Forming process of delayed fracture resistant bolt for bridge engineering

By optimizing the heating, forging and surface treatment processes, the delayed fracture resistance and durability of bolts used in bridge engineering are improved, the problems of material fatigue and insufficient delayed fracture resistance in the existing technology are solved, and the stability and safety of the bridge are ensured sex.

CN118847894AInactive Publication Date: 2024-10-29HAIYAN SHENGXIN STANDARD PARTS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411115955.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, the material fatigue performance of bolts in bridge engineering is relatively high, and the delayed fracture resistance needs to be further optimized, which affects the stability and safety of the bridge.

Method used

By optimizing heating, forging, tempering and surface treatment processes, including high-frequency induction heating, step heating and cooling, precision mold forming, tempering treatment, ammonia water degreasing, sulfuric acid solution pickling, phosphating and sodium nitrite solution blackening Processing to ensure the bolt's precise shape, dense internal structure, surface hardness and corrosion resistance.

Benefits of technology

It significantly improves the delayed fracture resistance and overall durability of bolts, reduces material fatigue, extends service life, and improves the safety and reliability of bridge projects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847894A_ABST
    Figure CN118847894A_ABST
Patent Text Reader

Abstract

The invention discloses a delayed fracture resistant bolt forming process for bridge engineering, which comprises the following steps: material preparation and primary heating: selecting high-strength alloy steel as a raw material, carrying out high-frequency induction heating on a straight strip material, carrying out primary softening and homogenization treatment, then quickly breaking the material, and cooling to room temperature; precise heating and forging are conducted, specifically, the primarily-treated workpiece is fed into a precise induction heater, and a stepped heating strategy is adopted for heating; then, the heated workpiece is rapidly put into a precision mold, and primary forging and pressing head preforming and secondary forging and pressing head forming are sequentially completed; the method has the beneficial effects that by optimizing the heating, forging and hardening and tempering processes, the internal defects of materials are reduced, the internal uniformity of metal is improved, and the delayed fracture resistance of the bolt is remarkably enhanced; through precise heating and cooling control and reasonable thermal refining, the fatigue performance of the material is effectively reduced, and the service life of the bolt is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bolt forming, and in particular relates to a delayed fracture resistant bolt forming process for bridge engineering. Background Art

[0002] Bridge engineering is an important part of modern infrastructure construction, and bolts, as key components connecting bridge steel structures, have a direct impact on the stability and safety of the entire bridge. With the increasing demand for bridge construction, the demand for high-strength bolts that can resist delayed fracture is also growing.

[0003] A warm upsetting weather-resistant delayed fracture resistant high-strength bolt forming process with publication number CN111570714A discloses the following steps: heating a straight strip material to 300-400°C by high frequency, cutting the strip material, cooling the strip material to room temperature, loading the strip material, and heating the strip material in an induction heater, wherein the temperature is controlled at 500-600°C, and the heating time is 2-3s; placing the heated workpiece in a mold, and sequentially performing a primary forging head preforming, a secondary forging head forming, and ejecting the workpiece to obtain a preformed workpiece; degreasing the preformed workpiece in ammonia water at a degreasing temperature of 30-35°C, washing the workpiece with water, and pickling the workpiece in a sulfuric acid solution for 10-20s at a pickling temperature of 5-15°C, washing the workpiece with water, phosphating the workpiece with water, air drying the workpiece with water, and blackening the workpiece in a sodium nitrite solution for 2-5min, washing the workpiece with water, and air drying the workpiece to obtain a warm upsetting weather-resistant delayed fracture resistant high-strength bolt.

[0004] Although the existing technology has improved the strength and weather resistance of bolts to a certain extent, in practical applications it still faces the problem of high material fatigue performance and the need to further optimize the delayed fracture resistance. Summary of the invention

[0005] The purpose of the present invention is to provide a delayed fracture resistant bolt forming process for bridge engineering, which significantly improves the delayed fracture resistance and overall durability of the bolts by optimizing multiple links such as heating, forging, tempering and surface treatment.

[0006] To achieve the above object, the present invention provides the following technical solution: a forming process for delayed fracture resistant bolts for bridge engineering, the forming process is as follows:

[0007] Material preparation and preliminary heating: High-strength alloy steel is selected as the raw material, and the straight strip is heated by high-frequency induction for preliminary softening and homogenization, and then the material is quickly cut and cooled to room temperature;

[0008] Precision heating and forging: The workpiece after preliminary treatment is sent to the precision induction heater and heated using a step-by-step heating strategy; then, the heated workpiece is quickly placed in a precision mold to complete the primary forging head preforming and secondary forging head forming in sequence, ensuring that the head shape is accurate and the internal structure is dense;

[0009] Quenching and tempering treatment: The preformed workpiece is subjected to a step-by-step cooling treatment, first rapidly cooled, then slowly cooled to room temperature; followed by tempering treatment;

[0010] Surface strengthening treatment: surface treatment of the quenched and tempered bolts;

[0011] Final inspection and packaging: The processed bolts are fully inspected to ensure that all indicators meet the requirements of the bridge project. Once qualified, they are packaged for rust prevention.

[0012] As a preferred technical solution of the present invention, the processed bolts are comprehensively inspected, including appearance inspection, dimension measurement, mechanical property test and delayed fracture resistance test.

[0013] As a preferred technical solution of the present invention, high-frequency induction heating is performed to 410-450°C.

[0014] As a preferred technical solution of the present invention, a step-by-step temperature increase strategy is used, in which the temperature is controlled at 520-580° C. and the heating time is controlled at 1-5 min.

[0015] As a preferred technical solution of the present invention, the preformed workpiece is subjected to a step-by-step temperature reduction treatment, firstly rapidly cooled to 320-360° C., and then cooled to room temperature.

[0016] As a preferred technical solution of the present invention, the quenched and tempered bolts are subjected to surface treatment, including ammonia water degreasing, sulfuric acid solution pickling, phosphating treatment, and sodium nitrite solution blackening treatment, and each step is followed by water washing and air drying.

[0017] As a preferred technical solution of the present invention, the temperature of the ammonia water degreasing is 32-34°C and the time is 2-4s; the temperature of the sulfuric acid solution pickling is 10-12°C and the time is 8-10s.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] By optimizing the heating, forging and quenching and tempering processes, the internal defects of the material are reduced, the internal uniformity of the metal is improved, and the delayed fracture resistance of the bolt is significantly enhanced;

[0020] Precise heating and cooling control, as well as reasonable quenching and tempering treatment, effectively reduce the fatigue performance of the material and extend the service life of the bolts;

[0021] The strict surface treatment process not only enhances the corrosion resistance and surface hardness of the bolts, but also improves their overall durability, ensuring the safety and reliability of the bridge project. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a flow chart of the molding process of the present invention. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] See also Figure 1 , which is the first embodiment of the present invention, provides a delayed fracture resistant bolt forming process for bridge engineering, comprising the following steps:

[0026] Material preparation and preliminary heating: High-strength alloy steel is selected as the raw material, and the straight strip is heated to 410℃ by high-frequency induction, and then the strip is initially softened and homogenized, and then the strip is quickly cut and cooled to room temperature to reduce thermal stress;

[0027] Precision heating and forging: The workpiece after preliminary treatment is sent to the precision induction heater and heated using a step-by-step heating strategy. The temperature is controlled at 520°C and the heating time is controlled at 1 minute. Subsequently, the heated workpiece is quickly placed in a precision mold to complete the primary forging head preforming and secondary forging head forming in sequence, ensuring that the head shape is accurate and the internal structure is dense.

[0028] Quenching and tempering treatment: The preformed workpiece is subjected to a step-by-step cooling treatment, first rapidly cooled to 320°C, then slowly cooled to room temperature; followed by tempering treatment;

[0029] Surface strengthening treatment: The surface treatment of the quenched and tempered bolts includes ammonia degreasing, sulfuric acid solution pickling, phosphating treatment, and sodium nitrite solution blackening treatment. Each step is followed by water washing and air drying. The temperature of ammonia degreasing is 32°C and the time is 2s; the temperature of sulfuric acid solution pickling is 10°C and the time is 8s.

[0030] Final inspection and packaging: The processed bolts are fully inspected, including appearance inspection, dimension measurement, mechanical property test and delayed fracture resistance test, etc., to ensure that all indicators meet the requirements of bridge engineering; after passing the inspection, they are rust-proofed and packaged for shipment.

[0031] Example 2

[0032] See also Figure 1 , which is the second embodiment of the present invention, provides a delayed fracture resistant bolt forming process for bridge engineering, comprising the following steps:

[0033] Material preparation and preliminary heating: High-strength alloy steel is selected as the raw material, and the straight strip is heated to 420℃ by high-frequency induction, and then the strip is initially softened and homogenized, and then the strip is quickly cut and cooled to room temperature to reduce thermal stress;

[0034] Precision heating and forging: The workpiece after preliminary treatment is sent to the precision induction heater and heated using a step-by-step heating strategy. The temperature is controlled at 540°C and the heating time is controlled at 2 minutes. Subsequently, the heated workpiece is quickly placed in a precision mold to complete the primary forging head preforming and secondary forging head forming in sequence, ensuring that the head shape is accurate and the internal structure is dense.

[0035] Quenching and tempering treatment: The preformed workpiece is subjected to a step-by-step cooling treatment, first rapidly cooled to 330°C, then slowly cooled to room temperature; followed by tempering treatment;

[0036] Surface strengthening treatment: The surface treatment of the quenched and tempered bolts includes ammonia degreasing, sulfuric acid solution pickling, phosphating treatment, and sodium nitrite solution blackening treatment. Each step is followed by water washing and air drying. The temperature of ammonia degreasing is 33°C and the time is 3s; the temperature of sulfuric acid solution pickling is 11°C and the time is 9s.

[0037] Final inspection and packaging: The processed bolts are fully inspected, including appearance inspection, dimension measurement, mechanical property test and delayed fracture resistance test, etc., to ensure that all indicators meet the requirements of bridge engineering; after passing the inspection, they are rust-proofed and packaged for shipment.

[0038] Example 3

[0039] See also Figure 1 , which is the third embodiment of the present invention, provides a delayed fracture resistant bolt forming process for bridge engineering, comprising the following steps:

[0040] Material preparation and preliminary heating: High-strength alloy steel is selected as the raw material, and the straight strip is heated to 430°C by high-frequency induction, and then the strip is initially softened and homogenized, and then quickly cut and cooled to room temperature to reduce thermal stress;

[0041] Precision heating and forging: The workpiece after preliminary treatment is sent to the precision induction heater and heated using a step-by-step heating strategy. The temperature is controlled at 560°C and the heating time is controlled at 3 minutes. Subsequently, the heated workpiece is quickly placed in a precision mold to complete the primary forging head preforming and secondary forging head forming in sequence, ensuring that the head shape is accurate and the internal structure is dense.

[0042] Quenching and tempering treatment: The preformed workpiece is subjected to a step-by-step cooling treatment, first rapidly cooled to 340°C, then slowly cooled to room temperature; followed by tempering treatment;

[0043] Surface strengthening treatment: The surface treatment of the quenched and tempered bolts includes ammonia degreasing, sulfuric acid solution pickling, phosphating treatment, and sodium nitrite solution blackening treatment. Each step is followed by water washing and air drying. The temperature of ammonia degreasing is 34°C and the time is 4s; the temperature of sulfuric acid solution pickling is 12°C and the time is 10s.

[0044] Final inspection and packaging: The processed bolts are fully inspected, including appearance inspection, dimension measurement, mechanical property test and delayed fracture resistance test, etc., to ensure that all indicators meet the requirements of bridge engineering; after passing the inspection, they are rust-proofed and packaged for shipment.

[0045] Example 4

[0046] See also Figure 1 , which is the fourth embodiment of the present invention, provides a delayed fracture resistant bolt forming process for bridge engineering, comprising the following steps:

[0047] Material preparation and preliminary heating: High-strength alloy steel is used as the raw material. The straight strip is heated to 450°C by high-frequency induction, and then initially softened and homogenized. The strip is then quickly cut and cooled to room temperature to reduce thermal stress.

[0048] Precision heating and forging: The workpiece after preliminary treatment is sent to the precision induction heater and heated using a step-by-step heating strategy. The temperature is controlled at 580°C and the heating time is controlled at 5 minutes. Subsequently, the heated workpiece is quickly placed in a precision mold to complete the primary forging head preforming and secondary forging head forming in sequence, ensuring that the head shape is accurate and the internal structure is dense.

[0049] Tempering treatment: The preformed workpiece is subjected to a step-by-step cooling treatment, first rapidly cooled to 360°C, then slowly cooled to room temperature; followed by tempering treatment;

[0050] Surface strengthening treatment: The surface treatment of the quenched and tempered bolts includes ammonia degreasing, sulfuric acid solution pickling, phosphating treatment, and sodium nitrite solution blackening treatment. Each step is followed by water washing and air drying. The temperature of ammonia degreasing is 34°C and the time is 4s; the temperature of sulfuric acid solution pickling is 12°C and the time is 10s.

[0051] Final inspection and packaging: The processed bolts are fully inspected, including appearance inspection, dimension measurement, mechanical property test and delayed fracture resistance test, etc., to ensure that all indicators meet the requirements of bridge engineering; after passing the inspection, they are rust-proofed and packaged for shipment.

[0052] Although the embodiments of the present invention have been shown and described, as detailed above, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A delayed fracture resistant bolt forming process for bridge engineering, characterized in that: The molding process is as follows: Material preparation and preliminary heating: High-strength alloy steel is selected as the raw material, and the straight strip is heated by high-frequency induction for preliminary softening and homogenization, and then the material is quickly cut and cooled to room temperature; Precision heating and forging: The workpiece after preliminary treatment is sent to the precision induction heater and heated using a step-by-step heating strategy; then, the heated workpiece is quickly placed in a precision mold to complete the primary forging head preforming and secondary forging head forming in sequence, ensuring that the head shape is accurate and the internal structure is dense; Quenching and tempering treatment: The preformed workpiece is subjected to a step-by-step cooling treatment, first rapidly cooled, then slowly cooled to room temperature; followed by tempering treatment; Surface strengthening treatment: surface treatment of the quenched and tempered bolts; Final inspection and packaging: The processed bolts are fully inspected to ensure that all indicators meet the requirements of the bridge project. Once qualified, they are packaged for rust prevention.

2. The delayed fracture resistant bolt forming process for bridge engineering according to claim 1 is characterized in that: The processed bolts are comprehensively inspected, including appearance inspection, dimension measurement, mechanical property test and delayed fracture resistance test.

3. The delayed fracture resistant bolt forming process for bridge engineering according to claim 1 is characterized in that: High frequency induction heating to 410-450℃.

4. The delayed fracture resistant bolt forming process for bridge engineering according to claim 1 is characterized in that: A step-by-step heating strategy is used, with the temperature controlled at 520-580°C and the heating time controlled at 1-5 minutes.

5. The delayed fracture resistant bolt forming process for bridge engineering according to claim 1 is characterized in that: The preformed workpiece is subjected to a step-by-step cooling treatment, first rapidly cooled to 320-360°C, and then cooled to room temperature.

6. The delayed fracture resistant bolt forming process for bridge engineering according to claim 1 is characterized in that: The quenched and tempered bolts are surface treated, including ammonia degreasing, sulfuric acid solution pickling, phosphating, and sodium nitrite solution blackening. Each step is followed by water washing and air drying.

7. The delayed fracture resistant bolt forming process for bridge engineering according to claim 6 is characterized in that: The temperature of the ammonia degreasing is 32-34°C and the time is 2-4s; the temperature of the sulfuric acid solution pickling is 10-12°C and the time is 8-10s.

Citation Information

Patent Citations

  • Warm heading weather-proof delayed fracture resistance high-strength bolt forming process

    CN111570714A