Method for manufacturing light-weight frame component by adopting liquid forging and pipe drawing process and frame component
Through liquid forging and pipe drawing technology combined with CNC machining, the problem of low mold durability and loose material in gravity casting of electric vehicle frame components has been solved, and the manufacturing of lightweight, high-strength and high-precision frame components has been achieved, reducing production costs. cost and improves the overall performance of the product.
Patent Information
- Application Number
- CN202411006389.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-29
AI Technical Summary
Existing electric vehicle frame components manufactured through gravity casting have problems with low mold durability, rough surfaces, loose materials and pinholes, resulting in increased product weight, high cost, insufficient strength and durability, and affecting the overall performance and safety of electric vehicles. .
Liquid forging and pipe drawing processes are used to produce lightweight frame components. Complex shapes are formed through liquid forging. The pipe drawing process is designed to have differentiated thicknesses at different stress-bearing positions. This is combined with CNC machining and hydraulic water-expansion molds to achieve precise material utilization and high strength. .
It achieves lightweight, high strength and high precision of frame components, extends the service life of the mold, reduces production costs, and improves the overall stability and durability of the product.
Smart Images

Figure CN118847749A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electric bicycle component forming, and in particular to a method for manufacturing a lightweight frame component by using liquid forging and tube drawing processes, and a frame component. Background Art
[0002] The frame components of electric vehicles include the head tube, down tube, motor seat, etc., which are key parts of the overall structure of electric vehicles. Gravity casting is usually used for one-piece molding. This method can achieve one-time molding of components and simplify the production process. However, gravity casting has some inherent defects, such as the low durability of the mold, which is prone to cracks under the impact of high-temperature molten liquid, shortening the service life of the mold. The surface of the casting is prone to roughness and unevenness, increasing the subsequent processing and handling costs. In addition, gravity casting leads to loose materials and pinhole problems, which will reduce the strength and durability of the casting and affect the overall performance and safety of the electric vehicle.
[0003] In order to improve the strength of the casting, the traditional approach is to increase the thickness of the product or design reinforcement ribs, resulting in a weight of about 5kg. The finished vehicle is heavy, which not only violates the original intention of lightweight design of electric vehicles, but also causes waste of materials. The mold is not durable, and a new mold needs to be replaced after 10,000 to 15,000 pieces, which is expensive. At the same time, this also means that more polishing and inspection work is required, further increasing production costs. Summary of the invention
[0004] In order to solve the above problems, the present application provides a method for manufacturing a lightweight frame component by using liquid forging and tube drawing process and a frame component.
[0005] The present application provides a method for manufacturing lightweight frame components using liquid forging and tube drawing processes, which adopts the following technical solutions: A method for manufacturing a lightweight frame component by using a liquid forging and tube drawing process comprises the following steps: Liquid forging is used to make a tube blank, the head end of the tube blank is formed into a head tube, the middle part is the base of the down tube, and the tail end is set in a circular shape, which is the base of the motor seat; The middle and tail ends of the tube are drawn out to make the middle and tail ends of the tube longer and thinner, and different wall thicknesses are processed at different stress positions; Expand the tail end of the tube to increase the outer diameter of the tail end of the tube; The tail end of the tube billet away from the middle of the tube billet is subjected to tube shrinkage treatment to achieve a reduced diameter of the port; The tail end of the tube is flattened to make the entire cross section of the tail end of the tube into an elliptical structure; The tail end of the tube billet is shifted to achieve flattening of the tail end of the tube billet; Perform bending and shaping treatment on the tail end of the tube blank; Performing forming treatment on the tube blank after bending and shaping; The formed tube blank is subjected to CNC machining to obtain the final product.
[0006] By adopting the above technical solutions, liquid forging can more easily form the complex shape of the head tube than frame parts manufactured by gravity casting. The pipe drawing process uses differentiated thickness design to use thicker materials only where needed, achieving precise use of materials, thereby reducing weight and saving materials. This process is suitable for the manufacture of frame parts that require high strength and lightness. The pipe drawing process makes the product surface smooth and reduces polishing costs. The use of hydraulic water expansion molds and CNC machining technology improves the accuracy and standardization of products. The mold is durable, reducing the frequency and cost of replacement; the material has a compact crystal structure, which improves the overall strength of the product.
[0007] Optionally, the step of bending and shaping the tail end of the tube blank includes: Perform a bending process on the tail end of the tube billet to make the bottom surface of the tail end of the tube billet concave, thus achieving a bending process on the tail end of the tube billet; The tail end of the tube billet is subjected to a secondary bending process to raise the end of the tube billet relative to the middle of the tube billet, thereby achieving secondary bending of the tail end of the tube billet.
[0008] By adopting the above technical solution, one bending process forms the initial bend, and the second bending process forms a more refined and complex tube shape. Through the two bending processes, the tail end of the tube can be given the desired spatial shape and functional characteristics.
[0009] Optionally, the step of forming the entire tube blank after bending and shaping includes: The tube blank after bending and shaping is subjected to water sealing process; The tube blank is subjected to a hydraulic forming process to achieve the overall forming of the tube blank.
[0010] By adopting the above technical solution, the pipe blank after bending and shaping is subjected to a water sealing process to realize pre-forming operation. Hydraulic forming helps to improve product accuracy and standardize products.
[0011] Optionally, in the step of drawing the tube from the middle and tail end of the tube blank, the tube drawing process is used to make the wall thickness range of the middle part of the tube blank be: 2±0.5mm, and the wall thickness range of the tail end of the tube blank be: 3.5±0.5mm.
[0012] By adopting the above technical solution, by processing different wall thicknesses at different stress-bearing positions and differentiated wall thickness design, it can be ensured that the material has sufficient thickness where high-strength support is required, while the wall thickness can be reduced in places where it does not need to bear greater forces, thereby reducing the overall weight.
[0013] Optionally, the outer diameter range of one end of the tube head end close to the middle of the tube is: 105±5mm, and in the step of expanding the tube tail end, the tube expansion process is used to make the outer diameter range of the tube tail end: 135±5mm.
[0014] By adopting the above technical solution, the size of the tail end of the tube blank can be effectively changed through the tube expansion process to match a motor or other drive component with a larger diameter.
[0015] Optionally, in the step of performing tube shrinkage treatment on the portion of the tube billet tail end away from the tube billet middle portion, the tube shrinkage process is used to make the outer diameter range of the tube billet tail end port be: 105±5mm.
[0016] By adopting the above technical solution, the tube shrinking process allows the tail end of the tube blank to form a wrapping space for the motor. The tube shrinking can enhance the local stiffness and strength of the tube port, and enhance its durability and reliability.
[0017] Optionally, the fillet radius value of the corner at the middle of the tail end of the tube blank is: 60±5mm; the fillet radius value of the corner at the tail end of the tube blank close to the middle of the tube blank is: 28.7±5mm.
[0018] The adoption of the above technical solution helps to smooth stress distribution, reduce stress concentration, and thus increase the fatigue life of the tube blank.
[0019] Optionally, the angle value of the corner in the middle of the tail end of the tube blank is: 107±5°.
[0020] By adopting the above technical solution, a suitable accommodation space is provided for the motor.
[0021] Optionally, the angle value of the corner at the tail end of the tube billet close to the middle of the tube billet is: 136±5°.
[0022] By adopting the above technical solutions, it is helpful to optimize the stress distribution of the tube blank, reduce stress concentration points, thereby reducing the risk of cracks and fractures, and help improve the overall stability and load-bearing capacity of the frame components.
[0023] In a second aspect, the present application provides a frame component, which is manufactured by the method for manufacturing a lightweight frame component using liquid forging and tube drawing process as described above.
[0024] In summary, the present application includes at least one of the following beneficial technical effects: 1. Compared with frame parts made by gravity casting, liquid forging can more easily form the complex shape of the head tube. The pipe drawing process uses differentiated thickness design to use thicker materials only where needed, achieving precise use of materials, thereby reducing weight and saving materials. This process is suitable for the manufacture of frame parts that require high strength and lightness. The pipe drawing process makes the product surface smooth and reduces polishing costs; 2. Use hydraulic water-swelling molds and CNC processing technology to improve product precision and standardization. The mold is durable, reducing replacement frequency and cost; the material has a compact crystal structure, which improves the overall strength of the product; 3. The tail end of the tube is bent once to form the initial bend, and the second bending forms a more delicate and complex tube shape. The two bending shaping processes can give the tail end of the tube the required spatial shape and functional characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a schematic structural diagram of a frame component in an embodiment of the present invention; Figure 2 It is a schematic flow chart of the liquid forging, tube drawing-tube expansion-tube reduction process in the method for manufacturing a lightweight frame component by using the liquid forging and tube drawing process in an embodiment of the present invention; Figure 3 It is a schematic flow chart of the flattening-shifting-one-time bending process in the method for manufacturing a lightweight frame component by using liquid forging and pipe drawing process in an embodiment of the present invention; Figure 4 It is a flow chart of secondary bending-water sealing-hydraulic forming-CNC machining steps in a method for manufacturing lightweight frame components by liquid forging and tube drawing process in an embodiment of the present invention.
[0026] Explanation of reference numerals: 100, frame component; 1, head pipe; 11, upper pipe joint; 2, down pipe; 3, motor seat; 200, tube blank; 201, head end of tube blank; 202, middle part of tube blank; 203, tail end of tube blank. DETAILED DESCRIPTION
[0027] The following will be combined with the attached Figure 1-4 , the technical solutions in the embodiments of the present application are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0028] The embodiment of the present application discloses a method for manufacturing a lightweight frame component using a liquid forging and pipe drawing process and a frame component 100. The frame component 100 is manufactured by the method for manufacturing a lightweight frame component using a liquid forging and pipe drawing process. In order to better understand the method, the structure of the frame component 100 is first described in detail. Figure 1 The frame component 100 is integrally formed from a tube blank 200. The head end 201 of the frame component 100 is a head tube 1, the middle part is a down tube 2, and the tail end is a motor seat 3 for installing a motor. The head tube 1, the down tube 2 and the motor seat 3 are an integral structure, which can reduce material input while ensuring overall strength, and help save costs. The angle between the axis of the head tube 1 and the axis of the down tube 2 is an obtuse angle. The head tube 1 is integrally formed with an upper tube joint 11 near the outer side of the down tube 2. The upper tube joint 11 is located above the down tube 2, which is convenient for connecting the head tube 1 with the upper tube and ensuring overall strength after installation.
[0029] As an optional embodiment, the upper tube joint 11 is a square frame structure, and the square frame structure is connected to the inner cavity of the head tube 1, which is convenient for plugging the upper tube and the upper tube joint 11, and ensuring the stability of the connection between the upper tube and the head tube 1. The motor seat 3 is an arc-shaped half-tube structure, and a mounting cavity for placing the motor is formed inside. A hollow cavity is formed axially inside the lower tube 2, which can be used to install batteries, etc., and a window connected to the hollow cavity is opened on the wall of the lower tube 2, and a cover can be matched and installed at the window.
[0030] Further, see Figures 2 to 4 The method for manufacturing lightweight frame components by liquid forging and tube drawing process comprises the following steps: Reference Figure 2 (a), a tube blank 200 is made by liquid forging, the head end 201 of the tube blank is formed into a head tube 1, the middle part 202 is the base of the lower tube 2, and the tail end 203 is set in a circular shape, which is the base of the motor seat 3. The tube blank 200 is formed by liquid forging, and the head end 201 of the tube blank is directly formed into a head tube 1 structure, and the head tube 1 has an upper tube joint 11, etc. The structure is relatively complex. By utilizing the fluidity of liquid or semi-solid metal, the precise forming of complex shapes can be achieved through the mold. Liquid forging can be carried out at a lower strain rate, which helps to reduce defects such as holes and cracks inside the material, thereby improving the internal quality and mechanical properties of the product. Secondly, liquid forging can produce a finer grain structure, which helps to improve the strength and toughness of the material, especially in applications requiring high strength and high toughness. In addition, the metal fluidity of liquid forging is better, and it can be easier to fill the complex shape of the mold, thereby achieving more complex geometric shapes and finer dimensional accuracy.
[0031] The length of the tube blank 200 formed by liquid forging is 815.5 mm, the outer diameter of the head pipe 1 near the middle part 202 of the tube blank is 105 mm, and the wall thickness is 3.5 mm. The outer diameter gradually increases from the head of the tube blank 200 to the middle part 202, and the outer diameter transitions to the middle part 202 and the tail end 203 of the tube blank is 110 mm, and the wall thickness is 4 mm.
[0032] The tail end 203 of the formed tube blank is circular, which is convenient for the tube drawing process. Figure 2 (a), the middle part 202 and the tail end 203 of the tube blank are subjected to a tube extraction process, so that the length of the middle part 202 and the tail end 203 of the tube blank becomes longer and the wall thickness becomes thinner, and different wall thicknesses are processed at different stress positions. One end of the tube blank 200 is fixed on the tube extraction machine, and then the other end of the tube blank 200 is pulled through a mold with a smaller diameter by mechanical force, so that the wall thickness of the tube blank 200 gradually becomes thinner and the length increases accordingly. Through multiple tube extraction processes, the tube blank 200 can achieve different wall thicknesses at different stress positions, such as thickening at the stress point and thinning at the stress-free point, thereby optimizing the use efficiency and structural strength of the material. After the tube blank 200 undergoes the tube extraction process, the wall thickness range of the middle part 202 of the tube blank is: 2±0.5mm, and the wall thickness range of the tail end 203 of the tube blank is: 3.5±0.5mm. In this embodiment, the wall thickness of the middle part 202 of the tube blank is 2mm, and the wall thickness of the tail end 203 of the tube blank is 3.5mm. The length of the tube blank 200 after tube drawing is 1036.7 mm.
[0033] By processing different wall thicknesses at different stress-bearing locations and designing differentiated wall thicknesses, it is possible to ensure that the material has sufficient thickness where high-strength support is required, while the wall thickness can be reduced where high forces are not required, thereby reducing the overall weight. The pipe drawing process can also make the surface of the pipe smoother, reduce the need for subsequent polishing, and further reduce production costs. In addition, this process also helps to reduce the internal stress of the material and improve the stability and reliability of the product.
[0034] Reference Figure 2 (b) The tube tail end 203 is expanded to increase the outer diameter of the tube tail end 203. The tube tail end 203 is squeezed by the die of the tube expander, and the tube tail end 203 is expanded by mechanical pressure, thereby increasing the diameter of the tube tail end 203. The length of the tube 200 after the tube is drawn is 1016.7mm. The outer diameter range of the tube tail end 203 is 135±5mm by the tube expansion process. In this embodiment, the outer diameter of the tube tail end 203 after the tube expansion is 135mm.
[0035] The tail end 203 of the tube blank is the base of the motor seat 3. The motor seat 3 is the location for installing the motor or other drive components. It is necessary to form a space to accommodate the motor or other drive components. The tube expansion process can effectively change the size of the tail end 203 of the tube blank to match the motor or other drive components with a larger diameter. The tube expansion process allows size adjustment based on existing materials instead of cutting and removing materials, which can reduce material waste, improve production efficiency and reduce costs.
[0036] Reference Figure 2 (c) The portion of the tube billet tail end 203 away from the tube billet middle portion 202 is subjected to tube shrinkage treatment to achieve the reduction of the port diameter. The tube shrinkage process is used to make the outer diameter range of the port of the tube billet tail end 203 be: 105±5mm. In this embodiment, the outer diameter of the port of the tube billet tail end 203 is 105mm. The portion of the tube billet tail end 203 away from the middle portion 202 is placed in the mold of the tube shrinking machine, and the portion of the tube billet tail end 203 away from the middle portion 202 is compressed in the mold by applying external pressure. The tube shrinkage treatment allows the tube billet tail end 203 to form a wrapping space for the motor. Tube shrinkage can enhance the local stiffness and strength of the tube port, and enhance its durability and reliability.
[0037] Reference Figure 3 (d) The tube tail end 203 is flattened to make the entire tube body have an elliptical cross section. The tube tail end 203 is placed in a mold with a specific shape, and then the tube 200 is compressed by applying pressure. This pressure acts on both sides of the tube 200, changing it from a circular cross section to an elliptical cross section. The flattening process can improve the resistance of the tube under bending or torsional loads.
[0038] Reference Figure 3 (e) The tube tail end 203 is displaced to achieve flattening of the tube tail end 203. One end of the tube 200 is fixed by a mechanical fixture or a mold, and then pressure is applied to the other end to move it along the direction perpendicular to the tube axis. A portion of the material at the tube tail end 203 is pushed to one side of the tube end, thereby achieving a flattening effect on the bottom surface of the tube tail end 203, which is convenient for the subsequent bending process.
[0039] The tube tail end 203 is subjected to bending and shaping treatment. Figure 3 (f), a bending process is performed on the tail end 203 of the tube blank to make the bottom surface of the tail end 203 of the tube blank concave, thereby achieving a single bending of the tail end 203 of the tube blank; Figure 4 (g) A secondary bending process is performed on the tail end 203 of the tube blank, so that the end of the tube blank 200 is raised relative to the middle part 202 of the tube blank, thereby achieving secondary bending of the tail end 203 of the tube blank.
[0040] The tail end 203 of the tube billet is bent and deformed by external force to achieve the desired shape. In the first bending process, the tail end 203 of the tube billet is placed on the mold, and then pressure is applied by the press to make the bottom surface of the tail end 203 of the tube billet concave, forming the first bend. The second bending process is to further process the tail end 203 of the tube billet on the basis of the first bending, so that its port is raised relative to the middle part 202 of the tube billet, forming a more delicate and complex pipe shape. The desired spatial shape and functional characteristics can be given to the tail end 203 of the tube billet through bending shaping.
[0041] After bending and shaping, the fillet radius value of the corner of the middle part 202 of the tube tail end 203 is: 60±5mm. In this embodiment, the fillet radius value of the corner of the middle part 202 of the tube tail end 203 is 60mm. At the corner of the tube 200, stress tends to concentrate, increasing the risk of crack formation. The fillet radius value of the corner of the tube tail end 203 close to the middle part 202 of the tube is: 28.7±5mm. In this embodiment, the fillet radius value of the corner of the tube tail end 203 close to the middle part 202 of the tube is 28.7mm. Filleting helps to smooth stress distribution, reduce stress concentration, and thus improve the fatigue life of the pipe fitting.
[0042] The angle value of the corner α at the middle of the tube tail end 203 is: 107±5°. In this embodiment, the angle value of the corner at the middle of the tube tail end 203 is 107°, providing a suitable accommodation space for the motor. The angle value of the corner β at the tube tail end 203 close to the tube middle 202 is: 136±5°. In this embodiment, the angle value of the corner at the tube tail end 203 close to the tube middle 202 is 136°.
[0043] The tube blank 200 after bending and shaping is subjected to forming treatment as a whole. Figure 4 (h), the tube blank 200 after bending and shaping is subjected to a water sealing process to realize a preforming operation. Figure 4 (i) The tube blank 200 is subjected to a hydraulic forming process to achieve the overall forming of the tube blank 200. High-pressure liquid is applied to the tube blank 200 through the hydraulic system, so that the tube blank 200 is subjected to uniform pressure in the mold, thereby achieving plastic deformation of the material. During the hydraulic forming process, the tube blank 200 is placed between the upper and lower molds, and hydraulic oil is pumped into the system to apply pressure to the tube blank 200 so that it is formed according to the shape of the mold. In this way, complex shapes of the tube blank 200 can be formed at a lower forming force. Secondly, hydraulic forming can improve production efficiency, shorten production cycles, help improve product precision, and standardize products.
[0044] Reference Figure 4(j), the formed tube blank 200 is subjected to CNC machining to obtain the final product. The motor seat 3 and the window on the lower tube 2 can be processed on the formed product by a milling machine. To match the installation of the motor, the motor seat 3 is a cap-like structure formed by multiple rounding processes to form an arc shape, with an arc-shaped top plate and side plates on both sides of the top plate, not a cylindrical structure, and needs to be cut by a milling machine. The product processed by the milling machine is ground, polished and deburred to obtain a finished product.
[0045] The frame component 100 manufactured by gravity casting is loose and has pinholes. It is necessary to increase the ribs and thickness to improve the strength of the product, so that the weight of the frame component 100 is about 5kg, the finished vehicle is heavy and wastes materials. The present invention adopts liquid forging and pipe drawing process. After CNC processing, the overall length of the frame component 100 is 893.8mm and the overall weight is about 2kg. Through differentiated thickness design, thicker materials are used only where needed, which realizes the precise use of materials, thereby reducing weight and saving materials. This process is suitable for the manufacture of frame components 100 that require high strength and lightness. The use of hydraulic water expansion molds and CNC processing technology improves the accuracy and standardization of products. The mold is durable, reducing the frequency and cost of replacement; the pipe drawing process makes the product surface smooth and reduces the polishing cost. The material has a compact crystal structure, which improves the overall strength of the product.
[0046] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0047] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for manufacturing lightweight frame components using liquid forging and tube drawing processes, characterized in that: The following steps are involved: A tube blank (200) is manufactured by liquid forging, wherein the head end (201) of the tube blank is formed into a head tube (1), the middle part (202) of the tube blank is the base of the lower tube (2), and the tail end (203) of the tube blank is arranged in a circular shape and is the base of the motor seat (3); The middle part (202) and the tail end (203) of the tube blank are subjected to a tube drawing process, so that the middle part (202) and the tail end (203) of the tube blank are longer and the wall thickness is thinner, and different wall thicknesses are processed at different stress-bearing positions; Performing a tube expansion process on the tube blank tail end (203) to increase the outer diameter of the tube blank tail end (203); The portion of the tube blank tail end (203) away from the tube blank middle portion (202) is subjected to tube shrinkage treatment to achieve a reduction in diameter of the port; The tube tail end (203) is flattened so that the entire cross section of the tube tail end (203) is an elliptical structure; The tail end (203) of the tube blank is shifted to achieve flattening of the tail end (203) of the tube blank; Performing a bending and shaping process on the tail end (203) of the tube blank; Performing a forming process on the tube blank (200) after being bent and shaped as a whole; The formed tube blank (200) is subjected to numerical control processing to obtain a final product.
2. The method for manufacturing lightweight frame components by liquid forging and tube drawing process according to claim 1, characterized in that: The step of bending and shaping the tube tail end (203) comprises: Performing a primary bending process on the tail end (203) of the tube blank to make the bottom surface of the tail end (203) of the tube blank concave, thereby achieving a primary bending of the tail end (203) of the tube blank; The tail end (203) of the tube blank is subjected to a secondary bending process, so that the end of the tube blank (200) is raised relative to the middle part (202) of the tube blank, thereby achieving the secondary bending of the tail end (203) of the tube blank.
3. The method for manufacturing lightweight frame components by liquid forging and tube drawing process according to claim 1, characterized in that: The step of forming the entire tube blank (200) after bending and shaping comprises: Performing a water sealing process on the tube blank (200) after bending and shaping; The tube blank (200) is subjected to a hydraulic forming process to achieve the overall forming of the tube blank (200).
4. The method for manufacturing lightweight frame components by liquid forging and tube drawing process according to claim 1, characterized in that: In the step of drawing the tube from the middle portion (202) and the tail end (203) of the tube blank, the wall thickness of the middle portion (202) of the tube blank is within the range of 2±0.5 mm, and the wall thickness of the tail end (203) of the tube blank is within the range of 3.5±0.5 mm.
5. The method for manufacturing lightweight vehicle frame components by liquid forging and tube drawing process according to claim 1, characterized in that: The outer diameter range of one end of the tube blank head end (201) close to the tube blank middle part (202) is: 105±5mm, and in the step of expanding the tube blank tail end (203), the tube expansion process is used to make the outer diameter range of the tube blank tail end (203) be: 135±5mm.
6. The method for manufacturing lightweight vehicle frame components by liquid forging and tube drawing process according to claim 5, characterized in that: In the step of shrinking the portion of the tube blank tail end (203) away from the tube blank middle portion (202), the tube shrinking process is used to make the outer diameter range of the port of the tube blank tail end (203) be: 105±5mm.
7. The method for manufacturing lightweight vehicle frame components by liquid forging and tube drawing process according to claim 1, characterized in that: The fillet radius of the corner in the middle of the tube tail end (203) is 60±5 mm.
8. The method for manufacturing lightweight vehicle frame components by liquid forging and tube drawing process according to claim 1, characterized in that: The angle value of the corner in the middle of the tube tail end (203) is: 107±5°.
9. The method for manufacturing lightweight vehicle frame components by liquid forging and tube drawing process according to claim 1, characterized in that: The fillet radius of the corner of the tube blank tail end (203) close to the tube blank middle part (202) is: 28.7±5mm; and / or, The angle value of the corner of the tube blank tail end (203) close to the tube blank middle part (202) is: 136±5°.
10. A frame component, characterized in that: The lightweight frame component is manufactured by the method for manufacturing the lightweight frame component by liquid forging and tube drawing process as claimed in any one of claims 1 to 9.
Citation Information
Patent Citations
Liquid-state die forging machining cast aluminum alloy and casting process thereof
CN109897994A
Integrated molding process for producing rear controller shell of lower tube of electric bicycle
CN111546002A
Integrated lower pipe motor seat of electric bicycle and processing technology thereof
CN114987671A
Head tube, lower tube and motor seat integrated forming structure and processing technology thereof
CN116691899A
Process and system for integrated structure of motor seat and lower pipe by adopting oil / water injection molding
CN117381336A
Cited By
Motor base and lower pipe forging and drawing integrated forming process
CN121289968A