timing from the time the first drop of solution A is added to solution B, and heat and stir to react for 18 hours. After the reaction is completed, wash it three times with deionized water and anhydrous ethanol in the order of water, ethanol, and water, transfer it to a volumetric flask and make up the volume to 100 mL to obtain an LDH precursor.

[0046] Step 3, take 10mL of the prepared LDH precursor in a stainless steel reactor. Add 0.4mL of Ce(OH)3 solution with Ce ions accounting for 10% of the molar amount of Zn element in the LDH precursor, and finally add deionized water to ensure that the liquid volume in the reactor is 20mL unchanged. The temperature of the homogeneous reactor is set to 180°C, and the temperature of the well-type swing furnace is set to 400°C. Install the reactor containing the precursor and Ce(OH)3, put it in the homogeneous reactor for preheating for 20min, and reduce the time required for the reaction system to heat up during the supercritical reaction. After the preheating is completed, the reactor is immediately transferred to the well-type swing furnace for supercritical reaction for 20min. After the reaction is completed, the reactor is placed in water for rapid cooling to obtain CuZnAl-LDO / CeO2 nanocomposite material. The product is centrifuged and washed 3 times with deionized water and anhydrous ethanol in the order of water, ethanol, and water. After cleaning, add an appropriate amount of anhydrous ethanol into the centrifuge tube, shake and disperse, and then dry in an oven to obtain a sample, which is recorded as 400°C-10Ce.

[0047] Example 3

[0048] Step 1: Ce(NO3)3·6H2O particles are fully dissolved in deionized water and stirred to obtain a 25ml Ce(NO3)3·6H2O solution with a concentration of 0.1mol / L. A NaOH solution with a concentration of 0.3mol / L is added dropwise to the Ce(NO3)3·6H2O solution. The titration process is stirred with a magnetic stirrer. After the titration, the stirring is continued to cause a precipitation reaction and stirred for 18h to fully react. After the reaction is completed, centrifuge and wash repeatedly until the pH value of the supernatant in the centrifuge tube is approximately equal to 7, so that the attachments on the centrifuge tube are dissolved, and the volume is fixed to 100mL to obtain an alkaline aqueous solution of Ce(OH)3.

[0049] Step 2. Weigh zinc nitrate, copper nitrate and aluminum nitrate in a molar ratio of 4:4:2, place them in a beaker and add 20 mL of deionized water with a pipette to obtain a solution A with a total molar weight of 0.05 mol. Then measure 96 mL of deionized water in a round-bottom flask, add 4 mL of ammonia water to the flask with a pipette to obtain a solution B. Then set the magnetic stirrer parameters to 65 ° C and start heating. Use a dropper to drip solution A into solution B drop by drop at a rate of 5 s / drop under rotor stirring conditions. Start timing from the time the first drop of solution A is added to solution B, and heat and stir to react for 18 hours. After the reaction is completed, wash it three times with deionized water and anhydrous ethanol in the order of water, ethanol, and water, transfer it to a volumetric flask and make up the volume to 100 mL to obtain an LDH precursor.

[0050] Step 3, take 10mL of the prepared LDH precursor in a stainless steel reactor. Add 0.8mL of Ce(OH)3 solution with Ce ions accounting for 20% of the molar amount of Zn element in the LDH precursor, and finally add deionized water to ensure that the liquid volume in the reactor is 20mL unchanged. The temperature of the homogeneous reactor is set to 180°C, and the temperature of the well-type swing furnace is set to 400°C. Install the reactor containing the precursor and Ce(OH)3, put it in the homogeneous reactor for preheating for 20min, and reduce the time required for the reaction system to heat up during the supercritical reaction. After the preheating is completed, the reactor is immediately transferred to the well-type swing furnace for supercritical reaction for 20min. After the reaction is completed, the reactor is placed in water for rapid cooling to obtain CuZnAl-LDO / CeO2 nanocomposite material. The product is centrifuged and washed 3 times with deionized water and anhydrous ethanol in the order of water, ethanol, and water. After cleaning, add an appropriate amount of anhydrous ethanol into the centrifuge tube, shake and disperse, and then dry in an oven to obtain a sample, which is recorded as 400°C-20Ce.

[0051] Example 4

[0052] Step 1: Ce(NO3)3·6H2O particles are fully dissolved in deionized water and stirred to obtain a 25ml Ce(NO3)3·6H2O solution with a concentration of 0.1mol / L. A NaOH solution with a concentration of 0.3mol / L is added dropwise to the Ce(NO3)3·6H2O solution. The titration process is stirred with a magnetic stirrer. After the titration, the stirring is continued to cause a precipitation reaction and stirred for 18h to fully react. After the reaction is completed, centrifuge and wash repeatedly until the pH value of the supernatant in the centrifuge tube is approximately equal to 7, so that the attachments on the centrifuge tube are dissolved, and the volume is fixed to 100mL to obtain an alkaline aqueous solution of Ce(OH)3.

[0053] Step 2. Weigh zinc nitrate, copper nitrate and aluminum nitrate in a molar ratio of 4:4:2, place them in a beaker and add 20 mL of deionized water with a pipette to obtain a solution A with a total molar weight of 0.05 mol. Then measure 96 mL of deionized water in a round-bottom flask, add 4 mL of ammonia water to the flask with a pipette to obtain a solution B. Then set the magnetic stirrer parameters to 65 ° C and start heating. Use a dropper to drip solution A into solution B drop by drop at a rate of 5 s / drop under rotor stirring conditions. Start timing from the time the first drop of solution A is added to solution B, and heat and stir to react for 18 hours. After the reaction is completed, wash it three times with deionized water and anhydrous ethanol in the order of water, ethanol, and water, transfer it to a volumetric flask and make up the volume to 100 mL to obtain an LDH precursor.

[0054] Step 3, take 10mL of the prepared LDH precursor in a stainless steel reactor. Add 0.4mL of Ce(OH)3 solution with Ce ions accounting for 10% of the molar amount of Zn element in the LDH precursor, and finally add deionized water to ensure that the liquid volume in the reactor is 20mL unchanged. The temperature of the homogeneous reactor is set to 180°C, and the temperature of the well-type swing furnace is set to 300°C. Install the reactor containing the precursor and Ce(OH)3, put it in the homogeneous reactor for preheating for 20min, and reduce the time required for the reaction system to heat up during the supercritical reaction. After the preheating is completed, the reactor is immediately transferred to the well-type swing furnace for supercritical reaction for 20min. After the reaction is completed, the reactor is placed in water for rapid cooling to obtain CuZnAl-LDO / CeO2 nanocomposite material. The product is centrifuged and washed 3 times with deionized water and anhydrous ethanol in the order of water, ethanol, and water. After cleaning, add an appropriate amount of anhydrous ethanol into the centrifuge tube, shake and disperse, and then dry in an oven to obtain a sample, which is recorded as 300°C-10Ce.

[0055] Example 5

[0056] Step 1: Ce(NO3)3·6H2O particles are fully dissolved in deionized water and stirred to obtain a 25ml Ce(NO3)3·6H2O solution with a concentration of 0.1mol / L. 75ml of NaOH solution with a concentration of 0.3mol / L is added dropwise to the Ce(NO3)3·6H2O solution. A magnetic stirrer is used to stir the solution during the titration process. After the titration, the solution is stirred for precipitation reaction and stirred for 18h to fully react. After the reaction is completed, the solution is repeatedly centrifuged and washed with water until the pH value of the supernatant in the centrifuge tube is approximately equal to 7, the attached materials on the centrifuge tube are dissolved, and the volume is fixed to 100mL to obtain an alkaline aqueous solution of Ce(OH)3.

[0057] Step 2. Weigh zinc nitrate, copper nitrate and aluminum nitrate in a molar ratio of 5:3:4, place them in a beaker and add 20 mL of deionized water with a pipette to obtain a liquid A with a total molar weight of 0.05 mol. Then measure 96 mL of deionized water in a round-bottom flask, add 4 mL of ammonia water to the flask with a pipette to obtain liquid B. Then set the magnetic stirrer parameters to 60°C and start heating. Use a dropper to drip liquid A into liquid B drop by drop at a rate of 5s / drop under rotor stirring conditions. Start timing from the time the first drop of liquid A is added to liquid B, and heat and stir to react for 20 hours. After the reaction is completed, wash it three times with deionized water and anhydrous ethanol in the order of water, ethanol, and water, transfer it to a volumetric flask and make up the volume to 100 mL to obtain an LDH precursor.

[0058] Step 3, take 10mL of the prepared LDH precursor in a stainless steel reactor. Add 0.4mL of Ce(OH)3 solution with Ce ions accounting for 10% of the molar amount of Zn element in the LDH precursor, and finally add deionized water to ensure that the liquid volume in the reactor is 20mL unchanged. The temperature of the homogeneous reactor is set to 190°C, and the temperature of the well-type swing furnace is set to 350°C. Install the reactor containing the precursor and Ce(OH)3, put it into the homogeneous reactor for preheating for 10min, and reduce the time required for the reaction system to heat up during the supercritical reaction. After the preheating is completed, the reactor is immediately transferred to the well-type swing furnace for supercritical reaction for 23min. After the reaction is completed, the reactor is placed in water for rapid cooling to obtain CuZnAl-LDO / CeO2 nanocomposite materials. The product is centrifuged and washed three times with deionized water and anhydrous ethanol in the order of water, ethanol, and water. After washing, add an appropriate amount of anhydrous ethanol to the centrifuge tube, shake and disperse it, and dry it in an oven to obtain a sample.

[0059] Example 6

[0060] Step 1: Ce(NO3)3·6H2O particles are fully dissolved in deionized water and stirred to obtain a 25ml Ce(NO3)3·6H2O solution with a concentration of 0.1mol / L. A NaOH solution with a concentration of 0.3mol / L is added dropwise to the Ce(NO3)3·6H2O solution. The titration process is stirred with a magnetic stirrer. After the titration, the stirring is continued to cause a precipitation reaction and stirred for 18h to fully react. After the reaction is completed, centrifuge and wash repeatedly until the pH value of the supernatant in the centrifuge tube is approximately equal to 7, so that the attachments on the centrifuge tube are dissolved, and the volume is fixed to 100mL to obtain an alkaline aqueous solution of Ce(OH)3.

[0061] Step 2. Weigh zinc nitrate, copper nitrate and aluminum nitrate in a molar ratio of 4.5:3.5:3, place them in a beaker and add 20 mL of deionized water with a pipette to obtain a liquid A with a total molar weight of 0.05 mol. Then measure 96 mL of deionized water in a round-bottom flask, add 4 mL of ammonia water to the flask with a pipette to obtain liquid B. Then set the magnetic stirrer parameters to 60°C and start heating. Use a dropper to add liquid A dropwise into liquid B at a rate of 5s / drop under rotor stirring conditions. Start timing from the time the first drop of liquid A is added to liquid B, and heat and stir to react for 20 hours. After the reaction is completed, wash it three times with deionized water and anhydrous ethanol in the order of water, ethanol, and water, transfer it to a volumetric flask and make up the volume to 100 mL to obtain an LDH precursor.

[0062] Step 3, take 10mL of the prepared LDH precursor in a stainless steel reactor. Add 0.4mL of Ce(OH)3 solution with Ce ions accounting for 10% of the molar amount of Zn element in the LDH precursor, and finally add deionized water to ensure that the liquid volume in the reactor is 20mL unchanged. The temperature of the homogeneous reactor is set to 185°C, and the temperature of the well-type swing furnace is set to 400°C. Install the reactor containing the precursor and Ce(OH)3, put it into the homogeneous reactor for preheating for 15min, and reduce the time required for the reaction system to heat up during the supercritical reaction. After the preheating is completed, the reactor is immediately transferred to the well-type swing furnace for supercritical reaction for 25min. After the reaction is completed, the reactor is placed in water for rapid cooling to obtain CuZnAl-LDO / CeO2 nanocomposite materials. The product is centrifuged and washed three times with deionized water and anhydrous ethanol in the order of water, ethanol, and water. After washing, add an appropriate amount of anhydrous ethanol to the centrifuge tube, shake and disperse it, and dry it in an oven to obtain a sample.

[0063] Comparative Example 1

[0064] Step 1: Ce(NO3)3·6H2O particles are fully dissolved in deionized water and stirred to obtain a 25ml Ce(NO3)3·6H2O solution with a concentration of 0.1mol / L. 75ml of NaOH solution with a concentration of 0.3mol / L is added dropwise to the Ce(NO3)3·6H2O solution. The titration process is stirred with a magnetic stirrer. After the titration, the stirring is continued to cause a precipitation reaction and stirred for 18h to fully react. After the reaction is completed, the solution is repeatedly centrifuged and washed with water. The pH value of the supernatant in the centrifuge tube is approximately equal to 7. The attachments on the centrifuge tube are dissolved and the volume is fixed to 100mL to obtain an alkaline aqueous solution of Ce(OH)3.

[0065] Step 2, weigh zinc nitrate, copper nitrate, and aluminum nitrate in a molar ratio of 4:4:2, place them in a beaker, and then add 20mL of deionized water with a pipette to obtain a liquid A with a total molar weight of 0.05mol. Then measure 96mL of deionized water in a round-bottom flask, and add 4mL of ammonia water to the flask with a pipette to obtain liquid B. Then set the magnetic stirrer parameters to 65℃ and start heating. Use a dropper to drip liquid A into liquid B drop by drop at a speed of 5s / drop under rotor stirring conditions. Start timing from the time the first drop of liquid A is added to liquid B, and heat and stir to react for 18h. After the reaction is completed, wash it with deionized water and anhydrous ethanol in the order of water, ethanol, and water for 3 times, and transfer it to a volumetric flask and adjust the volume to 100mL. Finally, a water-based ternary LDH precursor with a molar ratio of Zn:Cu:Al of 4:4:2 is obtained.

[0066] Step 3, take 10mL of the prepared LDH precursor in a stainless steel reactor, add deionized water, and ensure that the liquid volume in the reactor is 20mL unchanged. The temperature of the homogeneous reactor is set to 180°C, and the temperature of the well-type swing furnace is set to 400°C. The reactor containing the precursor and Ce(OH)3 is installed, placed in the homogeneous reactor for preheating for 20min, and the time required for the reaction system to heat up during the supercritical reaction is reduced. After the preheating is completed, the reactor is immediately transferred to the well-type swing furnace for supercritical reaction for 20min. After the reaction is completed, the reactor is placed in water and cooled rapidly to obtain a CuZnAl-LDO / -0CeO2 nanocomposite material. The product is centrifuged and washed 3 times with deionized water and anhydrous ethanol in the order of water, ethanol, and water. After the cleaning is completed, an appropriate amount of anhydrous ethanol is added to the centrifuge tube, and the sample is dried in an oven after being dispersed by shaking to obtain a sample, which is recorded as LDO-0Ce.

[0067] Figure 2 The XRD pattern (a) and TEM pattern (b) of CuZnAl-LDH prepared by the present invention are shown in FIG. Figure 2 In Figure a, it can be seen that the peaks of 11.7°, 23.5°, 34.8°, 39.2° and 46.8° shown in the XRD correspond to the (003), (006), (012), (015) and (018) crystal planes of LDH, respectively. It can be seen that the peaks of LDH are very obvious and have not shifted. Figure 2 Figure b shows that the prepared LDH is a complete hexagonal flake. It should be noted that CuZnAl-LDH refers to the LDH precursor prepared in step 2 of Example 1. Since the preparation methods and preparation parameters of step 2 of Example 1 to Example 3 are the same, only the XRD pattern of the LDH precursor of Example 1 is measured.

[0068] Figure 3 The XRD patterns (a) and TEM patterns (b) of the catalysts prepared in Examples 1 to 3 of the present invention and Comparative Example 1 are shown in Table 1. Figure 3 Figure a shows that the characteristic peak of CeO2 appears in XRD and LDH has been oxidized to LDO. Figure 3 Figure b shows that CeO2 nanoparticles are evenly dispersed on LDO with little agglomeration. In general, as the Ce content increases, the Ce element is first evenly dispersed on the LDO carrier, improving the interface electronic state of LDO and improving the catalytic performance. However, as the Ce doping increases further, the formation energy of Ce to form a high oxidation state increases, resulting in a decrease in active sites, thereby reducing the catalytic performance.

[0069] Figure 4 The performance of CuZnAl-LDO / CeO2 catalyst for photothermal catalytic CO2 hydrogenation to CO is shown in Figure 2. Figure 4It can be seen that the selectivity of the catalyst for CO is as high as 99%, and the catalytic performance is improved after compounding with CeO2, among which the photothermal catalytic activity of 300℃-10Ce is the best.

[0070] The invention has low cost and short synthesis time, and fully utilizes the advantages of the hydrothermal system. The supercritical one-step hydrothermal method is used to compound CeO2 nanoparticles of uniform size with CuZnAl-LDO to obtain the photothermal catalyst CuZnAl-LDO / CeO2, which effectively improves the transfer of electrons, enhances visible light absorption, reduces thermal conductivity, improves the utilization of solar energy, promotes the separation and transfer of photogenerated carriers, and thus improves the catalytic activity of the photothermal hydrogenation reduction of CO2 of the catalyst, and the selectivity for CO is 99%. The one-step supercritical hydrothermal method is simple and has good repeatability.

[0071] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0072] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A CuZnAl-LDO / CeO 2 A method for preparing a catalyst, It is characterized in that The following steps are involved: The zinc source, the copper source and the aluminum source are dispersed in water and mixed evenly to obtain a mixed solution, the mixed solution is mixed with ammonia water for coprecipitation reaction, and after the reaction is completed, the solution is washed to obtain a ternary LDH precursor solution; The ternary LDH precursor solution and the alkaline solution containing Ce ions undergo supercritical hydrothermal reaction. During the reaction, LDH itself is oxidized to obtain LDO sheets, and CeO is attached to the top of the LDO sheets. 2 The structure of nanoparticles was obtained by CuZnAl-LDO / CeO 2 catalyst.

2. A CuZnAl-LDO / CeO according to claim 1 2 A method for preparing a catalyst, It is characterized in that The amount of Ce ions added is 5% to 20% of the molar amount of the zinc source.

3. A CuZnAl-LDO / CeO according to claim 1 2 A method for preparing a catalyst, It is characterized in that The amount of Ce ions added was 10% of the molar amount of the zinc source.

4. A CuZnAl-LDO / CeO according to claim 1 2 A method for preparing a catalyst, It is characterized in that The preheating process of the supercritical hydrothermal reaction is to preheat at 180°C-190°C for 10min-20min.

5. A CuZnAl-LDO / CeO according to claim 4 2 A method for preparing a catalyst, It is characterized in that After preheating, react at 300°C-400°C for 20min-25min.

6. The CuZnAl-LDO / CeO according to claim 1 2 A method for preparing a catalyst, It is characterized in that In the mixed solution, the molar ratio of the zinc source, the copper source and the aluminum source is 4-5:3-4:2-4.

7. The CuZnAl-LDO / CeO according to claim 1 2 A method for preparing a catalyst, It is characterized in that The reaction temperature of the coprecipitation reaction is 60°C-70°C, and the reaction time is 16h-20h.

8. A CuZnAl-LDO / CeO prepared by the preparation method according to any one of claims 1 to 7 2 catalyst.

9. The CuZnAl-LDO / CeO according to claim 8 2 Catalysts for photothermal catalytic reduction of CO 2 Application in.

Citation Information

Patent Citations

  • Preparation method for depositing cerium dioxide on carbon nano-tube in overcritical water

    CN101054662A

  • Ternary composite metal oxide solid alkali catalyst and preparation method and application thereof

    CN109621939A

  • Cerium oxide-hydrotalcite composite catalyst as well as preparation method and application thereof

    CN111167432A

  • Rare-earth-based hydrotalcite adsorbent for removing phosphorus from wastewater and preparation method of rare-earth-based hydrotalcite adsorbent

    CN116943601A

  • Lanthanide-doped layered double hydroxides and method of producing same

    US20200325031A1